Sand casting process for heat-resistant steel exhaust manifold
Through the hot core box method and casting simulation analysis, the sand casting process of heat-resistant steel exhaust manifolds has been simplified, solving the problems of surface roughness and production efficiency in the existing technology, and achieving high-quality, low-cost mass production. .
Patent Information
- Application Number
- CN202411071209.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-01
AI Technical Summary
The existing sand casting process cannot meet the surface roughness requirements of heat-resistant steel exhaust manifolds, and the production process is complex and relies on high-cost coatings and precision machining, which limits the economy and efficiency of large-scale mass production.
The hot core box method is used to use green mold sand to manufacture the inner cavity sand core, and the exhaust manifold mold is divided into sand molds and split sand cores through casting simulation analysis, and X-RAY inspection equipment is used to detect internal defects to simplify the production process. Reduce paint usage, improve production efficiency and material cost economy.
Without the use of coatings, it meets the requirements for surface roughness Ra≤12.5μm of the inner cavity of the heat-resistant steel exhaust manifold, reduces the occurrence of quality defects such as pores, cracks and sintering sand, and improves the yield and production of castings. efficiency, achieving high-quality mass production under limited production conditions.
Smart Images

Figure CN118720051A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sand casting, and in particular to a sand casting process for a heat-resistant steel exhaust manifold. Background Art
[0002] As a key component of a car engine, the exhaust system's main responsibility is to effectively discharge the high-temperature and high-pressure exhaust gas generated by engine combustion, while the exhaust manifold is the core component of the exhaust system. The exhaust manifold is used to connect each cylinder of the engine with the main exhaust pipe to achieve efficient collection and discharge of exhaust gas.
[0003] The exhaust manifold also has high requirements for the surface roughness of the inner cavity. Increased roughness will lead to increased gas flow resistance, poor exhaust, aggravated thermal stress problems and accelerated corrosion, which will in turn affect the efficiency of the entire exhaust system and engine performance, and shorten the service life of the exhaust manifold. Therefore, during the design and manufacturing process, the surface roughness of the exhaust manifold inner cavity must be strictly controlled to meet working requirements.
[0004] In view of the working environment of the exhaust manifold, the existing technology usually uses heat-resistant steel to make the exhaust manifold. Heat-resistant steel is a special steel that can maintain its physical and chemical properties at high temperatures. Its heat resistance temperature can reach above 1000 degrees Celsius, and it has pressure resistance and corrosion resistance. Since the exhaust manifold has a complex inner cavity structure and has requirements on surface roughness, the existing technology usually uses a shell molding process to cast the exhaust manifold.
[0005] However, the shell molding process requires the use of expensive resin sand and precision-machined metal molds. The production process is complex, requires a high degree of automation of the equipment, and relies on the use of coatings, which has high requirements for production conditions. Therefore, under limited production conditions, in order to reduce production costs and reduce the use of coatings, an attempt is made to use sand casting technology to produce heat-resistant steel exhaust manifolds.
[0006] In order to achieve large-scale mass production of exhaust manifolds, green sand is selected as the material for sand cores in the sand casting process. Compared with other sand materials, green sand is suitable for the production of large castings, such as machine tool bases, etc. Its production process is relatively simple and suitable for mass production. However, the existing sand casting process often relies on the use of coatings to meet the surface roughness requirements of castings, and when using green sand, the existing sand casting process is difficult to meet the surface roughness requirements of heat-resistant steel exhaust manifolds. Summary of the invention
[0007] The purpose of the present invention is to provide a sand casting process for a heat-resistant steel exhaust manifold in view of the problems existing in the prior art.
[0008] To achieve the above object, the technical solution adopted by the present invention is:
[0009] A sand casting process for a heat-resistant steel exhaust manifold comprises the following steps:
[0010] Through casting simulation analysis, the mold of the exhaust manifold is divided into a sand mold and a plurality of split sand cores according to the structure of the exhaust manifold;
[0011] The split sand core comprises an outer shell sand core, a flow channel sand core and an inner cavity sand core, and the inner cavity sand core is manufactured by using a hot core box method and green sand;
[0012] Combining the shell sand core, the flow channel sand core, the sand mold and the inner cavity sand core not coated with paint for casting;
[0013] After the pouring is completed, the molded casting is processed and the internal defects of the casting are detected using X-RAY detection equipment.
