Niobium alloy ingot casting riser feeding method
Through vacuum consumable melting and two-stage feeding method of constant current reduction and low current maintenance, the problem of low yield and high production cost of niobium alloy ingots was solved, the riser depth was controlled within 50mm, and the finished product was improved. efficiency and reduce production costs.
Patent Information
- Application Number
- CN202410849249.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-01
AI Technical Summary
The feeding process of niobium alloy ingots is difficult. The step-by-step current reduction and maintenance method used in the preparation of conventional titanium, zirconium and their alloy ingots is not suitable for niobium alloys, resulting in low ingot yield and high production costs.
The vacuum consumable melting method is used to smelt the finished product of niobium alloy ingots, and in the stable stage of smelting, it is switched to a two-stage feeding method of uniform continuous current reduction and low current maintenance to control the smelting process parameters, reduce the melting speed, and avoid the depth of the molten pool. Too fast a drop and rapid loss of heat.
It effectively reduces the amount of sawing at the riser of niobium alloy ingots, increases the yield by about 5%, reduces production costs, and the process is repeatable and stable.
Smart Images

Figure CN118720072A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of niobium alloy ingot preparation, and in particular relates to a method for feeding shrinkage of a riser of a niobium alloy ingot. Background Art
[0002] Niobium alloy has excellent high temperature performance, good processing performance, and good plasticity, so it is widely used in aerospace, nuclear reactors and other industries. It has become the main material for manufacturing rocket engine radiation cooling nozzles. In addition, niobium alloy has excellent superconducting properties and is a relatively practical and low-cost superconducting material.
[0003] In addition, niobium alloy has a high melting point and high viscosity and belongs to the category of refractory metals. It is difficult to melt and feed the ingots. Unreasonable process parameters for ingot melting and feeding will directly reduce the quality and yield rate of the ingot products. In addition, niobium alloy raw materials are expensive, and a low yield rate will greatly increase production costs.
[0004] However, the step-by-step current reduction and shrinkage feeding method used in the preparation of conventional titanium, zirconium and their alloy ingots is not suitable for niobium alloy ingots. The multi-stage current maintenance shrinkage feeding method is not conducive to reducing the melting rate of niobium alloy. In addition, due to the high viscosity of niobium alloy, the multi-stage current maintenance shrinkage feeding method is also likely to cause the shrinkage hole position of the finished niobium alloy ingot to be deep, and the shrinkage hole depth is usually more than 80mm, which leads to a low yield rate of niobium alloy ingots. Therefore, it is very necessary to propose a niobium alloy ingot riser shrinkage feeding method that can effectively increase the shrinkage hole position, reduce the riser sawing amount, improve the yield rate and reduce the production cost. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a method for feeding shrinkage at the riser of a niobium alloy ingot, wherein the method for feeding shrinkage at the riser of a niobium alloy ingot can effectively improve the position of the shrinkage cavity, reduce the amount of riser sawing, increase the yield rate by about 5% and significantly reduce the production cost.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] The implementation scheme provided by the present invention is a method for feeding shrinkage of a riser of a niobium alloy ingot, comprising the following steps:
[0008] Using niobium alloy as a consumable electrode, a vacuum consumable melting method is used to melt the niobium alloy ingot finished product to obtain the niobium alloy ingot;
[0009] After the niobium alloy enters the shrinkage feeding stage from the smelting stability stage in the finished product smelting, the riser shrinkage is fed by two stages of uniform speed continuous current reduction and low current maintenance.
[0010] Preferably, the reduction rate of each section of the two sections of uniform-speed continuous current reduction is 500-1000 A / min and 100-350 A / min respectively.
[0011] Preferably, the low current is maintained until the end of the feeding stage, wherein the low current is 4.0-10.0 kA.
[0012] Preferably, the size of the niobium alloy consumable electrode for finished product smelting is Φ80-Φ240 mm. When the weight of the niobium alloy consumable electrode for finished product smelting is 1 / 6-1 / 4 times the weight of the entire niobium alloy consumable electrode for finished product smelting, the finished product smelting enters the feeding stage from the smelting stabilization stage.
[0013] Preferably, the size of the water-cooled copper crucible used for smelting the finished product is Φ160-Φ300 mm.
[0014] Preferably, the smelting current in the stable smelting stage is 7.0-18.0 kA, the smelting voltage setting value in the stable smelting stage is 20.0-45.0 V, the arc stabilizing current is AC 5-10 A, and the commutation period is 10-15 s.
[0015] Preferably, the allowable fluctuation range of the smelting current in the stable smelting stage is ±2kA of the melting current setting value in the stable smelting stage, and the allowable fluctuation range of the melting voltage in the stable smelting stage is ±5V of the melting voltage setting value in the stable smelting stage.
[0016] Preferably, the cooling water inlet temperature is controlled at 18.0-25.0°C; the cooling water outlet temperature is controlled at 25.0-35.0°C, so as to obtain a full molten pool.
[0017] Preferably, vacuum consumable smelting is used for final smelting of niobium alloy ingots. To ensure the smelting vacuum environment, a gas leakage rate test should be performed to ensure that it is less than 0.8 Pa / min.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1. The technical problem to be solved by the present invention is to propose a method for feeding the riser of a finished niobium alloy ingot in view of the difficulty of the feeding process of niobium alloy ingots. The method carries out the finished smelting process of niobium alloy ingots by vacuum consumable smelting, controls the smelting process parameters of the finished smelting and feeding stage of niobium alloy ingots, adopts two-stage uniform speed continuous current reduction and low current holding mode to feed the finished niobium alloy ingots, and the remaining weight of the consumable electrode at the beginning of the feeding stage is about 1 / 6 to 1 / 4 of the total weight of the whole consumable electrode. The method can obtain a finished niobium alloy ingot with a riser depth of ≤50mm, which proves the feasibility and stability of the process. The process can improve the yield rate of niobium alloy ingots, save production costs, and obtain a method for preparing niobium alloy ingots with a high yield rate.
[0020] 2. The present invention adopts a two-stage uniform speed continuous current reduction and low current maintenance smelting feeding method to feed the riser in the feeding stage. The finished niobium alloy ingot can obtain a riser depth of 50 mm or less, which improves the product yield and quality. In addition, the process method has repeatability and considerable stability, and the yield rate is increased by about 5%, which has certain economic value. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a current system diagram of the feeding process of the Φ160mm niobium alloy ingot of the present invention;
[0022] Figure 2 This is a current system diagram of the feeding process of a Φ220mm niobium alloy ingot of the present invention;
[0023] Figure 3 This is a current system diagram of the feeding process of a Φ300mm niobium alloy ingot of the present invention; DETAILED DESCRIPTION
[0024] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the protection scope of the present invention. The experimental methods described in the embodiments of the present invention are conventional methods unless otherwise specified.
