Method for refining primary alpha phase of hypoeutectic aluminum-silicon-magnesium alloy and application

By adding trace amounts of boron and rare earth elements to the aluminum-silicon-magnesium alloy, the problems of poor refining effect and silicon poisoning in the existing technology are solved, and stable refinement and cost reduction of the aluminum-silicon-magnesium alloy are achieved.

CN118720068APending Publication Date: 2024-10-01HUAWEI DIGITAL POWER TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310377707.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

It is difficult to effectively refine the primary α phase of aluminum-silicon-magnesium alloys with existing technology, and commonly used refiners can cause silicon poisoning and high costs.

Method used

By adding trace amounts of boron and rare earth elements to the molten hypoeutectic aluminum-silicon-magnesium alloy, the first and second melts are formed and kept at a suitable temperature to achieve alloy refinement, avoiding the use of fluorine salt methods and Contains titanium refiner.

Benefits of technology

The grain refinement of the aluminum-silicon-magnesium alloy is achieved, with high stability, avoiding silicon poisoning and high costs, and simplifying the process flow.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720068A_ABST
    Figure CN118720068A_ABST
Patent Text Reader

Abstract

The invention provides a method for refining a primary alpha phase of a hypoeutectic aluminum-silicon-magnesium alloy, which comprises the following steps: adding a boron element into a molten hypoeutectic aluminum-silicon-magnesium alloy to obtain a first melt, the boron element being 0.01-0.02% by weight of the hypoeutectic aluminum-silicon-magnesium alloy; rare earth elements are added into the first melt to obtain a second melt, and the rare earth elements account for 0.06%-0.1% of the first melt according to the weight percentage; and the second melt is poured into a mold to be cooled and solidified. The invention further provides the aluminum-silicon-magnesium alloy prepared through the method. The method has a good refining effect on the primary alpha phase of the hypoeutectic aluminum-silicon-magnesium alloy, a refiner does not need to be used, the process is simple, and cost reduction is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of metal materials, and in particular to a method for refining a primary α phase of a hypoeutectic aluminum-silicon-magnesium alloy and an aluminum-silicon-magnesium alloy prepared by using the aforementioned method for refining a primary α phase of a hypoeutectic aluminum-silicon-magnesium alloy. Background Art

[0002] With the general trend of lightweight materials, many industries have adopted "aluminum instead of steel". The improvement of material casting and forming technology has enabled lightweight alloys such as aluminum alloys to achieve lightweight structural parts while meeting performance requirements, among which aluminum silicon alloys are the most widely used.

[0003] In order to further improve the performance of Al-Si-Mg alloy, obtaining fine and uniform cast structure is the key to obtain excellent performance. Summary of the invention

[0004] In view of this, the embodiment of the present application provides a method for refining the primary α phase of a hypoeutectic aluminum-silicon-magnesium alloy and an aluminum-silicon-magnesium alloy prepared by using the above method for refining the primary α phase of a hypoeutectic aluminum-silicon-magnesium alloy. The above method has a good refining effect on the primary α phase of the hypoeutectic aluminum-silicon-magnesium alloy, and does not need to use a refining agent, the process is simple and is conducive to cost reduction.

[0005] A first aspect of an embodiment of the present application provides a method for refining the primary α phase of a hypoeutectic aluminum-silicon-magnesium alloy, comprising the steps of: adding a boron element to the molten hypoeutectic aluminum-silicon-magnesium alloy to obtain a first melt, wherein, by weight percentage, the boron element is 0.01% to 0.02% of the hypoeutectic aluminum-silicon-magnesium alloy; adding a rare earth element to the first melt to obtain a second melt, wherein, by weight percentage, the rare earth element is 0.06% to 0.1% of the first melt; and pouring the second melt into a mold to cool and solidify.

