High-temperature-resistant and high-humidity-resistant nano-copper and preparation method thereof

Through laser direct writing modification/reduction sintering technology, a stable hydrophobic anti-oxidation layer is formed, which solves the problem of oxidation failure of nano-copper in high temperature and high humidity environment, achieves efficient and economical anti-oxidation effect, simplifies the process flow and improves the Stability and conductivity of nanocopper.

CN118720129AActive Publication Date: 2024-10-01ZHEJIANG UNIV

Patent Information

Application Number
CN202410615773.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-17
Publication Date
2024-10-01
Estimated Expiration
2044-05-17

AI Technical Summary

Technical Problem

In the existing technology, nano-copper is prone to oxidation and failure in high-temperature and high-humidity environments. Existing anti-oxidation surface treatment methods are costly, cumbersome or require harsh conditions, making it difficult to achieve simple, effective and economical durability improvements.

Method used

Laser direct writing modification/reduction sintering method is used to modify nano-copper with formate-copper ion complex and alkyl hydrophobic layer to form a stable hydrophobic anti-oxidation layer and improve the thermal stability and corrosion resistance of nano-copper.

Benefits of technology

It achieves the long-term stability and conductivity of nano-copper in high-temperature and high-humidity environments, simplifies the process, reduces costs, is suitable for a variety of coating processes, and significantly improves the oxidation resistance of nano-copper.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720129A_ABST
    Figure CN118720129A_ABST
Patent Text Reader

Abstract

The invention discloses high-temperature-resistant and high-humidity-resistant nano-copper and a preparation method thereof. The high-temperature-resistant and high-humidity-resistant nano-copper is nano-copper of which the surface is modified with a formate-copper ion complex and an alkyl hydrophobic layer. According to the preparation method, on the basis of the oxidation inhibition effect of formic acid, photo-thermal reduction of nano copper oxide is synchronously induced through laser direct writing, a coordination passivation layer is formed on the surface of nano copper generated through sintering, and meanwhile, long-chain organic amine is introduced to obviously improve the hydrophobic performance of the nano copper; therefore, a more stable hydrophobic anti-oxidation layer is formed on the surface of the nano-copper. In addition, the high-temperature-resistant and high-humidity-resistant nano-copper prepared by the method has excellent conductivity, and can form good adhesion with a flexible / rigid substrate. Compared with the prior art, the process is simple, effective anti-oxidation / hydrophobization surface treatment is carried out based on laser patterning direct writing, and one-step integration of multiple properties of the high-temperature-resistant and high-humidity-resistant nano-copper is achieved while the machining efficiency is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to surface treatment of nano copper, in particular to high temperature and high humidity resistant nano copper and a preparation method thereof. Background Art

[0002] Nano copper, a copper material with unique physical and chemical properties at the nanoscale, has attracted widespread attention in recent years for its excellent performance in catalysis (high-efficiency catalysts and carriers), electronics and electrical (micro-electromechanical devices, conductive inks, printed circuit boards, etc.), antibacterial (medical care, food packaging, water treatment, etc.), energy (solar energy / lithium-ion batteries, thermal interface materials), and environmental remediation (heavy metal pollution purification). Compared with macroscopic copper materials, nano copper shows a higher specific surface area, stronger surface activity, and excellent electromechanical properties.

[0003] However, nano copper is very easy to fail in a long-term high temperature environment. Compared with bulk copper, its thermal stability is significantly degraded due to its small particle size and large specific surface area. In addition, in a high humidity environment, nano copper is also prone to corrosion, which in turn affects its conductivity and appearance. Moreover, further increase in humidity will promote the accelerated oxidation of the nano copper surface, ultimately leading to the formation of copper oxide.

[0004] In order to improve the oxidation resistance and durability of nano copper in high temperature and high humidity environments, a variety of anti-oxidation and anti-corrosion surface treatment methods have been developed:

[0005] (1) Surface coating: By coating the surface of nano-copper with a layer of stable substances (such as metals such as gold / silver / nickel, or non-metals such as silicon dioxide / carbon layer / polymer), oxygen and moisture can be effectively blocked from direct contact with nano-copper, thereby preventing its oxidation and aggregation.

[0006] (2) Surface passivation: Stable coordination functional groups are introduced onto the surface of nano-copper by chemical or physical methods to form a dense compound film and increase its surface energy, thereby improving stability under high temperature and high humidity.

[0007] (3) Surface modification: Form a self-assembled film on the surface of nano-copper by chemical bonding or other means (such as using thiol compounds) to effectively improve the surface properties of nano-copper, form a stable protective layer, and enhance its high temperature and high humidity antioxidant properties.

[0008] (4) Surface modification and composite materials: Nano-copper is composited and intercalated with other materials (such as ceramics, organic polymers, etc.) to prevent direct exposure to high heat and humidity environments under the effect of physical isolation. At the same time, the overall performance of nano-copper is enhanced by leveraging the characteristics of the composite material.

[0009] Among the above treatment methods, method (1) has a better antioxidant effect, but the cost is high and the process flow is relatively complicated. Although the nano copper obtained by methods (2) to (4) has a certain antioxidant effect, it will still undergo irreversible oxidation failure when exposed to high temperature and high humidity for a long time.