[0025] The inventors found that the voltage fluctuates greatly during the smelting process of niobium alloy because the viscosity of niobium alloy is high and the molten droplets will be elongated and then drip instead of dripping directly. If the multi-stage current maintenance shrinkage feeding method is directly adopted, it is easy to cause the shrinkage hole position of the finished niobium alloy ingot to be deep. The shrinkage hole depth is usually more than 80mm, which leads to a low yield of niobium alloy ingots.
[0026] In order to improve the yield rate and reduce production costs, the shrinkage compensation method provided by the present invention adopts a two-stage uniform and continuous current reduction method. In the first stage, the current reduction rate is controlled within an appropriate range to continuously reduce the melting rate and reduce the depth of the molten pool to avoid the rebound of the melting rate in the maintenance stage after the conventional current reduction. The current reduction is too fast, resulting in rapid loss of heat in the molten pool and rapid solidification, and effective liquid compensation cannot be performed. If the current is reduced too slowly, the melting rate is still at a high level and the depth of the molten pool decreases slowly, both of which may lead to poor shrinkage position lifting effect. After the first stage of rapid current reduction, the melting rate is greatly slowed down, the depth of the molten pool decreases rapidly, and the current value is relatively close to the minimum smelting current at this time. If the current continues to decrease at a high speed, no metal liquid will drip, the upper surface of the molten pool will solidify and cover first, and the shrinkage position cannot continue to be improved. Therefore, the current reduction rate needs to be slowed down in the second stage to ensure that the molten pool continues to become shallower and the top is not covered with a low melting rate, so that the shrinkage hole has sufficient time and conditions to continue to float up; the purpose of slowing down the current rate in the second stage is to further reduce the depth of the molten pool on the one hand, and to delay the excessive solidification of the upper surface of the molten pool on the other hand, which causes the shrinkage position to sink.
[0027] When the riser shrinkage is fed by low current maintenance after two stages of continuous current reduction at a uniform speed, the purpose of low current maintenance is to maintain the molten pool baking state at an extremely low melting speed, continuously provide heat to the upper part of the molten pool, and ensure that the upper surface is not sealed.
[0028] The technical solution of the present invention is further illustrated below in the form of specific examples.
[0029] Example 1
[0030] The method for feeding the riser of Φ160mm finished niobium alloy ingot mainly includes the following steps:
[0031] Step 1: Smelt the final product of niobium alloy ingot by vacuum consumable smelting. To ensure the vacuum environment of smelting, the leakage rate test should be carried out in the welding and smelting process in the furnace to ensure that it does not exceed 0.8Pa / min. In this embodiment, the consumable electrode has a specification of Φ80mm, the water-cooled copper crucible is cylindrical, and the specification of the water-cooled copper crucible is Φ160×L mm (i.e., the diameter is Φ160, and the height is not limited). In order to ensure that the material is clean and not polluted, the auxiliary electrode uses pure niobium or the same grade of material. The same grade of material here refers to the auxiliary electrode with the same grade as the consumable electrode. The process parameters include: the current setting value is 7.0kA in the stable stage of finished product smelting, the allowable fluctuation range is 6.0-8.0kA during the process, the smelting voltage setting value is 35.0V, the allowable voltage fluctuation range is 20.0-45.0V during the process, the arc stabilization current is AC 5.0A, the commutation period is 10s, and at the same time, the inlet and outlet water temperatures of the cooling water are controlled in the range of 18.0-25.0℃ and 25.0-35.0℃ respectively, so as to obtain a full molten pool.
[0032] Step 2: When the remaining weight of the niobium alloy consumable electrode reaches 1 / 6 to 1 / 4 of the initial weight, the stable smelting stage is transferred to the finished product feeding stage, and the step-by-step current reduction and low current maintenance feeding process is implemented to feed the niobium alloy ingot riser. Figure 1 As shown in the figure, during the shrinkage compensation stage of the finished product, it is divided into two parts. The first part is two stages of continuous current reduction, and the second part is a low current holding stage. First, in the initial current reduction stage of the continuous current reduction stage, the melting current reduction rate is maintained at 500A / min within 5 to 8 minutes, and the melting rate is gradually reduced. Then, the melting current reduction rate is maintained at 100A / min within 10 to 15 minutes to reduce the depth of the molten pool; the second part uses a low current of 4.0kA to maintain until the end of the shrinkage compensation stage to increase the shrinkage position. After the 1# niobium alloy ingot is cooled and taken out of the furnace, the riser is machined for flaw detection and sawing. The distance from the lower end of the shrinkage hole to the end face of the ingot head is 47mm.
[0033] Example 2
[0034] The method for feeding the riser of Φ160mm finished niobium alloy ingot mainly includes the following steps:
[0035] Step 1: The final finished product smelting of niobium alloy ingots is carried out by vacuum consumable smelting. To ensure the smelting vacuum environment, the leakage rate test should be carried out in the welding and smelting processes in the furnace to ensure that it does not exceed 0.8Pa / min. In this embodiment, the consumable electrode specification is Φ80mm, and the water-cooled copper crucible specification is Φ160×L mm. In order to ensure that the material is clean and not polluted, the auxiliary electrode uses pure niobium or the same grade of material. The process parameters include: the current setting value is 7.0kA in the stable stage of finished product smelting, the allowable fluctuation range during the process is 6.0~8.0kA, the smelting voltage setting value is 35.0V, the allowable voltage fluctuation range during the process is 20.0~45.0V, the arc stabilization current is selected to be AC 5.0A, the commutation period is 10s, and at the same time, the inlet and outlet water temperatures of the cooling water are controlled in the range of 18.0~25.0℃ and 25.0~35.0℃, respectively, so as to obtain a full molten pool.
[0036] Step 2: When the remaining weight of the niobium alloy consumable electrode reaches 1 / 6 to 1 / 4 of the initial weight, the stable smelting stage is transferred to the finished product feeding stage, and the step-by-step current reduction and low current maintenance feeding process is implemented to feed the niobium alloy ingot riser. Figure 1As shown in the figure, during the shrinkage compensation stage of the finished product, it is divided into two parts. The first part is two stages of continuous current reduction, and the second part is a low current holding stage. First, in the continuous current reduction stage, the initial current reduction stage is 5 to 8 minutes, the melting current reduction rate is maintained at 500A / min, and the melting rate is gradually reduced. Then, the melting current reduction rate is maintained at 100A / min within 10 to 15 minutes to reduce the depth of the molten pool; the second part uses a low current of 4.0kA to maintain until the end of the shrinkage compensation stage to increase the shrinkage position. After the 2# niobium alloy ingot is cooled and taken out of the furnace, the riser is machined for flaw detection and sawing. The distance from the lower end of the shrinkage hole to the end face of the ingot head is 42mm.