[0006] The above method provided by the present application has a good refining effect on the primary α phase of the hypoeutectic aluminum-silicon-magnesium alloy by adding a trace amount of boron and rare earth elements, and the grain refining effect is stable. In addition, the above method does not need to separately prepare a refiner by a fluoride salt method to refine the primary α phase of the hypoeutectic aluminum-silicon-magnesium alloy, and the process is simple and conducive to reducing costs. At the same time, it also avoids the silicon poisoning phenomenon caused by the use of commonly used titanium-containing refiners.

[0007] Based on the first aspect, in a possible implementation manner, the boron element comes from an Al-B alloy.

[0008] In the above possible implementation, the boron element comes from the Al-B alloy, thereby avoiding the introduction of other impurity elements to interfere with the refinement effect of the alloy.

[0009] Based on the first aspect, in a possible implementation manner, the rare earth element comes from an Al-rare earth element alloy, and the rare earth element is selected from at least one of Nb, La and Ce.

[0010] In the above possible implementation, the rare earth elements come from Al-rare earth element alloy, which avoids introducing other impurity elements to interfere with the refinement effect of the alloy.

[0011] Based on the first aspect, in a possible implementation method, the step of adding boron element to the molten hypoeutectic aluminum-silicon-magnesium alloy to obtain a first melt includes: adding boron element to the molten hypoeutectic aluminum-silicon-magnesium alloy at a temperature of 720±5°C to obtain a first melt and continuing to keep warm for 10 to 20 minutes.

[0012] In the above possible implementation, the above temperature is suitable for casting of aluminum-silicon-magnesium alloy and is also conducive to avoiding the burning of magnesium in the aluminum-silicon-magnesium alloy by long-term high temperature. After adding the boron element, continuing to keep the temperature for 10 to 20 minutes is conducive to fully homogenizing the elements in the first melt, thereby preventing the generation of element segregation and further facilitating the refinement of the alloy.

[0013] Based on the first aspect, in a possible implementation, the step of adding rare earth elements to the first melt to obtain a second melt includes: adding the rare earth elements to the first melt at a temperature of 720±5°C to obtain a second melt and continuing to keep the temperature for 10 to 20 minutes.

[0014] In the above possible implementation, the above temperature is suitable for casting of aluminum-silicon-magnesium alloy and is also conducive to avoiding the burning of magnesium in the aluminum-silicon-magnesium alloy by long-term high temperature. After adding the rare earth element, continuing to keep the temperature for 10 to 20 minutes is conducive to fully homogenizing the elements in the second melt, thereby preventing the occurrence of element segregation, and further facilitating the refinement of the alloy.

[0015] Based on the first aspect, in a possible implementation, before the step of adding boron element to the molten hypoeutectic aluminum-silicon-magnesium alloy, the above-mentioned method for refining the primary α phase of the hypoeutectic aluminum-silicon-magnesium alloy also includes: heating the hypoeutectic aluminum-silicon-magnesium alloy to 650°C to 670°C and then keeping the temperature until the hypoeutectic aluminum-silicon-magnesium alloy is melted.

[0016] In the above possible implementation, the hypoeutectic aluminum-silicon-magnesium alloy is heated to 650° C. to 670° C. and then kept warm, which helps to avoid the risk of burning elements in the alloy, such as magnesium, due to high-temperature shock.

[0017] Based on the first aspect, in a possible implementation method, before the step of heating the hypoeutectic aluminum-silicon-magnesium alloy to 650°C to 670°C, the above-mentioned method for refining the primary α phase of the hypoeutectic aluminum-silicon-magnesium alloy also includes: providing a furnace and heating the furnace to 480°C to 500°C; and placing the hypoeutectic aluminum-silicon-magnesium alloy in the heated furnace.

[0018] In the above possible implementation method, the furnace is preheated before the hypoeutectic aluminum-silicon-magnesium alloy is placed in the furnace, so that the furnace is dried before the alloy is placed, avoiding the influence of water vapor in the furnace on the hypoeutectic aluminum-silicon-magnesium alloy, thereby avoiding affecting the refinement effect of the alloy.