[0014] The present invention adopts a sand casting process to cast a heat-resistant steel exhaust manifold. Compared with the traditional shell molding process, it not only simplifies the production process and improves production efficiency, but also is more economical in terms of material cost and equipment investment. Since the inner cavity sand core does not need to be coated with paint, part of the cumbersome manual dipping process is omitted, reducing dependence on paint, thereby reducing paint consumption and labor costs.
[0015] The inner cavity sand core made of green sand can meet the surface roughness requirement of Ra≤12.5μm of the inner cavity of the heat-resistant steel exhaust manifold without using paint, avoiding quality defects such as pores, cracks, sintering and sand adhesion on the surface of the casting, achieving the purpose of improving the surface quality of the casting under limited production conditions and improving the economy of the casting process.
[0016] Preferably, the steps of the hot box method are as follows: preheating the hot box, injecting the coated sand into the hot box by a sand injection device, performing fire spraying on the surface of the formed sand core, then maintaining the temperature of the hot box to allow the surface of the sand core to form a crust, turning the hot box over and resetting it, then maintaining the temperature of the hot box to allow the surface of the sand core to solidify, and finally taking out the inner cavity sand core from the hot box.
[0017] The hot core box method can quickly respond to production needs, realize rapid molding and hardening of sand cores, shorten the production cycle, improve production efficiency, and meet the needs of large-scale production.
[0018] Preferably, the composition of the green sand is: 0-0.15% by weight of fine powder, 0.5-1.2% by weight of bentonite, 1.2-4% by weight of water, and 10±2% by weight of mud.
[0019] Preferably, the performance parameters of the green sand are as follows: compaction rate 39.5±3%, loss on ignition 1.5±0.5%, air permeability index 180±30, wet compressive strength 195±10Kpa, and blue absorption MB value 8.5±1%.
[0020] By adjusting the composition of the green sand and controlling the performance parameters of the green sand, the stability and consistency of the sand core during the manufacturing process can be ensured to meet the surface quality requirements of the casting, thereby improving the yield rate of the casting.
[0021] Preferably, the hot core box comprises a movable mold and a static mold, the preheating temperature of the movable mold and the static mold is 250±5°C, and during curing and crusting, the temperature of the movable mold and the static mold is maintained at 250±5°C.
[0022] By controlling the temperature of the hot core box, it can be ensured that the sand is heated evenly in the hot core box, which is beneficial to the crusting and curing process of the sand core surface, which can significantly improve the strength and density of the sand core and reduce the risk of deformation or breakage of the sand core in subsequent processes.
[0023] Preferably, the flame spraying treatment step is as follows: after the sand mixture is injected into the hot core box, the entire sand core surface is immediately heated by flame spraying using a flame heating device, and the flame spraying lasts for 50±1 seconds.
[0024] The flame blasting treatment can rapidly heat the surface of the sand core, so that the sand material close to the surface of the hot core box is hardened by heat, which helps to maintain the shape and dimensional accuracy of the sand core in the subsequent process, thereby improving the surface quality of the sand core.
[0025] Preferably, the step of crusting the surface of the sand core is as follows: after the flame spraying, the temperature of the hot core box is maintained so that the sand material close to the surface of the hot core box is hardened by heat to form a hard shell, and the whole process lasts for 20-30 seconds.
[0026] The crusted sand core surface can resist external pressure and impact, reduce the breakage rate of the sand core during pouring, cooling and the like, reduce the shedding and penetration of sand particles during pouring, thereby reducing the roughness of the casting surface, reducing the generation of defects such as pores and sand inclusions, and improving the casting yield rate.
[0027] Preferably, the steps of flipping and resetting the hot core box are as follows: flipping the hot core box to pour out the uncrusted part of the sand material, the flipping time is controlled between 20-60 seconds, and then flipping the hot core box to return it to its original position.
[0028] By flipping the hot core box, the unencrusted sand can be effectively poured out to prevent it from affecting the quality and stability of the sand core in subsequent processes. At the same time, part of the sand on the surface of the sand core has the opportunity to be redistributed, which helps to eliminate surface defects, improve the surface finish of the sand core, and provide a better foundation for subsequent processing.