[0010] In the prior art, the corresponding method (1) is taken as an example of "a method for preparing nano-carbon coated copper powder" with patent number CN201910232685.5, and the steps include: preparing a polyacrylonitrile solution: adding polyacrylonitrile powder to a solvent, and stirring it at 60°C to 80°C to obtain a polyacrylonitrile solution; coating a carbon-rich material: taking copper powder with a particle size of 0.1μm to 10μm, first pickling the copper powder with dilute sulfuric acid with a mass concentration of 2% to 8%, and then repeatedly washing the pickled copper powder with distilled water until The process is as follows: the copper powder after acid washing and water washing is placed in a vacuum drying oven, kept at 40°C to 80°C for 2 to 3 hours, and dried to obtain clean copper powder; the clean copper powder is weighed and added to the polyacrylonitrile solution, and electromagnetic stirring is performed to obtain a mixture; the carbon-rich material is pre-oxidized: the mixture is placed in a stainless steel reactor for pre-oxidation treatment; the carbon-rich material is pyrolyzed at high temperature to prepare nano-carbon-coated copper powder: the stainless steel reactor is evacuated to a vacuum degree of 1×10 -1 mpa~1×10 -3 mpa, and then fill the stainless steel reactor with inert gas for carbonization treatment, so that the carbon atoms in polyacrylonitrile are cracked into a two-dimensional carbon network structure at high temperature and evenly coated on the surface of the copper powder, and finally cooled to room temperature to obtain nano-carbon coated copper powder. Although the method of the present invention is simple and easy to implement, and the obtained antioxidant copper powder has good conductivity, the process is cumbersome and needs to be carried out in an inert gas, and the reaction conditions are relatively harsh.

[0011] In the prior art, corresponding to method (1), taking "Anti-oxidation super-hydrophobic copper film and preparation method thereof" with patent number CN202111250495.X as an example, the anti-oxidation super-hydrophobic copper film is a copper-carbon film formed by a graphitized carbon layer wrapped around a copper nanocluster, and a copper@carbon core-shell structure is evenly deposited on a substrate. The surface morphology of the copper-carbon film is in the shape of nano-peaks. The anti-oxidation super-hydrophobic copper film is prepared by chemical vapor deposition, and comprises the following steps: substrate cleaning, placing the cut substrate into an ultrasonic cleaning machine for ultrasonic cleaning; substrate etching, placing the substrate into an etching solution, and etching the substrate surface; precursor preparation, respectively weighing an organic metal precursor and a liquid organic precursor for standby use, wherein the organic metal precursor is Cu(I) or Cu(II) organic metal copper; and the liquid organic precursor is a hydrocarbon with a decomposition temperature lower than that of the organic metal precursor; charging, placing the etched substrate into a reaction zone of a tubular furnace, respectively loading the precursors into a raw material tank, closing the valve of the raw material tank and connecting the raw material tank to the tubular furnace; introducing hydrogen, introducing hydrogen into the tubular furnace to replace the air in the tubular furnace, and making the pressure in the tubular furnace Reach 1000~9000Pa;Argon is passed into, argon is passed into raw material tank, argon is completely filled with raw material tank, air is isolated, and the pressure in raw material tank is made to be the same as the pressure in tube furnace;Reaction zone heating, tube furnace is heated, the reaction zone in tube furnace is in reaction temperature, and the reaction temperature is 400~600 ℃;Raw material tank heating, raw material tank is heated, organometallic precursor and liquid organic precursor are all gasified;Deposition is carried out, raw material tank valve is opened, precursor is passed into reaction zone by argon gas and deposited, and the product after deposition will be deposited on the surface of substrate;Insulation, after deposition is completed, argon gas and raw material tank valve are quickly closed, the hydrogen concentration in tube furnace reaction zone is controlled, the temperature of tube furnace reaction zone is dropped to room temperature, and the anti-oxidation super-hydrophobic copper film is obtained. Although the method is easy to control, and has good repeatability, reaction requires high pressure environment and inert gas protection, thus inevitably greatly increases cost.

[0012] In the prior art, the corresponding method (1) is described in the patent number CN201710343566.8, "A novel anti-oxidation nano-copper solder paste and its preparation method and application". The metal film (gold or silver) is uniformly coated on the surface of nano-copper powder by magnetron sputtering process, and then the traditional nano-copper solder paste formula is used, and an appropriate amount of molding aid is added to finally prepare a novel anti-oxidation and anti-cracking anti-oxidation nano-copper solder paste. This invention avoids the oxidation of nano-copper by wrapping an inert metal gold / silver layer, and can serve for a long time without trouble in a high temperature and high humidity environment. However, it significantly increases the material cost and limits large-scale application.

[0013] In the prior art, corresponding to method (2), taking "a surface treatment method for copper-containing materials" with patent number CN201710751393.3 as an example, a surface treatment method for copper-containing materials is provided, which is simple in method, modifies or adsorbs formate on the surface of the copper material, enhances the antioxidant capacity of the copper material, and makes it have good conductivity. The copper-containing material is mixed with a polar solvent, and after adding a stabilizer and an auxiliary agent, it is sealed and pressurized for reaction, and then liquid-solid separation, washing, and drying are performed to complete the antioxidant surface treatment of the copper material. Among them, formate is used to treat the copper surface, and the formate redox potential is lower than that of copper. The formate oxidation kinetics is slow, which can effectively prevent the chemical or electrochemical corrosion of copper. It is applicable to all zero-valent or partially oxidized copper-containing materials. The copper-containing material treated by the invention has stronger antioxidant capacity, salt and alkali corrosion resistance and higher conductivity than before treatment, and can be used for copper-based conductive slurry, etc. However, the operation process is relatively cumbersome, the reaction time is long, and the closed reaction conditions of pressurization and heating are required, which is not suitable for efficient treatment under room temperature environment. In addition, it is difficult to prevent the copper-based conductive paste prepared by this method from being oxidized during long-term storage.

[0014] In the prior art, corresponding to method (2), taking "a method for preparing an antioxidant copper-based conductive ink" with patent number CN201710752246.8 as an example, the surface treatment of copper material: 250-3000 mesh copper powder is mixed with a polar solvent (at least one of an amide solvent, an alcohol solvent, an ester solvent, an ether solvent, and water), a formate stabilizer is added and mixed, and then a sealed reaction is carried out in a pressure-resistant container at 120-180°C for 0.01-100h, and then liquid-solid separation, washing, and drying are performed; the antioxidant copper-based conductive ink is prepared: the treated copper powder and other media of the conductive paste are compounded according to the mass percentage of 10%-74.5% of antioxidant copper powder, 0-20% of conductive particles, 20%-50% of organic solvent, 5%-30% of binder, and 0.5%-20% of additive, and the conductive paste is obtained by stirring evenly; the antioxidant copper-based conductive ink is printed and cured. The antioxidant copper-based conductive ink prepared by this invention has good stability, excellent conductivity and dispersibility, but it also has disadvantages such as relatively harsh reaction conditions and poor long-term storage of the antioxidant copper-based conductive ink.