[0019] Based on the first aspect, in a possible implementation method, before the step of adding boron element to the molten hypoeutectic aluminum-silicon-magnesium alloy, the above-mentioned method for refining the primary α phase of the hypoeutectic aluminum-silicon-magnesium alloy also includes: continuing to heat the molten hypoeutectic aluminum-silicon-magnesium alloy to 740°C to 760°C, then cooling it to 720±5°C, adding refining agent and completing refining.

[0020] In the above possible implementations, the process of heating to 740°C to 760°C is conducive to the uniform distribution of the elements in the hypoeutectic aluminum-silicon-magnesium alloy, which is conducive to preventing the occurrence of element segregation, and further conducive to the subsequent refinement of the alloy. Cooling after heating and refining at 720±5°C is conducive to avoiding the burning of magnesium in the alloy due to long-term high temperature.

[0021] Based on the first aspect, in a possible implementation, before the step of pouring the second melt into a mold for cooling and solidification, the method for refining the primary α phase of the hypoeutectic Al-Si-Mg alloy further includes: providing a mold and preheating it at a temperature not lower than 100°C for at least 30 minutes.

[0022] In the above possible implementation manner, the mold is preheated before pouring the second melt into the mold to remove water vapor on the mold to avoid the influence of water vapor on the second melt, thereby avoiding affecting the refinement effect of the alloy.

[0023] A second aspect of an embodiment of the present application provides an aluminum-silicon-magnesium alloy, which is prepared by the method of refining the primary α phase of the hypoeutectic aluminum-silicon-magnesium alloy as described above.

[0024] The aluminum-silicon-magnesium alloy produced by the above method provided in the present application effectively refines the grains during the aluminum-silicon-magnesium alloy casting process, thereby facilitating the improvement of the product performance of the aluminum-silicon-magnesium alloy casting. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic flow chart of a method for refining the primary α phase of a hypoeutectic Al-Si-Mg alloy according to an embodiment of the present application.

[0026] Figure 2 It is a schematic flow chart of a method for refining the primary α phase of a hypoeutectic Al-Si-Mg alloy according to another embodiment of the present application.

[0027] Figure 3 It is a scanning electron microscope image of the metallographic structure of the aluminum ingot of comparative example 1 of the present application.

[0028] Figure 4 It is a scanning electron microscope image of the metallographic structure of the aluminum ingot of comparative example 2 of the present application.

[0029] Figure 5 It is a scanning electron microscope image of the metallographic structure of the aluminum ingot of comparative example 3 of the present application.

[0030] Figure 6 It is a scanning electron microscope image of the metallographic structure of the aluminum ingot according to one embodiment of the present application. DETAILED DESCRIPTION

[0031] The following specific embodiments illustrate the implementation of the present application, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. Although the description of the present application will be introduced in conjunction with the embodiments, this does not mean that the features of this application are limited to the implementation. On the contrary, the purpose of introducing the application in conjunction with the implementation is to cover other options or modifications that may be extended based on the claims of the present application. In order to provide a deep understanding of the present application, the following description will include many specific details. The present application can also be implemented without using these details. In addition, in order to avoid confusion or blurring the focus of the present application, some specific details will be omitted in the description. It should be noted that the embodiments in the present application and the features in the embodiments can be combined with each other without conflict.

[0032] Hereinafter, if used, the terms "first", "second", etc. are used for descriptive purposes only and are not to be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first", "second", etc. may explicitly or implicitly include one or more of the features.

[0033] The embodiments of the present application are described below in conjunction with the accompanying drawings in the embodiments of the present application. The data range values ​​recorded in the present application should include the end values ​​unless otherwise specified.