[0029] Preferably, the step of curing the surface layer of the sand core is as follows: maintaining the temperature of the hot core box for 120±1 seconds, so that the sand material hardens itself through the residual heat and the heat released by the hardening reaction.
[0030] After the surface layer of the sand core is solidified, a solid shell is formed, which significantly improves the structural stability of the sand core, so that the sand core can withstand harsh conditions such as high temperature and high pressure in the subsequent casting process without being easily deformed or damaged.
[0031] At the same time, the solidification of the sand core surface helps to reduce the gas intrusion and penetration of the sand core during the casting process, reduces the probability of defects such as pores and sand holes inside the casting, and improves the finished product rate and quality reliability of the casting.
[0032] Preferably, for the casting cast and the inner cavity sand core manufactured according to the process, the surface roughness of the inner cavity of the casting is Ra≤12.5 μm.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] (1) The present invention adopts a sand casting process to cast a heat-resistant steel exhaust manifold. Compared with the traditional shell molding process, it not only simplifies the production process and improves the production efficiency, but also is more economical in terms of material cost and equipment investment. Since the inner cavity sand core does not need to be coated with paint, part of the cumbersome manual dipping process is omitted, reducing the dependence on paint, thereby reducing paint consumption and labor costs.
[0035] (2) The present invention adopts a sand casting process and uses an inner sand core made of green sand. Without using any coating, it can meet the surface roughness requirement of the inner cavity of the heat-resistant steel exhaust manifold Ra≤12.5μm, avoid the appearance of quality defects such as pores, cracks, sintering and sand adhesion on the surface of the casting, achieve the purpose of improving the surface quality of the casting under limited production conditions, and improve the economy of the casting process. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 A schematic diagram of a sand casting process according to an embodiment of the present invention;
[0037] Figure 2 It is a schematic diagram of the process of making sand cores by the hot core box method in an embodiment of the present invention;
[0038] Figure 3 Schematic diagram of the structure of a heat-resistant steel exhaust manifold in an embodiment of the present invention;
[0039] Figure 4 Schematic diagram of the structure of the mold of the exhaust manifold in an embodiment of the present invention;
[0040] Figure 5 It is a schematic diagram of the structure of the inner cavity sand core in an embodiment of the present invention;
[0041] Figure 6 It is a structural cross-sectional view of a mold of an exhaust manifold in an embodiment of the present invention;
[0042] In the figure: 1. Heat-resistant steel exhaust manifold; 2. Sand mold; 3. Shell sand core; 4. Flow channel sand core; 5. Inner cavity sand core. DETAILED DESCRIPTION
[0043] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] Embodiment 1: Figure 1-6 As shown, the specific scheme of the first embodiment is as follows: A sand casting process for a heat-resistant steel exhaust manifold comprises the following steps:
[0045] S1. Using Magma soft casting simulation software, the heat-resistant steel exhaust manifold 1 is subjected to casting simulation analysis. According to the shape of the exhaust manifold, the upward placement of the casting outlet flange ball head is determined to optimize the gas emission and metal liquid flow during the casting process.
[0046] S2. Through simulation analysis, confirm the position and size of the riser to ensure that the molten metal can be effectively compensated during the solidification process to avoid the occurrence of defects such as shrinkage cavities and shrinkage.
[0047] S3. Refer to the simulated flow and actual production experience to design a reasonable flow path solution to ensure that the molten metal can smoothly and evenly fill the entire mold and reduce the occurrence of defects.
[0048] S4. According to the structure and size of the exhaust manifold, the mold of the exhaust manifold is divided into a sand mold 2 and several split sand cores. The split sand cores include an outer shell sand core 3, a flow channel sand core 4 and an inner cavity sand core 5, wherein there are four inner cavity sand cores 5. The sand mold 2 is a casting mold for manufacturing the shape of the heat-resistant steel exhaust manifold 1, and the split sand core is a casting mold for manufacturing the complex cavity inside the heat-resistant steel exhaust manifold 1 during the casting process.