[0015] In the prior art, corresponding to method (3), taking "Anti-oxidation copper film / copper wire and its preparation method and application" with patent number CN202110912124.7 as an example, anti-oxidation copper powder, alcohol solvent, amine solvent, resin, and additive are ground and mixed, and degassed to obtain an anti-oxidation copper slurry; the anti-oxidation copper slurry is coated on a substrate, dried and pre-cured under an inert atmosphere to obtain a copper film precursor 1 / copper wire precursor 1; the copper film precursor 1 / copper wire precursor 1 is cured under an inert atmosphere to obtain a copper film precursor 2 / copper wire precursor 2; the copper film precursor 2 / copper wire precursor 2 is placed in a compound containing a thiol group or a disulfide bond to obtain an anti-oxidation copper film / copper wire. Although the copper film / copper wire obtained by the invention has excellent oxidation resistance, an inert atmosphere is required to obtain high conductivity, and the preparation conditions are relatively harsh.

[0016] In the prior art, corresponding to method (2) and method (3), taking "Anti-oxidation copper material and its preparation method" with patent number CN202010578213.8 as an example, the anti-oxidation copper material is a copper material whose surface is modified with formate and thiol, and the thiol is adsorbed on the surface of the copper material modified by the formate. The preparation method of the above-mentioned anti-oxidation copper material comprises the following steps: adding a formate solution with a concentration of 1 to 15 mol / L and a solvent to a first container and stirring evenly to obtain a mixed solution, then placing the copper material in the first container containing the above-mentioned mixed solution, reacting at a temperature of 80 to 180°C for 0.5 to 24 hours, pouring off the supernatant, and adding a 1.0×10 -4 ~1.0×10 -1 mol / L of mercaptan for 0.5 to 30 minutes, and then undergo liquid-solid separation, washing and drying to obtain the antioxidant copper material. In the present invention, the modification process of the copper material only requires an ordinary open container environment and a short time to significantly improve the antioxidant capacity of the copper material, and has the advantages of simple preparation and low cost. However, the acquisition of the pre-raw materials involves conditions such as closed high-pressure heating, which limits the high-efficiency preparation to a certain extent.

[0017] In the prior art, corresponding to method (4), taking "Anti-oxidation Copper Nanowire Transparent Electrode and Preparation Method and Application thereof" with patent number CN202210906888.X as an example, the copper nanowire stock solution prepared by the liquid phase method is taken, washed with a non-polar organic solvent and centrifuged, and the obtained copper nanowires are dissolved in anhydrous ethanol to obtain a copper nanowire dispersion; the copper nanowire dispersion is diluted with deionized water and ultrasonically treated; an organic acid solution is added to the obtained solution, and ultrasonically treated at the same time to remove the coating agent on the surface of the copper nanowires; the obtained solution is filtered and purified by a filter membrane, and then the copper nanowires are redissolved in anhydrous ethanol, and the aforementioned dilution, filtration and purification are repeated. The membrane filtration purification and re-dissolution process obtains the copper nanowire spray liquid for standby use; the spray liquid is subjected to high pressure spraying on a flexible substrate to form a film, and a heating platform is used to heat and evaporate the solvent at the bottom of the flexible substrate to obtain a copper nanowire film; the copper nanowire film is added to the organic acid solution for immersion treatment, then rinsed with anhydrous ethanol, and then vacuum dried to preliminarily obtain a copper nanowire transparent electrode; the obtained copper nanowire transparent electrode is subjected to argon plasma treatment, and then vacuum stored to obtain a copper nanowire transparent electrode with stronger conductivity; an aluminum oxide protective layer is deposited on the surface of the obtained copper nanowire transparent electrode by atomic layer deposition technology to obtain an anti-oxidation copper nanowire transparent electrode. In the present invention, the aluminum oxide deposited by atomic layer deposition is dense, has good isolation effect, and has strong anti-oxidation performance, and the thickness of the introduced aluminum oxide shell is uniform at the nanometer level, which has almost no effect on the light transmittance and square resistance of the transparent electrode. Argon plasma treatment can play a welding role on the copper nanowire conductive network, greatly reducing the contact resistance and improving the conductivity. However, this method not only involves expensive physical vapor deposition (atomic layer deposition), but also involves abnormal conditions such as argon atmosphere and high-pressure spraying, which is not conducive to large-scale processing.

[0018] In the prior art, the corresponding method (4) is to take the "A method for preparing an anti-oxidation micro-nano copper material" with patent number CN201910399914.2 as an example, using a micro-nano copper preparation device to prepare micro-nano copper powder; placing an organic coating agent in the vacuum chamber of the in-situ coating device, and sublimating or vaporizing the organic coating agent in the vacuum chamber by heating; introducing an inert gas into the preparation system, and the micro-nano copper powder is introduced into the vacuum chamber of the in-situ coating device along with the inert gas, and the sublimated or vaporized organic coating agent contacts and coats the surface of the micro-nano copper particles. Although the vacuum heating and inert atmosphere in the invention form a good organic coating on the surface of the micro-nano copper ions, greatly improving the anti-oxidation and dispersibility of the micro-nano copper particles and reducing their surface activity, the specific processing environment of the whole process will inevitably cause cost-effectiveness problems, which does not meet the actual application requirements.

[0019] Therefore, developing an antioxidant surface treatment method for high temperature and high humidity resistant nano-copper with simple preparation, efficient processing, strong compatibility and high cost-effectiveness is the current technical challenge to solve the application of nano-copper in functional fields such as catalysis, electronic and electrical, antibacterial, energy, and environmental remediation. Summary of the invention

[0020] The purpose of the present invention is to provide a high temperature and high humidity resistant nano copper and a preparation method thereof in view of the deficiencies in the prior art. The nano copper is prepared by laser direct writing modification / reduction sintering, and the method is simple, efficient and has excellent effect.