[0034] The method of commercial aluminum alloy grain refinement is usually to add Al-TiB, Al-Ti-C and Al-Ti-BC master alloys to the metal melt. Within a certain range (0.1wt.% ~ 1.0wt.%), it can have a significant effect on refining the melt grains (such as commercial Al-5Ti-B). The addition of Al-Ti-B and Al-Ti-C will generate TiB2 or TiC particles in situ in the Al alloy melt, which plays a role in refining the grains. However, the heterogeneous core particles TiB2 continue to nucleate and grow, and the TiB2 particle size distribution in the alloy is relatively wide, which leads to low TiB2 particle utilization during the refinement process and limited refinement effect.

[0035] At the same time, the most widely used commercial refiner Al-5Ti-B will produce "Si poisoning phenomenon" when refining Al-Si alloy, resulting in almost no refining effect; and in the Al-B refiner with too high B content, B and Sr will "Sr, B mutual poisoning", so the grain refinement of industrial Al-Si alloy has always been a difficult problem in research. The present invention aims to provide a method for refining the primary α phase of hypoeutectic aluminum-silicon-magnesium alloy.

[0036] In order to solve the above problems, the present application embodiment provides a method for refining the primary α phase of the hypoeutectic Al-Si-Mg alloy. Figure 1 , the above method comprises the following steps:

[0037] Step S21, adding boron element to the molten hypoeutectic aluminum-silicon-magnesium alloy to obtain a first melt, wherein, by weight percentage, the boron element is 0.01% to 0.02% of the hypoeutectic aluminum-silicon-magnesium alloy.

[0038] Step S22, adding rare earth elements into the first melt to obtain a second melt, wherein, by weight percentage, the rare earth elements account for 0.06% to 0.1% of the first melt.

[0039] Step S23, pouring the second melt into a mold to cool and solidify. The cooling is natural cooling.

[0040] The addition of a trace amount of boron and rare earth elements in the above method has a good refining effect on the primary α phase of the hypoeutectic aluminum-silicon-magnesium alloy, and the grain refining effect is stable. In addition, the above method does not need to separately prepare a refiner by a fluoride salt method to refine the primary α phase of the hypoeutectic aluminum-silicon-magnesium alloy, and the process is simple and conducive to reducing costs. At the same time, it also avoids the silicon poisoning phenomenon caused by the use of commonly used titanium-containing refiners and the mutual poisoning phenomenon of strontium and boron.

[0041] In this embodiment, the boron element may come from an Al-B alloy, which avoids introducing other impurity elements to interfere with the refinement effect of the alloy during the refinement process. In this embodiment, the Al-B alloy may be in a powder form, which is conducive to its dispersion in the molten hypoeutectic aluminum-silicon-magnesium alloy, thereby facilitating the full homogenization of the elements in the first melt, thereby facilitating the prevention of element segregation and facilitating the refinement of the alloy. The Al-B alloy may be, but is not limited to, at least one of an Al-3wt%B alloy, an Al-5wt%B alloy, and an Al-20wt%B alloy. The rare earth element may come from an Al-rare earth element alloy, which avoids introducing other impurity elements to interfere with the refinement effect of the alloy during the refinement process. The rare earth element may be selected from at least one of Nb, La, and Ce. In this embodiment, the rare earth element is Nb, and the rare earth element may come from an Al-Nb alloy. The Al-Nb alloy is in a powder form, which is conducive to its dispersion in the first melt, thereby facilitating the full homogenization of the elements in the second melt, thereby facilitating the prevention of element segregation and facilitating the refinement of the alloy. The Al-Nb alloy may be, but is not limited to, at least one of an Al-10wt% Nb alloy and an Al-15wt% Nb alloy.

[0042] In some embodiments, the boron element may also come from other alloys. The rare earth element may also come from other alloys.

[0043] In some embodiments, in step S21, boron element may be added to the molten hypoeutectic aluminum-silicon-magnesium alloy at a temperature of 720±5°C to obtain the first melt, and the temperature is kept for 10 to 20 minutes. The hypoeutectic aluminum-silicon-magnesium alloy at 720±5°C is suitable for casting and is also beneficial for avoiding the burning of magnesium in the aluminum-silicon-magnesium alloy by long-term high temperature, and the temperature is kept for 10 to 20 minutes to fully homogenize the elements in the first melt, thereby preventing the generation of element segregation, and further facilitating the refinement of the alloy.