[0037] Example 3
[0038] The method for feeding the riser of Φ160mm finished niobium alloy ingot mainly includes the following steps:
[0039] Step 1: The final finished product smelting of niobium alloy ingots is carried out by vacuum consumable smelting. To ensure the smelting vacuum environment, the leakage rate test should be carried out in the welding and smelting processes in the furnace to ensure that it does not exceed 0.8Pa / min. In this embodiment, the specification of the consumable electrode is Φ100mm, and the specification of the water-cooled copper crucible is Φ160×Lmm. In order to ensure that the material is clean and not polluted, the auxiliary electrode uses pure niobium or the same grade of material. The process parameters include: the current setting value is 7.0kA in the stable stage of finished product smelting, the allowable fluctuation range during the process is 6.0~8.0kA, the smelting voltage setting value is 35.0V, the allowable voltage fluctuation range during the process is 20.0~45.0V, the arc stabilization current is selected to be AC 5.0A, the commutation period is 10s, and at the same time, the inlet and outlet temperatures of the cooling water are controlled in the range of 18.0~25.0℃ and 25.0~35.0℃, respectively, so as to obtain a full molten pool.
[0040] Step 2: When the remaining weight of the niobium alloy consumable electrode reaches 1 / 6 to 1 / 4 of the initial weight, the stable smelting stage is transferred to the finished product feeding stage, and the step-by-step current reduction and low current maintenance feeding process is implemented to feed the niobium alloy ingot riser. Figure 1 As shown in the figure, during the shrinkage compensation stage of the finished product, it is divided into two parts. The first part is two stages of continuous current reduction, and the second part is a low current holding stage. First, in the initial current reduction stage of the continuous current reduction stage, the melting current reduction rate is maintained at 550A / min within 5 to 8 minutes, and the melting rate is gradually reduced. Then, the melting current reduction rate is maintained at 120A / min within 10 to 15 minutes to reduce the depth of the molten pool; the second part uses a low current of 4.0kA to maintain until the end of the shrinkage compensation stage to increase the shrinkage position. After the 3# niobium alloy ingot is cooled and taken out of the furnace, the riser is machined for flaw detection and sawing. The distance from the lower end of the shrinkage hole to the end face of the ingot head is 39mm.
[0041] Example 4
[0042] The method for feeding the riser of Φ160mm finished niobium alloy ingot mainly includes the following steps:
[0043] Step 1: The final finished product smelting of niobium alloy ingots is carried out by vacuum consumable smelting. To ensure the smelting vacuum environment, the leakage rate test should be carried out in the welding and smelting processes in the furnace to ensure that it does not exceed 0.8Pa / min. In this embodiment, the specification of the consumable electrode is Φ100mm, and the specification of the water-cooled copper crucible is Φ160×L mm. In order to ensure that the material is clean and not polluted, the auxiliary electrode uses pure niobium or the same grade of material. The process parameters include: the current setting value is 7.0kA in the stable stage of finished product smelting, the fluctuation range allowed during the process is 6.0~8.0kA, the smelting voltage setting value is 35.0V, the voltage fluctuation range allowed during the process is 20.0~45.0V, the arc stabilization current is selected as AC 5.0A, the commutation period is 10s, and at the same time, the inlet and outlet temperatures of the cooling water are controlled in the range of 18.0~25.0℃ and 25.0~35.0℃, respectively, so as to obtain a full molten pool.
[0044] Step 2: When the remaining weight of the niobium alloy consumable electrode reaches 1 / 6 to 1 / 4 of the initial weight, the stable smelting stage is transferred to the finished product feeding stage, and the step-by-step current reduction and low current maintenance feeding process is implemented to feed the niobium alloy ingot riser. Figure 1 As shown in the figure, during the shrinkage compensation stage of the finished product, it is divided into two parts. The first part is two stages of continuous current reduction, and the second part is a low current holding stage. First, in the initial current reduction stage of the continuous current reduction stage, the melting current reduction rate is maintained at 550A / min within 5 to 8 minutes, and the melting rate is gradually reduced. Then, the melting current reduction rate is maintained at 120A / min within 10 to 15 minutes to reduce the depth of the molten pool; the second part uses a low current of 4.0kA to maintain until the end of the shrinkage compensation stage to increase the shrinkage position. After the 4# niobium alloy ingot is cooled and taken out of the furnace, the riser is machined for flaw detection and sawing. The distance from the lower end of the shrinkage hole to the end face of the ingot head is 45mm.
[0045] Example 5
[0046] The method for feeding the riser of Φ160mm finished niobium alloy ingot mainly includes the following steps:
[0047] Step 1: The final finished product smelting of niobium alloy ingots is carried out by vacuum consumable smelting. To ensure the smelting vacuum environment, the leakage rate test should be carried out in the welding and smelting processes in the furnace to ensure that it does not exceed 0.8Pa / min. In this embodiment, the consumable electrode specification is Φ110mm, and the water-cooled copper crucible specification is Φ160×Lmm. In order to ensure that the material is clean and not polluted, the auxiliary electrode uses pure niobium or the same grade of material. The process parameters include: the current setting value is 7.0kA in the stable stage of finished product smelting, the allowable fluctuation range during the process is 6.0~8.0kA, the smelting voltage setting value is 35.0V, the allowable voltage fluctuation range during the process is 20.0~45.0V, the arc stabilization current is selected to be AC 5.0A, the commutation period is 10s, and at the same time, the inlet and outlet water temperatures of the cooling water are controlled in the range of 18.0~25.0℃ and 25.0~35.0℃, respectively, so as to obtain a full molten pool.
[0048] Step 2: When the remaining weight of the niobium alloy consumable electrode reaches 1 / 6 to 1 / 4 of the initial weight, the stable smelting stage is transferred to the finished product feeding stage, and the step-by-step current reduction and low current maintenance feeding process is implemented to feed the niobium alloy ingot riser. Figure 1 As shown in the figure, during the shrinkage compensation stage of the finished product, it is divided into two parts. The first part is two stages of continuous current reduction, and the second part is a low current holding stage. First, in the initial current reduction stage of the continuous current reduction stage, the melting current reduction rate is maintained at 580A / min within 5 to 8 minutes, and the melting rate is gradually reduced. Then, the melting current reduction rate is maintained at 150A / min within 10 to 15 minutes to reduce the depth of the molten pool; the second part uses a low current of 4.0kA to maintain until the end of the shrinkage compensation stage to increase the shrinkage position. After the 5# niobium alloy ingot is cooled and taken out of the furnace, the riser is machined for flaw detection and sawing, and the distance from the lower end of the shrinkage hole to the end face of the ingot head is 50mm.