[0021] The technical solution adopted by the present invention is as follows:

[0022] A high temperature and high humidity resistant nano copper, which is a nano copper with a formate-copper ion complex and an alkyl hydrophobic layer modified on the surface;

[0023] The preparation method mainly comprises the following steps:

[0024] An alcohol solvent, an organic dispersant, an organic auxiliary agent 1, an organic auxiliary agent 2, a long-chain organic amine and an appropriate amount of formic acid are mixed and heated and stirred to obtain a functional precursor solution; an appropriate amount of nano-copper oxide is added to the functional precursor solution, and fully ultrasonically dispersed to obtain a functional nano-copper oxide ink; the functional nano-copper oxide ink is coated on a pretreated substrate, heated and dried to obtain a functional nano-copper oxide film; the functional nano-copper oxide film is subjected to laser direct writing modification / reduction sintering to obtain high temperature and high humidity resistance nano-copper.

[0025] The alcohol solvent is selected from one or more of monohydric alcohol, dihydric alcohol and polyhydric alcohol; the organic dispersant is selected from one or more of polyacrylamide organic polymer, polyethylene oxide organic polymer, hexadecyltrimethylammonium bromide, tannin and lignin, but not limited thereto; the organic auxiliary agent 1 is an organic amide, which is selected from one or more of formamide, acetamide, propionamide, butanamide, valeramide, acetylmethylamine, acetylethylamine, propionylethylamine, isopropylamide, lactamide, butyrylmethylamine, isobutylamide, methylacetamide, acetylvinylamine, N,N-dimethylformamide, N,N-dimethylacetamide and N-ethylacetamide, but not limited thereto; the organic auxiliary agent 2 is an organic alcoholamine, which is selected from one or more of ethanolamine, diethanolamine, triethanolamine, methylethanolamine, dimethylethanolamine, isopropanolamine, ethylpropanolamine, isobutanolamine, hexanolamine, cyclohexanolamine, N-methylethanolamine, N,N-dimethylethanolamine. The long-chain organic amine is selected from one or more of dodecylamine, tetradecylamine, hexadecylamine, octadecylamine, eicosylamine, docosylamine, dodecylbenzylamine, hexadecylbenzylamine, eicosylbenzylamine, dodecyldimethylamine, dodecyltrimethylamine, tetradecyldimethylamine, hexadecyldimethylamine, octadecylmethylamine, octadecyldimethylamine, octadecylethylamine, octadecyldiethylamine, octadecylaniline, eicosyldimethylamine, docosyltrimethylamine, N-methyloctadecylamine, N,N-dimethyldodecylamine, N,N-dimethylhexadecylamine, N,N-dimethyloctadecylamine, N-ethyldodecylamine, N-butyldodecylamine, diethylenetriamine, and oleylamine, but is not limited thereto; the heating and stirring temperature is 50-70°C, the rotation speed is 600-1500rpm, and the time is 2-20h.

[0026] The nano copper oxide is selected from one or more of copper oxide nanoparticles, copper oxide nanowires, copper oxide nanosheets, copper oxide nanorods, and copper oxide nanoshuttles, but is not limited thereto; the real-time temperature of the ultrasonic dispersion is 50-60° C., the ultrasonic pulse width is 0.1 s, and the ultrasonic time is 0.1-2 h; the functional nano copper oxide ink comprises 34.8-45.1 wt% of nano copper oxide, 38.6-43.5 wt% of alcohol solvents, 5.9-8.5 wt% of organic dispersants, 0.0-2.5 wt% of organic additives 1, 0.0-5.2 wt% of organic additives 2, 4.5-5.0 wt% of long-chain organic amines, and 3.4-4.0 wt% of formic acid.

[0027] The coating method is selected from one or more of spin coating, spray coating, scraping coating, brush coating, drip coating, and screen printing, but not limited thereto; the pretreatment is oxygen plasma surface treatment, and the treatment time is 60s to 150s; the substrate includes a flexible substrate and a rigid substrate, the flexible substrate is selected from one or more of polyimide (PI), polyethylene terephthalate (PET), polyvinyl alcohol (PVA), and polyethylene naphthalate (PEN), but not limited thereto; the rigid substrate is selected from one or more of polyetheretherketone (PEEK), polyphenylene sulfide (PPS), polysulfone (PSF), liquid crystal polymer (LCP), glass, silicon wafer, and ceramic, but not limited thereto;

[0028] The heating and drying temperature is 50-80°C and the time is 2-12 hours.

[0029] The laser is a continuous green light with a wavelength of 532nm; the power of the laser direct writing modification / reduction sintering is 100-300mW, the speed is 20-200mm / s, and the scanning period is 20-40μm; the laser direct writing modification / reduction sintering is based on the oxidation inhibition effect of formic acid, and synchronously induces the photothermal reduction of nano copper oxide through laser direct writing, and forms a coordination passivation layer on the surface of the nano copper generated by sintering, and at the same time introduces long-chain organic amines to significantly improve the hydrophobic properties of nano copper, so that a more stable hydrophobic anti-oxidation layer is formed on the surface of the nano copper.