[0044] In some embodiments, in step S22, rare earth elements may be added to the first melt at a temperature of 720±5°C to obtain the second melt, and the temperature is kept at 10 to 20 minutes. The hypoeutectic aluminum-silicon-magnesium alloy at 720±5°C is suitable for casting and is also beneficial for avoiding the burning of magnesium in the aluminum-silicon-magnesium alloy by long-term high temperature, while keeping the temperature for 10 to 20 minutes is beneficial for fully homogenizing the elements in the second melt, thereby preventing element segregation and further facilitating the refinement of the alloy.

[0045] In some embodiments, before step S23, the above method for refining the primary α phase of the hypoeutectic aluminum-silicon-magnesium alloy may further include: providing a mold and preheating it at a temperature not lower than 100°C for at least 30 minutes. Before pouring the second melt into the mold, the mold is preheated to remove moisture on the mold to avoid the influence of moisture on the smelting quality, thereby avoiding affecting the refinement effect of the alloy. Preferably, the preheating temperature of the mold is about 200°C. Similarly, other tools used in the above method and in contact with the alloy or its melt can be preheated in the above manner before use to remove moisture.

[0046] In some embodiments, see Figure 2 Before step S21, the above method for refining the primary α phase of the hypoeutectic Al-Si-Mg alloy may further include the following steps:

[0047] Step S11, providing a furnace and heating the furnace to 480° C. to 500° C. and then placing the hypoeutectic Al-Si-Mg alloy in the furnace.

[0048] The hypoeutectic Al-Si-Mg alloy is placed in the furnace after the furnace is preheated, so that the furnace is dried before the alloy is placed, so as to avoid the influence of water vapor in the furnace on the smelting quality, thereby avoiding the influence on the refinement effect of the alloy.

[0049] The furnace may be, but is not limited to, a resistance crucible furnace.

[0050] Step S12, heating the hypoeutectic aluminum-silicon-magnesium alloy to 650° C. to 670° C. and then maintaining the temperature until the hypoeutectic aluminum-silicon-magnesium alloy is melted.

[0051] Heating the hypoeutectic aluminum-silicon-magnesium alloy to 650°C to 670°C and then keeping it warm helps to avoid the risk of burning elements in the alloy, such as magnesium, due to high-temperature shock during the melting process.

[0052] Step S13, further heating the molten hypoeutectic aluminum-silicon-magnesium alloy to 740° C. to 760° C., cooling it to 720±5° C., adding a refining agent and completing the refining.

[0053] The process of heating to 740°C to 760°C is conducive to the uniform distribution of the elements in the hypoeutectic aluminum-silicon-magnesium alloy, which is conducive to preventing the segregation of elements and further conducive to the subsequent refinement of the alloy. After heating, cooling to 720±5°C for refining is conducive to avoiding the burning of magnesium in the alloy due to long-term high temperature.

[0054] The refining agent may be but is not limited to hexachloroethane.

[0055] In some embodiments, at least one of the above step S11 and step S13 may be omitted.

[0056] The embodiment of the present application also provides an aluminum-silicon-magnesium alloy, which is prepared by the method of refining the primary α phase of the hypoeutectic aluminum-silicon-magnesium alloy as described above. The aluminum-silicon-magnesium alloy prepared by the above method effectively refines the grains during the aluminum-silicon-magnesium alloy casting process, thereby facilitating the improvement of the product performance of the aluminum-silicon-magnesium alloy casting.

[0057] The present application is described in more detail below using examples and comparative examples. However, the following examples are only provided to help understand the present application, and the content of the present application is not limited by the following examples.