[0049] S5. Prepare green sand. The composition of green sand is as follows: 0-0.15% by weight of fine powder, 0.5-1.2% by weight of bentonite, 1.2-4% by weight of water, and 10±2% by mud content. The performance parameters of green sand are as follows: compaction rate 39.5±3%, loss on ignition 1.5±0.5%, permeability index 180±30, wet compressive strength 195±10Kpa, and blue absorption MB value 8.5±1%.
[0050] S6. Using the hot core box method, green sand is used to manufacture the inner cavity sand core 5. The hot core box includes a moving mold and a static mold. The specific steps of the hot core box method are as follows:
[0051] 1. Hot box preheating steps: Heat the hot box to 250±5℃, ready to receive sand.
[0052] 2. Sand shooting step: The green sand is quickly shot into the preheated hot core box cavity through the sand shooting device, and compressed air or mechanical vibration is used to compact the sand layer and completely fill the hot core box.
[0053] 3. Flame sintering step: Use flame heating equipment to quickly and evenly flame the surface of the sand core for 50 seconds to preheat the sand surface and promote the subsequent crusting process.
[0054] 4. Encrusting step: After sintering, maintain the temperature of the hot core box at 250±5℃, so that the sand close to the mold surface is heated, and the surface of the sand core begins to harden and form a hard shell. The encrusting time is controlled within 20 seconds.
[0055] 5. Flip and pour out the remaining sand steps: When a hard shell is formed on the surface of the sand core, flip the mold to pour out the uncrusted sand. The flipping time is 40 seconds, and then flip the hot core box back to its original position.
[0056] 6. Curing step: Maintain the temperature of the hot core box at 250±5℃, so that the sand inside the sand core can harden itself through the residual heat and the heat released by the hardening reaction to achieve the purpose of complete curing. The curing time is 120 seconds.
[0057] 7. Coring step: After the sand core is completely solidified, remove the sand core from the hot core box to complete the entire production process.
[0058] S7, combining the shell sand core 3, the runner sand core 4, the sand mold 2 and the inner cavity sand core 5 not coated with paint, and casting, the selected casting material is GX40CrNiSi25-12 heat-resistant cast steel, and the casting temperature is 1650℃-1600℃;
[0059] S8. After pouring is completed, the molded casting is processed and the internal defects of the casting are detected using X-RAY detection equipment.
[0060] The inventor cast a heat-resistant steel exhaust manifold 1 according to the process of the first embodiment. After testing, the surface roughness Ra of the inner cavity of the heat-resistant steel exhaust manifold 1 was found to be ≤6.3 μm.
[0061] In order to further verify the effectiveness of the casting process of the present invention, the inventors also carried out the following specific examples and comparative examples:
[0062] Embodiment 2: Embodiment 2 differs from Embodiment 1 in that, in the specific steps of the hot box method, the turning time is 20 seconds or 60 seconds.
[0063] The inventor cast a heat-resistant steel exhaust manifold 1 according to the process of the second embodiment. After testing, the surface roughness Ra of the inner cavity of the heat-resistant steel exhaust manifold 1 was found to be ≤12.5 μm.
[0064] Embodiment 3: Embodiment 3 is different from Embodiment 1 in that, in the specific steps of the hot box method, the crusting time is 30 seconds, and the turning time is 20 seconds or 40 seconds.
[0065] The inventor cast a heat-resistant steel exhaust manifold 1 according to the process of the third embodiment. After testing, the surface roughness Ra of the inner cavity of the heat-resistant steel exhaust manifold 1 was ≤12.5 μm.
[0066] The inventors manufactured inner cavity sand cores 5 according to the processes of Example 1, Example 2 and Example 3, respectively, and conducted multiple tests on each inner cavity sand core 5, and the test results all met the following standards:
[0067] AFS particle size is 80-85; LOI ≤ 2.5%; gas evolution of sand core during casting process ≤ 16.0 ml / g; melting point ≥ 95°C; flexural strength at room temperature ≥ 7.0 MPa; tensile strength at room temperature ≥ 2.0 MPa; Among them, LOI refers to the percentage of mass reduction of sand core material after burning, and the test temperature of flexural strength and tensile strength at room temperature is 20°C ~ 25°C.
[0068] Comparative Example 1: The difference between this Comparative Example 1 and Example 1 is that, in the specific steps of the hot box method, the temperature of the hot box during preheating, crusting and curing is 230°C, there is no flame sintering step, no crusting step, no turning over and pouring out the remaining sand step, and the curing time is 80 seconds, 90 seconds or 100 seconds.