[0049] Example 6
[0050] The method for feeding the riser of Φ160mm finished niobium alloy ingot mainly includes the following steps:
[0051] Step 1: The final finished product smelting of niobium alloy ingots is carried out by vacuum consumable smelting. To ensure the smelting vacuum environment, the leakage rate test should be carried out in the welding and smelting processes in the furnace to ensure that it does not exceed 0.8Pa / min. In this embodiment, the consumable electrode specification is Φ110mm, and the water-cooled copper crucible specification is Φ160×Lmm. In order to ensure that the material is clean and not polluted, the auxiliary electrode uses pure niobium or the same grade of material. The process parameters include: the current setting value is 7.0kA in the stable stage of finished product smelting, the allowable fluctuation range during the process is 6.0~8.0kA, the smelting voltage setting value is 35.0V, the allowable voltage fluctuation range during the process is 20.0~45.0V, the arc stabilization current is selected to be AC 5.0A, the commutation period is 10s, and at the same time, the inlet and outlet water temperatures of the cooling water are controlled in the range of 18.0~25.0℃ and 25.0~35.0℃, respectively, so as to obtain a full molten pool.
[0052] Step 2: When the remaining weight of the niobium alloy consumable electrode reaches 1 / 6 to 1 / 4 of the initial weight, the stable smelting stage is transferred to the finished product feeding stage, and the step-by-step current reduction and low current maintenance feeding process is implemented to feed the niobium alloy ingot riser. Figure 1 As shown in the figure, during the shrinkage compensation stage of the finished product, it is divided into two parts. The first part is two stages of continuous current reduction, and the second part is a low current maintenance stage. First, the initial current reduction stage system is to maintain the melting current reduction rate at 580A / min within 5 to 8 minutes, gradually reduce the melting rate, and then maintain the melting current reduction rate at 150A / min within 10 to 15 minutes to reduce the depth of the molten pool; the second part uses a low current of 4.0kA to maintain until the end of the shrinkage compensation stage to increase the shrinkage position. After the 6# niobium alloy ingot is cooled and taken out of the furnace, the riser is machined for flaw detection and sawing. The distance from the lower end of the shrinkage hole to the end face of the ingot head is 46mm.
[0053] Table 1 below shows the repeatability and stability test of the feeding process for 6 niobium alloy ingots of the same specification #1~#6Φ160mm. The feeding test process parameters and riser depth of the Φ160mm niobium alloy ingot are shown in Table 1.
[0054] Table 1 Niobium alloy ingot feeding test process parameters and riser depth
[0055]
[0056]
[0057] After setting and executing the shrinkage feeding process for 6 niobium alloy ingots of the same specification #1~#6Φ160mm, the depth of the ingot riser detected after machining was ≤50mm, the shrinkage feeding effect was stable, the yield rate of niobium alloy ingots was improved, the waste of raw materials was reduced, and the shrinkage feeding solidification process of Φ160mm ingot niobium alloy was obtained.
[0058] Example 7
[0059] The method for feeding the riser of Φ220mm finished niobium alloy ingot mainly includes the following steps:
[0060] Step 1: The final finished product smelting of niobium alloy ingots is carried out by vacuum consumable smelting. To ensure the smelting vacuum environment, the leakage rate test should be carried out in the welding and smelting processes in the furnace to ensure that it does not exceed 0.8Pa / min. In this embodiment, the consumable electrode specification is Φ150mm, and the water-cooled copper crucible specification is Φ220×Lmm. In order to ensure that the material is clean and not polluted, the auxiliary electrode uses pure niobium or the same grade of material. The process parameters include: the current setting value is 11.0kA in the stable stage of finished product smelting, the allowable fluctuation range in the process is 10.0~13.0kA, the smelting voltage setting value is 35.0V, the allowable voltage fluctuation range in the process is 20.0~45.0V, the arc stabilization current is selected to be AC 6.0A, the commutation period is 10s, and at the same time, the inlet and outlet water temperatures of the cooling water are controlled in the range of 18.0~25.0℃ and 25.0~35.0℃, respectively, so as to obtain a full molten pool.
[0061] Step 2: When the remaining weight of the niobium alloy consumable electrode reaches 1 / 6 to 1 / 4 of the initial weight, the stable smelting stage is transferred to the finished product feeding stage, and the step-by-step current reduction and low current maintenance feeding process is implemented to feed the niobium alloy ingot riser. Figure 2 As shown in the figure, during the shrinkage compensation stage of the finished product, it is divided into two parts. The first part is two stages of continuous current reduction, and the second part is a low current holding stage. First, in the initial current reduction stage of the continuous current reduction stage, the melting current reduction rate is maintained at 600A / min within 5 to 8 minutes, and the melting rate is gradually reduced. Then, the melting current reduction rate is maintained at 170A / min within 10 to 15 minutes to reduce the depth of the molten pool; the second part uses a low current of 6.0kA to maintain until the end of the shrinkage compensation stage to increase the shrinkage position. After the 7# niobium alloy ingot is cooled and taken out of the furnace, the riser is machined for flaw detection and sawing. The distance from the lower end of the shrinkage hole to the end face of the ingot head is 48mm.
[0062] Example 8
[0063] The method for feeding the riser of Φ220mm finished niobium alloy ingot mainly includes the following steps:
[0064] Step 1: The final finished product smelting of niobium alloy ingots is carried out by vacuum consumable smelting. To ensure the smelting vacuum environment, the leakage rate test should be carried out in the welding and smelting processes in the furnace to ensure that it does not exceed 0.8Pa / min. In this embodiment, the consumable electrode specification is Φ150mm, and the water-cooled copper crucible specification is Φ220×Lmm. In order to ensure that the material is clean and not polluted, the auxiliary electrode uses pure niobium or the same grade of material. The process parameters include: the current setting value is 11.0kA in the stable stage of finished product smelting, the allowable fluctuation range in the process is 10.0~13.0kA, the smelting voltage setting value is 35.0V, the allowable voltage fluctuation range in the process is 20.0~45.0V, the arc stabilization current is selected to be AC 6.0A, the commutation period is 10s, and at the same time, the inlet and outlet water temperatures of the cooling water are controlled in the range of 18.0~25.0℃ and 25.0~35.0℃, respectively, so as to obtain a full molten pool.
[0065] Step 2: When the remaining weight of the niobium alloy consumable electrode reaches 1 / 6 to 1 / 4 of the initial weight, the stable smelting stage is transferred to the finished product feeding stage, and the step-by-step current reduction and low current maintenance feeding process is implemented to feed the niobium alloy ingot riser. Figure 2 As shown in the figure, during the shrinkage compensation stage of the finished product, it is divided into two parts. The first part is two stages of continuous current reduction, and the second part is a low current holding stage. First, in the initial current reduction stage of the continuous current reduction stage, the melting current reduction rate is maintained at 600A / min within 5 to 8 minutes, and the melting rate is gradually reduced. Then, the melting current reduction rate is maintained at 170A / min within 10 to 15 minutes to reduce the depth of the molten pool; the second part uses a low current of 6.0kA to maintain until the end of the shrinkage compensation stage to increase the shrinkage position. After the 8# niobium alloy ingot is cooled and taken out of the furnace, the riser is machined for flaw detection and sawing. The distance from the lower end of the shrinkage hole to the end face of the ingot head is 43mm.