[0030] The laser direct writing modification / reduction sintering based on laser processing of the present invention mainly includes three aspects: first, the instantaneous temperature field constructed by laser high-energy irradiation can promote formic acid and nano copper oxide to undergo partial redox reaction, so that the zero-valent copper surface obtained by reduction is rearranged into Cu (110) crystal plane; then the copper ions in the reaction product continue to coordinate and complex with the formate obtained by decomposition to form a passivation protective film on the surface of nano copper, which can effectively improve the thermal stability of nano copper in a high temperature environment. Second, after the aforementioned coordination passivation layer is formed, the hydrophilic amino group contained in the introduced long-chain organic amine will interact with the oxide layer on the surface of nano copper and the exposed copper atoms through chemical bonding, thereby stably adsorbing on the surface of nano copper; then, the hydrophobic long carbon chain in the long-chain organic amine molecule will be arranged in a directional manner, facing the outside, while the hydrophilic amino group is fixed on the surface of nano copper. This directional arrangement of molecules changes the physical and chemical properties of the surface of nano copper, making it exhibit strong hydrophobicity (anti-high humidity corrosion). Third, under the action of laser photothermal, the reducing solvent, dispersant and organic additive in the functional nano copper oxide film are decomposed into aldehyde and carboxyl groups to fully reduce the divalent copper ions to zero-valent copper; at the same time, the molten nano copper adheres to each other under the surface plasma resonance effect, and fuses and agglomerates as the specific surface area decreases, and finally repeatedly melts and solidifies under the action of laser pattern scanning to generate a uniform and continuous conductive matrix. The synergistic effect of the above three aspects is the key to significantly improving the oxidation resistance and stability of nano copper in high temperature and high humidity environments.

[0031] Compared with the prior art, the advantages of the present invention are:

[0032] (1) Functional nano copper oxide ink is simple to prepare, low-cost, easy to store for a long time, not subject to oxidation risk, and suitable for various coating processes such as printing, coating, and printing.

[0033] (2) Laser direct writing modification can induce the coordination passivation of formic acid on the surface of nanocopper and the hydrophobic adsorption of long-chain organic amines on the surface of nanocopper. Compared with the case where there is no formate and long-chain organic amine and the case where only formate acts, it has stronger antioxidant ability and stability in high temperature and high humidity environment.

[0034] (3) Laser reduction sintering can pattern nano-copper oxide after selective photothermal irradiation to generate a nano-copper matrix with excellent conductivity and adhesion.

[0035] (4) Laser direct writing modification / reduction sintering does not rely on cumbersome process steps such as pre-treatment and post-treatment, as well as the addition of external chemical reagents. It does not require vacuum or inert atmosphere and can be carried out directly in the atmospheric environment. The treatment process is simple and it is an environmentally friendly anti-oxidation surface treatment method.

[0036] (5) Laser direct writing modification / reduction sintering is not limited by the shape and size of nano-copper materials and is suitable for multi-scale nano-copper.

[0037] (6) The laser direct writing modification / reduction sintering process is highly efficient and can significantly shorten the production cycle compared to traditional surface treatment methods. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is an optical photograph of the prepared functional nano copper oxide ink;

[0039] Figure 2 The optical photo of the prepared rectangular pattern high temperature and high humidity resistant nano copper electrode and the magnified optical microscope photo of the interface;

[0040] Figure 3 The relative resistance change of high temperature resistant nano copper with different formic acid concentrations at 180°C over time;

[0041] Figure 4 The relative resistance change of high temperature and high humidity resistant nano copper with different oleylamine concentrations at 180°C over time;

[0042] Figure 5 The relative resistance changes of nano copper (original), high temperature resistant nano copper (FA) and high temperature and humidity resistant nano copper (FFA) at 180°C over time;

[0043] Figure 6 The relative resistance change of nano copper with high temperature and humidity resistance at 180℃, 190℃, 200℃, 210℃ and 220℃ respectively over time;

[0044] Figure 7 To compare the relative resistance changes of nano copper, high temperature resistant nano copper and high temperature and high humidity resistant nano copper over time at 80°C and 90% RH;

[0045] Figure 8 Optical microscope photos of control nano copper, high temperature resistant nano copper and high temperature and high humidity resistant nano copper before and after being subjected to 80℃ and 90%RH;

[0046] Fig. 9 To compare the relative resistance changes of nano-copper, high temperature resistant nano-copper and high temperature and high humidity resistant nano-copper over time during 22 cycles between 25°C, 30%RH and 90%RH; Fig.10 To compare the relative resistance changes of nano-copper, high temperature resistant nano-copper and high temperature and high humidity resistant nano-copper over time during 22 cycles between 80% RH, 20°C and 90°C. DETAILED DESCRIPTION

[0047] The present invention is described in detail below by way of embodiments in combination with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and are therefore only used as examples, and cannot be used to limit the protection scope of the present invention.

[0048] Embodiment 1:

[0049] S1: Weigh 0.65 g of polyvinyl pyrrolidone and 0.297 g of formic acid, mix them in 3.0 mL of ethylene glycol, and heat and stir them uniformly at 60° C. and 1000 rpm for 6 h to obtain a functional precursor solution 1;

[0050] S2: Weigh 0.377 g of oleylamine and mix it in the functional precursor solution 1, and evenly heat and stir at 55° C. and 1000 rpm for 2 h to obtain a functional precursor solution;

[0051] S3: Weigh 1.5 g of copper oxide nanowires (40 nm) and place them in a functional precursor solution for full ultrasonic dispersion. The ultrasonic real-time temperature is 55° C., the ultrasonic pulse width is 0.1 s, and the ultrasonic time is 2.5 min to obtain a functional nano copper oxide solution 1;

[0052] S4: Weigh 1.5 g of copper oxide nanowires (40 nm) and place them in the functional nano copper oxide solution 1 for full ultrasonic dispersion. The ultrasonic real-time temperature is 55° C., the ultrasonic pulse width is 0.1 s, and the ultrasonic time is 3 min to obtain a functional nano copper oxide ink;

[0053] S5: Mechanically shake the functional nano copper oxide ink for 0.5 min and let it stand for later use;

[0054] S6: Take a flexible polyimide film substrate with a thickness of 50 μm and a size of 30×30 mm, wash the surface impurities with isopropanol ultrasonic for 5 min, and dry it for later use;

[0055] S7: subjecting the flexible polyimide film substrate to oxygen plasma surface treatment for 120 s;

[0056] S8: The flexible polyimide film substrate treated in S7 is vacuum adsorbed on the spin coating chuck of the spin coater, and 1.0 mL of functional nano copper oxide ink is dropped on the center of the substrate, and the substrate is spin-coated at a speed of 1500 rpm for 10 s and 800 rpm for 5 s;