[0069] The inventors manufactured the inner cavity sand core 5 according to the process of comparative example 1. After testing, it was found that the inner cavity sand core 5 failed to fully solidify or bond after pouring, resulting in loose sand particles and the formation of a "green sand" phenomenon.
[0070] Comparative Example 2: The difference between Comparative Example 2 and Example 1 is that, in the specific steps of the hot box method, the temperature of the hot box during preheating, crusting and curing is 230°C, there is no flame sintering step, no crusting step, no turning over and pouring out the remaining sand step, and the curing time is 100 seconds, 110 seconds or 120 seconds.
[0071] The inventor cast a heat-resistant steel exhaust manifold 1 according to the process of comparative example 2. After testing, it was found that pores appeared on the surface of the inner cavity of the heat-resistant steel exhaust manifold 1 and the overall surface was not smooth.
[0072] Comparative Example 3: The difference between Comparative Example 3 and Example 1 is that, in the specific steps of the hot box method, the flame spraying time is 15 seconds or 30 seconds, there is no crusting step, and there is no turning and pouring out the remaining sand step.
[0073] The inventor cast a heat-resistant steel exhaust manifold 1 according to the process of comparative example 3. After testing, it was found that pores appeared on the surface of the inner cavity of the heat-resistant steel exhaust manifold 1 and the overall surface was not smooth.
[0074] Comparative Example 4: The difference between Comparative Example 4 and Example 1 is that, in the specific steps of the hot box method, the flame spraying time is 45 seconds, 60 seconds or 75 seconds, there is no crusting step, and there is no turning and pouring out the remaining sand step.
[0075] The inventor cast a heat-resistant steel exhaust manifold 1 according to the process of comparative example 4. After testing, the surface roughness Ra of the inner cavity of the heat-resistant steel exhaust manifold 1 was found to be ≤25 μm.
[0076] Comparative Example 5: The difference between Comparative Example 5 and Example 1 is that, in the specific steps of the hot box method, the temperature of the hot box during preheating, crusting and curing is 270°C, the flame spraying time is 15 seconds or 30 seconds, there is no crusting step, and there is no turning over and pouring out the remaining sand.
[0077] The inventor cast a heat-resistant steel exhaust manifold 1 according to the process of comparative example 5. After testing, it was found that the surface of the inner cavity of the heat-resistant steel exhaust manifold 1 had sintering and sand adhesion, and the surface was rough.
[0078] Comparative Example 6: The difference between Comparative Example 6 and Example 1 is that, in the specific steps of the hot box method, the flame spraying time is 45 seconds or 60 seconds, there is no crusting step, and there is no turning over and pouring out the remaining sand step.
[0079] The inventor cast a heat-resistant steel exhaust manifold 1 according to the process of comparative example 6. After testing, small holes appeared on the surface of the inner cavity of the heat-resistant steel exhaust manifold 1, and the surface roughness Ra≤25μm.
[0080] Comparative Example 7: The difference between Comparative Example 7 and Example 1 is that, in the specific steps of the hot box method, the flame spraying time is 75 seconds, the crusting time is 10 seconds, and there is no turning over and pouring out the remaining sand steps.
[0081] The inventor cast a heat-resistant steel exhaust manifold 1 according to the process of comparative example 7. After testing, it was found that the surface of the inner cavity of the heat-resistant steel exhaust manifold 1 had sintering and sand adhesion, and the surface was rough.
[0082] Comparative Example 8: The difference between Comparative Example 8 and Example 1 is that, in the specific steps of the hot box method, the crusting time is 30 seconds and the turning time is 60 seconds.
[0083] The inventor cast a heat-resistant steel exhaust manifold 1 according to the process of comparative example 8. After testing, small holes appeared on the surface of the inner cavity of the heat-resistant steel exhaust manifold 1, and the surface roughness Ra≤25μm.
[0084] Comparative Example 9: The difference between Comparative Example 9 and Example 1 is that, in the specific steps of the hot box method, the crusting time is 40 seconds, and the turning time is 20 seconds, 40 seconds or 60 seconds.