[0066] Example 9
[0067] The method for feeding the riser of Φ220mm finished niobium alloy ingot mainly includes the following steps:
[0068] Step 1: The final finished product smelting of niobium alloy ingots is carried out by vacuum consumable smelting. To ensure the smelting vacuum environment, the leakage rate test should be carried out in the furnace welding and smelting process to ensure that it does not exceed 0.8Pa / min. In this embodiment, the consumable electrode specification is Φ160mm, and the water-cooled copper crucible specification is Φ220×Lmm. In order to ensure that the material is clean and not polluted, the auxiliary electrode uses pure niobium or the same grade of material. The process parameters include: the current setting value is 11.0kA in the stable stage of finished product smelting, the allowable fluctuation range in the process is 10.0~13.0kA, the smelting voltage setting value is 35.0V, the allowable voltage fluctuation range in the process is 20.0~45.0V, the arc stabilization current is selected to be AC 6.0A, the commutation period is 10s, and at the same time, the cooling water inlet and outlet water temperatures are controlled in the range of 18.0~25.0℃ and 25.0~35.0℃, respectively, so as to obtain a full molten pool.
[0069] Step 2: When the remaining weight of the niobium alloy consumable electrode reaches 1 / 6 to 1 / 4 of the initial weight, the stable smelting stage is transferred to the finished product feeding stage, and the step-by-step current reduction and low current maintenance feeding process is implemented to feed the niobium alloy ingot riser. Figure 2 As shown in the figure, during the shrinkage compensation stage of the finished product, it is divided into two parts. The first part is two stages of continuous current reduction, and the second part is a low current holding stage. First, in the initial current reduction stage of the continuous current reduction stage, the melting current reduction rate is maintained at 700A / min within 5 to 8 minutes, and the melting rate is gradually reduced. Then, the melting current reduction rate is maintained at 200A / min within 10 to 15 minutes to reduce the depth of the molten pool; the second part uses a low current of 6.0kA to maintain until the end of the shrinkage compensation stage to increase the shrinkage position. After the 9# niobium alloy ingot is cooled and taken out of the furnace, the riser is machined for flaw detection and sawing. The distance from the lower end of the shrinkage hole to the end face of the ingot head is 39mm.
[0070] Example 10
[0071] The method for feeding the riser of Φ220mm finished niobium alloy ingot mainly includes the following steps:
[0072] Step 1: The final finished product smelting of niobium alloy ingots is carried out by vacuum consumable smelting. To ensure the smelting vacuum environment, the leakage rate test should be carried out in the welding and smelting processes in the furnace to ensure that it does not exceed 0.8Pa / min. In this embodiment, the consumable electrode specification is Φ150mm, and the water-cooled copper crucible specification is Φ220×Lmm. In order to ensure that the material is clean and not polluted, the auxiliary electrode uses pure niobium or the same grade of material. The process parameters include: the current setting value is 11.0kA in the stable stage of finished product smelting, the allowable fluctuation range in the process is 10.0~13.0kA, the smelting voltage setting value is 35.0V, the allowable voltage fluctuation range in the process is 20.0~45.0V, the arc stabilization current is selected to be AC 6.0A, the commutation period is 10s, and at the same time, the inlet and outlet water temperatures of the cooling water are controlled in the range of 18.0~25.0℃ and 25.0~35.0℃, respectively, so as to obtain a full molten pool.
[0073] Step 2: When the remaining weight of the niobium alloy consumable electrode reaches 1 / 6 to 1 / 4 of the initial weight, the stable smelting stage is transferred to the finished product feeding stage, and the step-by-step current reduction and low current maintenance feeding process is implemented to feed the niobium alloy ingot riser. Figure 2 As shown in the figure, during the shrinkage compensation stage of the finished product, it is divided into two parts. The first part is two stages of continuous current reduction, and the second part is a low current holding stage. First, in the initial current reduction stage of the continuous current reduction stage, the melting current reduction rate is maintained at 600A / min within 5 to 8 minutes, and the melting rate is gradually reduced. Then, the melting current reduction rate is maintained at 170A / min within 10 to 15 minutes to reduce the depth of the molten pool; the second part uses a low current of 6.0kA to maintain until the end of the shrinkage compensation stage to increase the shrinkage position. After the 10# niobium alloy ingot is cooled and taken out of the furnace, the riser is machined for flaw detection and sawing. The distance from the lower end of the shrinkage hole to the end face of the ingot head is 42mm.
[0074] Embodiment 11
[0075] The method for feeding the riser of Φ220mm finished niobium alloy ingot mainly includes the following steps:
[0076] Step 1: The final finished product smelting of niobium alloy ingots is carried out by vacuum consumable smelting. To ensure the smelting vacuum environment, the leakage rate test should be carried out in the welding and smelting processes in the furnace to ensure that it does not exceed 0.8Pa / min. In this embodiment, the consumable electrode specification is Φ170mm, and the water-cooled copper crucible specification is Φ220×L mm. In order to ensure that the material is clean and not polluted, the auxiliary electrode uses pure niobium or the same grade of material. The process parameters include: the current setting value is 11.0kA in the stable stage of finished product smelting, the fluctuation range allowed during the process is 10.0~13.0kA, the smelting voltage setting value is 35.0V, the voltage fluctuation range allowed during the process is 20.0~45.0V, the arc stabilization current is selected to be AC 6.0A, the commutation period is 10s, and at the same time, the inlet and outlet water temperatures of the cooling water are controlled in the range of 18.0~25.0℃ and 25.0~35.0℃, respectively, so as to obtain a full molten pool.
[0077] Step 2: When the remaining weight of the niobium alloy consumable electrode reaches 1 / 6 to 1 / 4 of the initial weight, the stable smelting stage is transferred to the finished product feeding stage, and the step-by-step current reduction and low current maintenance feeding process is implemented to feed the niobium alloy ingot riser. Figure 2 As shown in the figure, during the shrinkage compensation stage of the finished product, it is divided into two parts. The first part is two stages of continuous current reduction, and the second part is a low current holding stage. First, in the initial current reduction stage of the continuous current reduction stage, the melting current reduction rate is maintained at 780A / min within 5 to 8 minutes, and the melting rate is gradually reduced. Then, the melting current reduction rate is maintained at 230A / min within 10 to 15 minutes to reduce the depth of the molten pool; the second part uses a low current of 6.0kA to maintain until the end of the shrinkage compensation stage to increase the shrinkage position. After the 11# niobium alloy ingot is cooled and taken out of the furnace, the riser is machined for flaw detection and sawing. The distance from the lower end of the shrinkage hole to the end face of the ingot head is 48mm.