[0057] S9: placing the flexible polyimide film substrate after spin coating the functional nano copper oxide ink in a constant temperature blast drying oven or a vacuum drying oven for heating and drying at a temperature of 50° C. for 3 hours to obtain a functional nano copper oxide film;

[0058] S10: placing the flexible polyimide film substrate covered with the functional nano copper oxide film on a laser processing platform with a 532nm wavelength continuous green light, and adjusting the height of the processing platform for laser focusing;

[0059] S11: Draw a rectangular electrode pattern with a size of 9×3 mm, so that the laser performs patterned direct writing (laser direct writing modification / reduction sintering) along the rectangular electrode pattern filling path with a power of 210 mW, a speed of 40 mm / s, and a line scanning period of 30 μm, and converts the black nano-copper oxide at the scanning path into red nano-copper to obtain a high temperature and high humidity resistant nano-copper electrode.

[0060] Figure 1 This is an optical photograph of the prepared functional nano-copper oxide ink.

[0061] Figure 2 The optical photograph of the prepared rectangular pattern high temperature and high humidity resistant nano copper electrode and the magnified optical microscope photograph of the interface.

[0062] Embodiment 2:

[0063] S1: Weigh 0.65 g polyvinyl pyrrolidone, 0.297 g formic acid and 0.2 g isopropanolamine, mix them in 3.0 mL ethylene glycol, and heat and stir them uniformly at 60 °C and 1000 rpm for 8 h to obtain functional precursor solution 1;

[0064] S2: Weigh 0.39 g of oleylamine and mix it in the functional precursor solution 1, and heat and stir uniformly at 60°C and 1000 rpm for 2 h to obtain a functional precursor solution;

[0065] S3 to S10 are the same as in Example 1;

[0066] S11: Draw a rectangular electrode pattern with a size of 9×3 mm, so that the laser performs patterned direct writing (laser direct writing modification / reduction sintering) along the rectangular electrode pattern filling path with a power of 180 mW, a speed of 60 mm / s, and a line scanning period of 30 μm, and converts the black nano copper oxide at the scanning path into red nano copper to obtain a high temperature and high humidity resistant nano copper electrode.

[0067] Embodiment 3:

[0068] S1: Weigh 0.65 g polyvinyl pyrrolidone, 0.297 g formic acid and 0.4 g N,N-dimethylformamide, mix in 3.0 mL ethylene glycol, and heat and stir uniformly at 60 °C and 1000 rpm for 6 h to obtain functional precursor solution 1;

[0069] S2: Weigh 0.39 g of oleylamine and mix it in the functional precursor solution 1, and heat and stir uniformly at 60°C and 1000 rpm for 2 h to obtain a functional precursor solution;

[0070] S3 to S10 are the same as in Example 1;

[0071] S11: Draw a rectangular electrode pattern with a size of 9×3 mm, so that the laser performs patterned direct writing (laser direct writing modification / reduction sintering) along the rectangular electrode pattern filling path with a power of 190 mW, a speed of 60 mm / s, and a line scanning period of 30 μm, and converts the black nano copper oxide at the scanning path into red nano copper to obtain a high temperature and high humidity resistant nano copper electrode.

[0072] Embodiment 4:

[0073] S1: Weigh 0.65 g of polyvinyl pyrrolidone and 0.158 g / 0.226 g / 0.297 g / 0.371 g / 0.448 g of formic acid in sequence, mix in 3.0 mL of ethylene glycol, and heat and stir uniformly at 60 °C and 1000 rpm for 6 h to obtain 5 precursor solutions with different formic acid concentrations;

[0074] S2: Weigh 1.5 g of copper oxide nanowires (40 nm) respectively and place them in 5 precursor solutions for full ultrasonic dispersion. The ultrasonic real-time temperature is 55° C., the ultrasonic pulse width is 0.1 s, and the ultrasonic time is 2.5 min to obtain 5 nano copper oxide solutions 1;

[0075] S3: Weigh 1.5 g of copper oxide nanowires (40 nm) respectively and place them in 5 nano copper oxide solutions 1 for full ultrasonic dispersion. The ultrasonic real-time temperature is 55° C., the ultrasonic pulse width is 0.1 s, and the ultrasonic time is 3 min to obtain 5 nano copper oxide inks with different formic acid concentrations;

[0076] S4: Mechanically shake the nano copper oxide ink for 3 minutes and let it stand for later use;

[0077] S5: Take 5 flexible polyimide film substrates with a thickness of 50 μm and a size of 30×30 mm, wash the surface impurities with isopropanol ultrasonic for 5 min, and dry them for later use;

[0078] S6: subjecting the flexible polyimide film substrate to oxygen plasma surface treatment for 120 s;

[0079] S7: The flexible polyimide film substrate treated in S6 was vacuum adsorbed on the spin coating chuck of the spin coater in sequence, and 1.0 mL of nano copper oxide ink with different formic acid concentrations was dripped on the center of the substrate in sequence, and the coating was performed at a speed of 1500 rpm for 10 s and 800 rpm for 5 s;

[0080] S8: placing the flexible polyimide film substrate after spin coating the nano copper oxide ink in a constant temperature blast drying oven or a vacuum drying oven for heating and drying at a temperature of 50° C. for 3 hours to obtain a nano copper oxide film;

[0081] S9: placing the flexible polyimide film substrate covered with the nano copper oxide film on a laser processing platform with a 532nm wavelength continuous green light in sequence, and adjusting the height of the processing platform for laser focusing;

[0082] S10: Draw a rectangular electrode pattern with a size of 9×3 mm, so that the laser performs pattern direct writing (laser direct writing passivation / reduction sintering) along the rectangular electrode pattern filling path in sequence at a power of 210 mW, a speed of 40 mm / s, and a line scanning period of 30 μm, and converts the black nano copper oxide at the scanning path into red nano copper to obtain a high temperature resistant nano copper electrode;

[0083] S11: Manually apply a thin silver paste to both ends of each high-temperature resistant nano-copper electrode to draw out the electrode, and place it in a vacuum drying oven for heating and drying at a temperature of 60° C. for 3 hours;

[0084] S12: designing a voltage divider circuit board according to the resistance value of the high temperature resistant nano copper electrode, and connecting each high temperature resistant nano copper electrode in turn through an alligator clip wire, and connecting to a data acquisition instrument through a DuPont line;

[0085] S13: placing the high temperature resistant nano copper electrode in a constant temperature blast drying oven, setting the temperature to 180° C., and recording the partial pressure change in real time through a data acquisition instrument;

[0086] S14: The data results are converted into relative resistance changes of the high temperature resistant nano copper electrode through a voltage division formula.