[0085] The inventor cast a heat-resistant steel exhaust manifold 1 according to the process of comparative example nine. After testing, it was found that the surface of the inner cavity of the heat-resistant steel exhaust manifold 1 had sintering and sand adhesion, and the surface was rough.
[0086] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A sand casting process for a heat-resistant steel exhaust manifold, characterized in that: The steps include: Through casting simulation analysis, the mold of the exhaust manifold is divided into a sand mold and a plurality of split sand cores according to the structure of the exhaust manifold; The split sand core comprises an outer shell sand core, a flow channel sand core and an inner cavity sand core, and the inner cavity sand core is manufactured by using a hot core box method and green sand; Combining the shell sand core, the flow channel sand core, the sand mold and the inner cavity sand core not coated with paint for casting; After the pouring is completed, the molded casting is processed and the internal defects of the casting are detected using X-RAY detection equipment.
2. The sand casting process of a heat-resistant steel exhaust manifold according to claim 1, characterized in that: The steps of the hot box method are as follows: preheating the hot box, injecting the coated sand into the hot box through a sand injection device, performing a fire spraying treatment on the surface of the formed sand core, then maintaining the temperature of the hot box to allow the surface of the sand core to form a crust, turning the hot box over and resetting it, then maintaining the temperature of the hot box to allow the surface of the sand core to solidify, and finally taking out the inner cavity sand core from the hot box.
3. The sand casting process of a heat-resistant steel exhaust manifold according to claim 1, characterized in that: The green sand has the following components: 0-0.15% by weight of fine powder, 0.5-1.2% by weight of bentonite, 1.2-4% by weight of water, and 10±2% by weight of mud.
4. The sand casting process of a heat-resistant steel exhaust manifold according to claim 1, characterized in that: The performance parameters of the green sand are as follows: compaction rate 39.5±3%, loss on ignition 1.5±0.5%, air permeability index 180±30, wet compressive strength 195±10Kpa, and blue absorption MB value 8.5±1%.
5. The sand casting process of a heat-resistant steel exhaust manifold according to claim 2, characterized in that: The hot core box comprises a movable mold and a static mold. The preheating temperature of the movable mold and the static mold is 250±5°C. During solidification and crusting, the temperature of the movable mold and the static mold is maintained at 250±5°C.
6. The sand casting process of a heat-resistant steel exhaust manifold according to claim 2, characterized in that: The steps of the flame spraying treatment are as follows: after the sand mixture is injected into the hot core box, the entire sand core surface is immediately heated by flame spraying using a flame heating device, and the flame spraying lasts for 50±1 seconds.
7. The sand casting process of a heat-resistant steel exhaust manifold according to claim 2, characterized in that: The steps of forming a crust on the surface of the sand core are as follows: after the flame treatment, the temperature of the hot core box is maintained so that the sand material close to the surface of the hot core box is hardened by heat to form a hard shell. The whole process lasts for 20-30 seconds.
8. The sand casting process for a heat-resistant steel exhaust manifold according to claim 2, characterized in that: The steps of flipping and resetting the hot core box are as follows: flipping the hot core box to pour out the uncrusted part of the sand material, the flipping time is controlled between 20-60 seconds, and then flipping the hot core box to return it to its original position.
9. The sand casting process for a heat-resistant steel exhaust manifold according to claim 2, characterized in that: The steps of curing the surface layer of the sand core are as follows: maintaining the temperature of the hot core box for 120±1 seconds, so that the sand material hardens itself through the residual heat and the heat released by the hardening reaction.
10. The sand casting process of a heat-resistant steel exhaust manifold according to claim 1, characterized in that: According to the casting casted by the process and the inner cavity sand core manufactured, the surface roughness of the inner cavity of the casting is Ra≤12.5μm.
Citation Information
Patent Citations
Casting sand core hot box and sand core molding method
CN104162632A
Hot-box mold for prolonging pre-coated sand core exhaust passage and sand core forming method
CN108296441A
Engine flywheel casing green sand built-in functionalized precoated sand core casting mold
CN109128029A
Heat-resistant steel process for variable-section turbocharger shell
CN114523075A
Process for producing cast steel exhaust manifold from green sand
CN115945639A
Cited By
Gate valve body casting device, gate valve production process and gate valve
CN119973048A