[0058] Comparative Example 1

[0059] After heating the resistance crucible furnace to 500°C, add the hypoeutectic aluminum-silicon-magnesium alloy (Al-7Si-0.3Mg) raw material, heat the raw material to 650°C and keep it warm until the raw material melts. Heat the molten raw material to 750°C, cool it to 720°C, add hexachloroethane for refining, and keep it warm for 15 minutes after the refining is completed to obtain a melt. Provide a mold preheated at 200°C for 30 minutes, and pour the above melt into the mold to cool and solidify to obtain an aluminum ingot.

[0060] Take samples of aluminum ingots and observe the metallographic structure. Figure 3 .

[0061] Comparative Example 2

[0062] After heating the resistance crucible furnace to 500°C, add the hypoeutectic aluminum-silicon-magnesium alloy (Al-7Si-0.3Mg) raw material, heat the raw material to 650°C and keep it warm until the raw material melts. Heat the molten raw material to 750°C, cool it to 720°C, and add hexachloroethane to complete the refining. Add 0.08% niobium element (in the form of Al-10wt% Nb alloy) based on the weight of the hypoeutectic aluminum-silicon-magnesium alloy raw material to the refined molten hypoeutectic aluminum-silicon-magnesium alloy at a temperature of 720°C, and keep it warm for 15 minutes to obtain a melt. Provide a mold preheated at 200°C for 30 minutes, and pour the above melt into the mold to cool and solidify to obtain an aluminum ingot.

[0063] Take samples of aluminum ingots and observe the metallographic structure. Figure 4 .

[0064] Comparative Example 3

[0065] After heating the resistance crucible furnace to 500°C, add the hypoeutectic aluminum-silicon-magnesium alloy (Al-7Si-0.3Mg) raw material, heat the raw material to 650°C and keep it warm until the raw material melts. Heat the molten raw material to 750°C, cool it to 720°C, and add hexachloroethane to complete the refining. Add 0.01% of the boron element (in the form of Al-3wt% B alloy) based on the weight of the hypoeutectic aluminum-silicon-magnesium alloy raw material to the refined molten hypoeutectic aluminum-silicon-magnesium alloy at a temperature of 720°C, and keep it warm for 15 minutes to obtain a melt. Provide a mold preheated at 200°C for 30 minutes, and pour the above melt into the mold to cool and solidify to obtain an aluminum ingot.

[0066] Take samples of aluminum ingots and observe the metallographic structure. Figure 5 .

[0067] Example

[0068] After heating the resistance crucible furnace to 500°C, add the hypoeutectic aluminum-silicon-magnesium alloy (Al-7Si-0.3Mg) raw material, heat the raw material to 650°C and keep it warm until the raw material melts. Heat the molten raw material to 750°C, cool it to 720°C, and add hexachloroethane to complete the refining. Add 0.01% of the boron element (in the form of Al-3wt% B alloy) based on the weight of the hypoeutectic aluminum-silicon-magnesium alloy raw material to the refined molten hypoeutectic aluminum-silicon-magnesium alloy at a temperature of 720°C, and keep it warm for 15 minutes to obtain the first melt. Add 0.08% of the niobium element (in the form of Al-10wt% Nb alloy) based on the weight of the hypoeutectic aluminum-silicon-magnesium alloy raw material to the first melt at a temperature of 720°C, and keep it warm for 15 minutes to obtain the second melt. Provide a mold preheated at 200°C for 30 minutes, and pour the above second melt into the mold to cool and solidify to obtain an aluminum ingot.

[0069] Take samples of aluminum ingots and observe the metallographic structure. Figure 6 .

[0070] It can be seen from the metallographic structures of the aluminum ingots corresponding to the above-mentioned comparative examples 1-3 and the embodiment that the grain structure of the aluminum ingot corresponding to the embodiment has a better refinement effect than that of comparative examples 1-3.

[0071] It should be noted that the above are only specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application; the implementation methods of the present application and the features in the implementation methods can be combined with each other without conflict. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.