[0087] Figure 3 The relative resistance change of high temperature resistant nano copper with different formic acid concentrations at 180°C over time. It can be seen that when the relative content of formic acid is 91%, its high temperature resistance after laser direct writing modification is the best (the relative resistance change rate is about 0.38). When the formic acid content decreases, the complex formed by its reaction and coordination with the surface of nano copper is not enough to resist oxygen invasion, and the high temperature oxidation resistance is poor. When the formic acid content increases, it will trigger additional reactions at the interface with nano copper, affecting the passivation effect and surface properties, and will cause the high temperature oxidation resistance of nano copper to fail in the long run.

[0088] Embodiment 5:

[0089] S1: Weigh 5 times 0.65 g of polyvinyl pyrrolidone and 0.297 g of formic acid, mix them in 3.0 mL of ethylene glycol, and heat and stir them uniformly at 60° C. and 1000 rpm for 6 h to obtain functional precursor solution 1;

[0090] S2: Weigh 0.122 g / 0.208 g / 0.297 g / 0.391 g / 0.488 g of oleylamine in sequence and mix them in the functional precursor solution 1, and heat and stir them uniformly at 55° C. and 1000 rpm for 4 h to obtain 5 functional precursor solutions with different oleylamine concentrations;

[0091] S3: Weigh 1.5 g of copper oxide nanowires (40 nm) respectively and place them in 5 functional precursor solutions for full ultrasonic dispersion. The ultrasonic real-time temperature is 55° C., the ultrasonic pulse width is 0.1 s, and the ultrasonic time is 2.5 min to obtain 5 functional nano copper oxide solutions 1;

[0092] S4: Weigh 1.5 g of copper oxide nanowires (40 nm) respectively and place them in 5 functional nano copper oxide solutions 1 for full ultrasonic dispersion. The ultrasonic real-time temperature is 55° C., the ultrasonic pulse width is 0.1 s, and the ultrasonic time is 3 min to obtain 5 functional nano copper oxide inks with different oleylamine concentrations;

[0093] S5-S7 are the same as S4-S6 in Example 4;

[0094] S8: Vacuum adsorb the flexible polyimide film substrate onto the spin coating chuck of the spin coater in sequence, and drip 1.0 mL of functional nano copper oxide ink with different oleylamine concentrations on the center of the substrate in sequence, and spin coat at 1500 rpm for 10 s and 800 rpm for 5 s;

[0095] S9: placing the flexible polyimide film substrate after spin coating the functional nano copper oxide ink in a constant temperature blast drying oven or a vacuum drying oven for heating and drying at a temperature of 55° C. for 4 hours to obtain a functional nano copper oxide film;

[0096] S10: placing the flexible polyimide film substrate covered with the functional nano copper oxide film on a laser processing platform with a continuous green light of 532 nm wavelength in sequence, and adjusting the height of the processing platform for laser focusing;

[0097] S11: Draw a rectangular electrode pattern with a size of 9×3 mm, so that the laser performs pattern direct writing (laser direct writing modification / reduction sintering) along the rectangular electrode pattern filling path in sequence at a power of 210 mW, a speed of 40 mm / s, and a line scanning period of 30 μm, and converts the black nano copper oxide at the scanning path into red nano copper to obtain a high temperature and high humidity resistant nano copper electrode;

[0098] S12: Manually apply a thin silver paste to both ends of each high temperature and high humidity resistant nano copper electrode to draw out the electrode, and place it in a vacuum drying oven for heating and drying at a temperature of 60° C. for 3 hours;

[0099] S13: designing a voltage divider circuit board according to the resistance value of the high temperature and high humidity resistant nano copper electrode, and connecting each high temperature and high humidity resistant nano copper electrode in turn through an alligator clip wire, and connecting the data acquisition instrument through a DuPont line;

[0100] S14: placing the high temperature and high humidity resistant nano copper electrode in a constant temperature blast drying oven, setting the temperature to 180° C., and recording the partial pressure change in real time through a data acquisition instrument;

[0101] S15: The data results are converted into the relative resistance change of the high temperature and high humidity resistant nano copper electrode through the voltage division formula.

[0102] Figure 4 The relative resistance change of high temperature and high humidity resistant nano copper with different oleylamine concentrations at 180°C over time. It can be seen that on the basis of the optimal formic acid relative content (91%), when the relative oleylamine content is 91%, its high temperature oxidation resistance after laser direct writing modification is greatly improved (the relative resistance change rate is about 0.04). And after adding different contents of oleylamine, the thermal stability of nano copper is enhanced overall.