[0078] Example 12
[0079] The method for feeding the riser of Φ220mm finished niobium alloy ingot mainly includes the following steps:
[0080] Step 1: The final finished product smelting of niobium alloy ingots is carried out by vacuum consumable smelting. To ensure the smelting vacuum environment, the leakage rate test should be carried out in the welding and smelting processes in the furnace to ensure that it does not exceed 0.8Pa / min. In this embodiment, the consumable electrode specification is Φ150mm, and the water-cooled copper crucible specification is Φ220×Lmm. In order to ensure that the material is clean and not polluted, the auxiliary electrode uses pure niobium or the same grade of material. The process parameters include: the current setting value is 11.0kA in the stable stage of finished product smelting, the allowable fluctuation range in the process is 10.0~13.0kA, the smelting voltage setting value is 35.0V, the allowable voltage fluctuation range in the process is 20.0~45.0V, the arc stabilization current is selected to be AC 6.0A, the commutation period is 10s, and at the same time, the inlet and outlet water temperatures of the cooling water are controlled in the range of 18.0~25.0℃ and 25.0~35.0℃, respectively, so as to obtain a full molten pool.
[0081] Step 2: When the remaining weight of the niobium alloy consumable electrode reaches 1 / 6 to 1 / 4 of the initial weight, the stable smelting stage is transferred to the finished product feeding stage, and the step-by-step current reduction and low current maintenance feeding process is implemented to feed the niobium alloy ingot riser. Figure 2 As shown in the figure, during the shrinkage compensation stage of the finished product, it is divided into two parts. The first part is two stages of continuous current reduction, and the second part is a low current holding stage. First, in the initial current reduction stage of the continuous current reduction stage, the melting current reduction rate is maintained at 600A / min within 5 to 8 minutes, and the melting rate is gradually reduced. Then, the melting current reduction rate is maintained at 170A / min within 10 to 15 minutes to reduce the depth of the molten pool; the second part uses a low current of 6.0kA to maintain until the end of the shrinkage compensation stage to increase the shrinkage position. After the 12# niobium alloy ingot is cooled and taken out of the furnace, the riser is machined for flaw detection and sawing. The distance from the lower end of the shrinkage hole to the end face of the ingot head is 47mm.
[0082] Table 2 below shows the repeatability and stability test of the shrinkage feeding process for 6 niobium alloy ingots of the same specification #7~#12Φ220mm. The shrinkage feeding test process parameters and riser depth of the Φ220mm niobium alloy ingot are shown in Table 2.
[0083] Table 2 Niobium alloy ingot feeding test process parameters and riser depth
[0084]
[0085] After setting and executing the shrinkage feeding process for 6 niobium alloy ingots of the same specification #7~#12Φ220mm, the depth of the ingot riser detected after machining was ≤50mm, the shrinkage feeding effect was stable, the yield rate of niobium alloy ingots was improved, the waste of raw materials was reduced, and the shrinkage feeding solidification process of Φ220mm ingot-type niobium alloy was obtained.
[0086] Example 13
[0087] The riser feeding method for Φ300mm finished niobium alloy ingot mainly includes the following steps:
[0088] Step 1: The final finished product smelting of niobium alloy ingots is carried out by vacuum consumable smelting. To ensure the smelting vacuum environment, the leakage rate test should be carried out in the welding and smelting processes in the furnace to ensure that it does not exceed 0.8Pa / min. In this embodiment, the consumable electrode specification is Φ210mm, and the water-cooled copper crucible specification is Φ300×Lmm. In order to ensure that the material is clean and not polluted, the auxiliary electrode uses pure niobium or the same grade of material. The process parameters include: the current setting value is 15.0kA in the stable stage of finished product smelting, the fluctuation range allowed during the process is 14.0~18.0kA, the smelting voltage setting value range is 38.0V, the voltage fluctuation range allowed during the process is 20.0~45.0V, the arc stabilization current is selected to be AC 8.0A, the commutation period is 15s, and at the same time, the inlet and outlet temperatures of the cooling water are controlled in the range of 18.0~25.0℃ and 25.0~35.0℃, respectively, so as to obtain a full molten pool.
[0089] Step 2: When the remaining weight of the niobium alloy consumable electrode reaches 1 / 6 to 1 / 4 of the initial weight, the stable smelting stage is transferred to the finished product feeding stage, and the step-by-step current reduction and low current maintenance feeding process is implemented to feed the niobium alloy ingot riser. Figure 3 As shown in the figure, during the shrinkage compensation stage of the finished product, it is divided into two parts. The first part is two stages of continuous current reduction, and the second part is a low current holding stage. First, in the initial current reduction stage of the continuous current reduction stage, the melting current reduction rate is maintained at 800A / min within 5 to 8 minutes, and the melting rate is gradually reduced. Then, the melting current reduction rate is maintained at 280A / min within 10 to 15 minutes to reduce the depth of the molten pool; the second part uses a low current of 8.0kA to maintain until the end of the shrinkage compensation stage to increase the shrinkage position. After the 13# niobium alloy ingot is cooled and taken out of the furnace, the riser is machined for flaw detection and sawing. The distance from the lower end of the shrinkage hole to the end face of the ingot head is 46mm.
[0090] Embodiment 14
[0091] The riser feeding method for Φ300mm finished niobium alloy ingot mainly includes the following steps:
[0092] Step 1: The final finished product smelting of niobium alloy ingots is carried out by vacuum consumable smelting. To ensure the smelting vacuum environment, the leakage rate test should be carried out in the welding and smelting processes in the furnace to ensure that it does not exceed 0.8Pa / min. In this embodiment, the consumable electrode specification is Φ210mm, and the water-cooled copper crucible specification is Φ300×Lmm. In order to ensure that the material is clean and not polluted, the auxiliary electrode uses pure niobium or the same grade of material. The process parameters include: the current setting value is 15.0kA in the stable stage of finished product smelting, the fluctuation range allowed during the process is 14.0~18.0kA, the smelting voltage setting value range is 38.0V, the voltage fluctuation range allowed during the process is 20.0~45.0V, the arc stabilization current is selected to be AC 8.0A, the commutation period is 15s, and at the same time, the inlet and outlet temperatures of the cooling water are controlled in the range of 18.0~25.0℃ and 25.0~35.0℃, respectively, so as to obtain a full molten pool.