Claims

1. A method for refining the primary α phase of a hypoeutectic aluminum-silicon-magnesium alloy, characterized in that: Includes steps: Adding boron to the molten hypoeutectic aluminum-silicon-magnesium alloy to obtain a first melt, wherein the boron element is 0.01% to 0.02% by weight of the hypoeutectic aluminum-silicon-magnesium alloy; Adding a rare earth element to the first melt to obtain a second melt, wherein the rare earth element is 0.06% to 0.1% by weight of the first melt; and The second melt is poured into a mold to be cooled and solidified.

2. The method for refining the primary α phase of hypoeutectic Al-Si-Mg alloy according to claim 1, characterized in that: The boron element comes from Al-B alloy.

3. The method for refining the primary α phase of hypoeutectic Al-Si-Mg alloy according to claim 1, characterized in that: The rare earth element comes from an Al-rare earth element alloy, and the rare earth element is selected from at least one of Nb, La and Ce.

4. The method for refining the primary α phase of hypoeutectic Al-Si-Mg alloy according to claim 1, characterized in that: The step of adding boron element to the molten hypoeutectic aluminum-silicon-magnesium alloy to obtain a first melt comprises: Boron element is added into the molten hypoeutectic aluminum-silicon-magnesium alloy at a temperature of 720±5°C to obtain a first melt and the first melt is kept warm for 10 to 20 minutes.

5. The method for refining the primary α phase of hypoeutectic Al-Si-Mg alloy according to claim 4, characterized in that: The step of adding rare earth elements to the first melt to obtain a second melt comprises: The rare earth element is added into the first melt at a temperature of 720±5° C. to obtain a second melt and the temperature is kept constant for 10 to 20 minutes.

6. The method for refining the primary α phase of a hypoeutectic Al-Si-Mg alloy according to any one of claims 1 to 5, characterized in that: Before the step of adding boron element to the molten hypoeutectic aluminum-silicon-magnesium alloy, the method further comprises: The hypoeutectic aluminum-silicon-magnesium alloy is heated to 650° C. to 670° C. and then kept warm until the hypoeutectic aluminum-silicon-magnesium alloy is melted.

7. The method for refining the primary α phase of hypoeutectic Al-Si-Mg alloy according to claim 6, characterized in that: Before the step of heating the hypoeutectic aluminum-silicon-magnesium alloy to 650° C. to 670° C., the method further comprises: Providing a furnace and heating the furnace to 480° C. to 500° C.; and The hypoeutectic aluminum-silicon-magnesium alloy is placed in the heated furnace.

8. The method for refining the primary α phase of hypoeutectic Al-Si-Mg alloy according to claim 6, characterized in that: Before the step of adding boron element to the molten hypoeutectic aluminum-silicon-magnesium alloy, the method further comprises: The molten hypoeutectic aluminum-silicon-magnesium alloy is further heated to 740° C. to 760° C., then cooled to 720±5° C., a refining agent is added, and refining is completed.

9. The method for refining the primary α phase of hypoeutectic Al-Si-Mg alloy according to claim 1, characterized in that: Before the step of pouring the second melt into a mold for cooling and solidification, the method further comprises: Provide a mold and preheat it at a temperature not less than 100°C for at least 30 minutes.

10. An aluminum-silicon-magnesium alloy, characterized in that: The Al-Si-Mg alloy is prepared by the method for refining the primary α phase of the hypoeutectic Al-Si-Mg alloy as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Al-Si-Mg-Sm rare earth cast aluminum alloy and preparation method thereof

    CN102758108A

  • Tissue control method for near-eutectic cast aluminum-silicon alloy

    CN103938004A

  • High-performance cast near-eutectic aluminium-silicon alloy for pressure-containing parts and preparation method thereof

    CN103938036A

  • Cast aluminum alloy with high strength and tenacity and preparation method thereof

    CN105803272A

  • High-strength and high-toughness die-cast aluminum alloy and preparation method thereof

    CN108034870A