[0093] Step 2: When the remaining weight of the niobium alloy consumable electrode reaches 1 / 6 to 1 / 4 of the initial weight, the stable smelting stage is transferred to the finished product feeding stage, and the step-by-step current reduction and low current maintenance feeding process is implemented to feed the niobium alloy ingot riser. Figure 3 As shown in the figure, during the shrinkage compensation stage of the finished product, it is divided into two parts. The first part is two stages of continuous current reduction, and the second part is a low current holding stage. First, in the initial current reduction stage of the continuous current reduction stage, the melting current reduction rate is maintained at 800A / min within 5 to 8 minutes, and the melting rate is gradually reduced. Then, the melting current reduction rate is maintained at 280A / min within 10 to 15 minutes to reduce the depth of the molten pool; the second part uses a low current of 8.0kA to maintain until the end of the shrinkage compensation stage to increase the shrinkage position. After the 14# niobium alloy ingot is cooled and taken out of the furnace, the riser is machined for flaw detection and sawing. The distance from the lower end of the shrinkage hole to the end face of the ingot head is 45mm.
[0094] Embodiment 15
[0095] The riser feeding method for Φ300mm finished niobium alloy ingot mainly includes the following steps:
[0096] Step 1: The final finished product smelting of niobium alloy ingots is carried out by vacuum consumable smelting. To ensure the smelting vacuum environment, the leakage rate test should be carried out in the welding and smelting processes in the furnace to ensure that it does not exceed 0.8Pa / min. In this embodiment, the consumable electrode specification is Φ220mm, and the water-cooled copper crucible specification is Φ300×Lmm. In order to ensure that the material is clean and not polluted, the auxiliary electrode uses pure niobium or the same grade of material. The process parameters include: the current setting value is 15.0kA in the stable stage of finished product smelting, the fluctuation range allowed in the process is 14.0~18.0kA, the smelting voltage setting value range is 38.0V, the voltage fluctuation range allowed in the process is 20.0~45.0V, the arc stabilization current is selected as AC 8.0A, the commutation period is 15s, and at the same time, the inlet and outlet water temperatures of the cooling water are controlled in the range of 18.0~25.0℃ and 25.0~35.0℃, respectively, so as to obtain a full molten pool.
[0097] Step 2: When the remaining weight of the niobium alloy consumable electrode reaches 1 / 6 to 1 / 4 of the initial weight, the stable smelting stage is transferred to the finished product feeding stage, and the step-by-step current reduction and low current maintenance feeding process is implemented to feed the niobium alloy ingot riser. Figure 3 As shown in the figure, during the shrinkage compensation stage of the finished product, it is divided into two parts. The first part is two stages of continuous current reduction, and the second part is a low current holding stage. First, in the initial current reduction stage of the continuous current reduction stage, the melting current reduction rate is maintained at 900A / min within 5 to 8 minutes, and the melting rate is gradually reduced. Then, the melting current reduction rate is maintained at 300A / min within 10 to 15 minutes to reduce the depth of the molten pool; the second part uses a low current of 8.0kA to maintain until the end of the shrinkage compensation stage to increase the shrinkage position. After the 15# niobium alloy ingot is cooled and taken out of the furnace, the riser is machined for flaw detection and sawing. The distance from the lower end of the shrinkage hole to the end face of the ingot head is 47mm.
[0098] Example 16
[0099] The riser feeding method for Φ300mm finished niobium alloy ingot mainly includes the following steps:
[0100] Step 1: The final finished product smelting of niobium alloy ingots is carried out by vacuum consumable smelting. To ensure the smelting vacuum environment, the leakage rate test should be carried out in the welding and smelting processes in the furnace to ensure that it does not exceed 0.8Pa / min. In this embodiment, the consumable electrode specification is Φ210mm, and the water-cooled copper crucible specification is Φ300×Lmm. In order to ensure that the material is clean and not polluted, the auxiliary electrode uses pure niobium or the same grade of material. The process parameters include: the current setting value is 15.0kA in the stable stage of finished product smelting, the fluctuation range allowed during the process is 14.0~18.0kA, the smelting voltage setting value range is 38.0V, the voltage fluctuation range allowed during the process is 20.0~45.0V, the arc stabilization current is selected to be AC 8.0A, the commutation period is 15s, and at the same time, the inlet and outlet temperatures of the cooling water are controlled in the range of 18.0~25.0℃ and 25.0~35.0℃, respectively, so as to obtain a full molten pool.
[0101] Step 2: When the remaining weight of the niobium alloy consumable electrode reaches 1 / 6 to 1 / 4 of the initial weight, the stable smelting stage is transferred to the finished product feeding stage, and the step-by-step current reduction and low current maintenance feeding process is implemented to feed the niobium alloy ingot riser. Figure 3 As shown in the figure, during the shrinkage compensation stage of the finished product, it is divided into two parts. The first part is two stages of continuous current reduction, and the second part is a low current holding stage. First, in the initial current reduction stage of the continuous current reduction stage, the melting current reduction rate is maintained at 800A / min within 5 to 8 minutes, and the melting rate is gradually reduced. Then, the melting current reduction rate is maintained at 280A / min within 10 to 15 minutes to reduce the depth of the molten pool; the second part uses a low current of 8.0kA to maintain until the end of the shrinkage compensation stage to increase the shrinkage position. After the 14# niobium alloy ingot is cooled and taken out of the furnace, the riser is machined for flaw detection and sawing. The distance from the lower end of the shrinkage hole to the end face of the ingot head is 44mm.
[0102] Embodiment 17
[0103] The riser feeding method for Φ300mm finished niobium alloy ingot mainly includes the following steps:
[0104] Step 1: The final finished product of niobium alloy ingot is melted by vacuum consumable melting. To ensure the vacuum environment of melting, the leakage rate test should be carried out in the furnace welding and melting process to ensure that it does not exceed 0.8Pa / min. In this embodiment, the specification of the consumable electrode is Φ230mm, and the specification of the water-cooled copper crucible is Φ300×L mm. In order to ensure that the material is clean and not polluted, the auxiliary electrode uses pure niobium or the same grade of material. The process parameters include: the current setting value is 15.0kA in the stable stage of finished product melting, the fluctuation range allowed in the process is 14.0~18.0kA, the melting voltage setting value range is 38.0V, the voltage fluctuation range allowed in the process is 20.0~45.0V, the arc stabilization current is selected as AC 8.0A, the commutation period is 15s, and at the same time, the inlet and outlet temperatures of the cooling water are controlled in the range of 18.0~25.0℃ and 25.0~35.0℃, respectively, so as to obtain a full molten pool.
[0105] Step 2: When the remaining weight of the niobium alloy consumable electrode reaches 1 / 6 to 1 / 4 of the initial weight, the stable smelting stage is transferred to the finished product feeding stage, and the step-by-step current reduction and low current maintenance feeding process is implemented to feed the niobium alloy ingot riser. Figure 3 As shown in the figure, during the shrinkage compensation stage of the finished product, it is divided into two parts. The first part is two stages of continuous current reduction, and the second part is a low current holding stage. First, in the initial current reduction stage of the continuous current reduction stage, the melting current reduction rate is maintained at 1000A / min within 5 to 8 minutes, and the melting rate is gradually reduced. Then, the melting current reduction rate is maintained at 350A / min within 10 to 15 minutes to reduce the depth of the molten pool; the second part uses a low current of 8.0kA to maintain until the end of the shrinkage compensation stage to increase the shrinkage position. After the 13# niobium alloy ingot is cooled and taken out of the furnace, the riser is machined for flaw detection and sawing, and the distance from the lower end of the shrinkage hole to the end face of the ingot head is 50mm.
[0106] Embodiment 18
[0107] The riser feeding method for Φ300mm finished niobium alloy ingot mainly includes the following steps:
[0108] Step 1: The final finished product smelting of niobium alloy ingots is carried out by vacuum consumable smelting. To ensure the smelting vacuum environment, the leakage rate test should be carried out in the welding and smelting processes in the furnace to ensure that it does not exceed 0.8Pa / min. In this embodiment, the consumable electrode specification is Φ210mm, and the water-cooled copper crucible specification is Φ300×Lmm. In order to ensure that the material is clean and not polluted, the auxiliary electrode uses pure niobium or the same grade of material. The process parameters include: the current setting value is 15.0kA in the stable stage of finished product smelting, the fluctuation range allowed during the process is 14.0~18.0kA, the smelting voltage setting value range is 38.0V, the voltage fluctuation range allowed during the process is 20.0~45.0V, the arc stabilization current is selected to be AC 8.0A, the commutation period is 15s, and at the same time, the inlet and outlet temperatures of the cooling water are controlled in the range of 18.0~25.0℃ and 25.0~35.0℃, respectively, so as to obtain a full molten pool.
[0109] Step 2: When the remaining weight of the niobium alloy consumable electrode reaches 1 / 6 to 1 / 4 of the initial weight, the stable smelting stage is transferred to the finished product feeding stage, and the step-by-step current reduction and low current maintenance feeding process is implemented to feed the niobium alloy ingot riser. Figure 3 As shown in the figure, during the shrinkage compensation stage of the finished product, it is divided into two parts. The first part is two stages of continuous current reduction, and the second part is a low current holding stage. First, in the initial current reduction stage of the continuous current reduction stage, the melting current reduction rate is maintained at 800A / min within 5 to 8 minutes, and the melting rate is gradually reduced. Then, the melting current reduction rate is maintained at 280A / min within 10 to 15 minutes to reduce the depth of the molten pool; the second part uses a low current of 8.0kA to maintain until the end of the shrinkage compensation stage to increase the shrinkage position. After the 13# niobium alloy ingot is cooled and taken out of the furnace, the riser is machined for flaw detection and sawing. The distance from the lower end of the shrinkage hole to the end face of the ingot head is 49mm.
[0110] Table 3 below shows the repeatability and stability test of the feeding process for 6 niobium alloy ingots of the same specification of #13~#18Φ300mm. The feeding test process parameters and riser depth of the Φ300mm niobium alloy ingot are shown in Table 3.
[0111] Table 3 Process parameters and riser depth of niobium alloy ingot feeding test
[0112]
[0113] After setting and executing the shrinkage feeding process for 6 niobium alloy ingots of the same specification #13~#18Φ220mm, the depth of the ingot riser detected after machining was ≤50mm, the shrinkage feeding effect was stable, the yield rate of niobium alloy ingots was improved, the waste of raw materials was reduced, and the shrinkage feeding solidification process of Φ300mm ingot niobium alloy was obtained.
[0114] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A method for feeding shrinkage of a riser of a niobium alloy ingot, characterized in that: The steps include: Using niobium alloy as a consumable electrode, a vacuum consumable melting method is used to melt the niobium alloy ingot finished product to obtain the niobium alloy ingot; After the niobium alloy enters the shrinkage feeding stage from the smelting stability stage in the finished product smelting, the riser shrinkage is fed by two stages of uniform speed continuous current reduction and low current maintenance.
2. A niobium alloy ingot riser feeding method as claimed in claim 1, characterized in that: The reduction rate of each section of the two sections of uniform-speed continuous current reduction is 500-1000A / min and 100-350A / min respectively.
3. A method for feeding shrinkage of a niobium alloy ingot riser according to claim 1, characterized in that: The low current is maintained until the end of the feeding stage, wherein the low current is 4.0-10.0 kA.
4. A method for feeding shrinkage of a niobium alloy ingot riser according to claim 1, characterized in that: The size of the niobium alloy consumable electrode for finished product smelting is Φ80-Φ240mm. When the weight of the niobium alloy consumable electrode for finished product smelting is 1 / 6-1 / 4 times the weight of the entire niobium alloy consumable electrode for finished product smelting, the finished product smelting enters the shrinkage feeding stage from the smelting stabilization stage.
5. A method for feeding shrinkage of a niobium alloy ingot riser as claimed in claim 1, characterized in that: The size of the water-cooled copper crucible used for smelting the finished product is Φ160-Φ300 mm.
6. A method for feeding shrinkage of a niobium alloy ingot riser as claimed in claim 1, characterized in that: The smelting current in the stable smelting stage is 7.0-18.0 kA, the smelting voltage setting value in the stable smelting stage is 20.0-45.0 V, the arc stabilizing current is AC 5-10 A, and the commutation period is 10-15 s.
7. A method for feeding shrinkage of a niobium alloy ingot riser as claimed in claim 6, characterized in that: The allowable fluctuation range of the smelting current in the stable smelting stage is ±2kA of the smelting current setting value in the stable smelting stage, and the allowable fluctuation range of the smelting voltage in the stable smelting stage is ±5V of the smelting voltage setting value in the stable smelting stage.
8. A method for feeding shrinkage of a niobium alloy ingot riser as claimed in claim 1, characterized in that: The cooling water inlet temperature is controlled at 18.0-25.0°C; the cooling water outlet temperature is controlled at 25.0-35.0°C to obtain a full molten pool.
9. A method for feeding shrinkage of a niobium alloy ingot riser according to claim 1, characterized in that: The vacuum consumable smelting method is used for the final smelting of niobium alloy ingots. In order to ensure the smelting vacuum environment, a gas leakage rate test should be carried out to ensure that it is less than 0.8Pa / min.
Citation Information
Cited By
Method for eliminating short circuit in smelting feeding stage of titanium alloy cast ingot
CN119456964A
A method for eliminating short circuits during the feeding stage of titanium alloy ingot melting.
CN119456964B