[0103] Embodiment 6:

[0104] S1: Weigh 0.65 g of polyvinyl pyrrolidone and mix it in 3.0 mL of ethylene glycol, and heat and stir evenly at 60 °C and 1000 rpm for 2 h to obtain a control precursor solution;

[0105] S2: Weigh 1.5 g of copper oxide nanowires (40 nm) and place them in a control precursor solution for full ultrasonic dispersion. The ultrasonic real-time temperature is 55° C., the ultrasonic pulse width is 0.1 s, and the ultrasonic time is 2.5 min to obtain a control nano copper oxide solution 1;

[0106] S3: Weigh 1.5 g of copper oxide nanowires (40 nm) and place them in the control nano copper oxide solution 1 for full ultrasonic dispersion. The ultrasonic real-time temperature is 55° C., the ultrasonic pulse width is 0.1 s, and the ultrasonic time is 3 min to obtain a control nano copper oxide ink;

[0107] S4: Mechanically shake the control nano copper oxide ink for 0.5 min and let it stand for later use;

[0108] S5-S6 are the same as S6-S7 in Example 1;

[0109] S7: Vacuum adsorb the flexible polyimide film substrate on the spin coating chuck of the spin coater, and drop 1.0 mL of the control nano copper oxide ink at the center of the substrate, and spin coat at 1500 rpm for 10 s and 800 rpm for 5 s;

[0110] S8: placing the flexible polyimide film substrate after spin coating the control nano copper oxide ink in a constant temperature blast drying oven or a vacuum drying oven for heating and drying at a temperature of 60° C. for 2 h to obtain a control nano copper oxide film;

[0111] S9: placing the flexible polyimide film substrate covered with the control nano copper oxide film on a laser processing platform with a 532nm wavelength continuous green light, and adjusting the height of the processing platform for laser focusing;

[0112] S10: Draw a rectangular electrode pattern with a size of 9×3 mm, so that the laser performs patterned direct writing (laser reduction sintering) along the rectangular electrode pattern filling path at a power of 210 mW, a speed of 40 mm / s, and a line scanning period of 30 μm, and converts the black nano-copper oxide at the scanning path into red nano-copper to obtain a control nano-copper electrode.

[0113] S11: Manually apply a thin silver paste to both ends of the control nano-copper electrode to draw out the electrode, and place it in a vacuum drying oven for heating and drying at 60°C for 3 hours;

[0114] S12: designing a voltage divider circuit board according to the resistance value of the control nano-copper electrode, and connecting the control nano-copper electrode through an alligator clip wire, and connecting the data acquisition instrument through a DuPont line;

[0115] S13: Weigh 0.65 g of polyvinyl pyrrolidone and 0.297 g of formic acid, mix them in 3.0 mL of ethylene glycol, and evenly heat and stir at 60° C. and 1000 rpm for 6 h to obtain a formic acid precursor solution;

[0116] S14: Weigh 1.5 g of copper oxide nanowires (40 nm) and place them in a formic acid precursor solution for full ultrasonic dispersion. The ultrasonic real-time temperature is 55° C., the ultrasonic pulse width is 0.1 s, and the ultrasonic time is 2.5 min to obtain a formic acid nano copper oxide solution 1;

[0117] S15: Weigh 1.5 g of copper oxide nanowires (40 nm) and place them in the formic acid nano-copper oxide solution 1 for full ultrasonic dispersion, with the ultrasonic real-time temperature being 55° C., the ultrasonic pulse width being 0.1 s, and the ultrasonic time being 3 min, to obtain formic acid nano-copper oxide ink;

[0118] S16: Mechanically shake the formic acid nano copper oxide ink for 3 minutes and let it stand for standby use;

[0119] S17-S18 are the same as S6-S7 in Example 1;

[0120] S19: Vacuum adsorb the flexible polyimide film substrate on the spin coating chuck of the spin coater, and drip 1.0 mL of formic acid nano copper oxide ink on the center of the substrate, spin coating at 1500 rpm for 10 s and 800 rpm for 5 s;

[0121] S20: placing the flexible polyimide film substrate after spin coating the formic acid nano copper oxide ink in a constant temperature blast drying oven or a vacuum drying oven for heating and drying at a temperature of 50° C. for 3 hours to obtain a formic acid nano copper oxide film;

[0122] S21: placing a flexible polyimide film substrate covered with formic acid nano-copper oxide film on a laser processing platform with a 532nm wavelength continuous green light, and adjusting the height of the processing platform for laser focusing;

[0123] S22: Draw a rectangular electrode pattern with a size of 9×3 mm, so that the laser performs pattern direct writing (laser direct writing passivation / reduction sintering) along the rectangular electrode pattern filling path at a power of 210 mW, a speed of 40 mm / s, and a line scanning period of 30 μm, and converts the black nano copper oxide at the scanning path into red nano copper to obtain a high temperature resistant nano copper electrode;

[0124] S23: Manually apply a thin silver paste to both ends of the high temperature resistant nano copper electrode to draw out the electrode, and place it in a vacuum drying oven for heating and drying at a temperature of 60° C. for 3 h;

[0125] S24: designing a voltage divider circuit board according to the resistance value of the high temperature resistant nano copper electrode, connecting the high temperature resistant nano copper electrode through an alligator clip wire, and connecting the data acquisition instrument through a DuPont line;

[0126] S25 to S35 are the same as S1 to S11 in Example 1;

[0127] S36: Manually apply a thin silver paste on both ends of the high temperature and high humidity resistant nano copper electrode to draw out the electrode, and place it in a vacuum drying oven for heating and drying at a temperature of 60°C for 3 hours;

[0128] S37: Design a voltage divider circuit board based on the resistance value of the high temperature and high humidity resistant nano copper electrode, connect the high temperature and high humidity resistant nano copper electrode through alligator clip wires, and connect the data acquisition instrument through DuPont wires;

[0129] S38: placing the control nano-copper electrode, the high temperature resistant nano-copper electrode and the high temperature and high humidity resistant nano-copper electrode in a constant temperature blast drying oven, setting the temperature to 180° C., and recording the partial pressure changes in real time through a data acquisition instrument;

[0130] S39: The data results are converted into relative resistance changes of the control nano-copper electrode, the high-temperature resistant nano-copper electrode and the high-temperature and high-humidity resistant nano-copper electrode through the voltage division formula.

[0131] Figure 5 The relative resistance changes of control nano-copper, high temperature resistant nano-copper and high temperature and high humidity resistant nano-copper over time at 180°C. It can be seen that since the control nano-copper did not undergo coordination passivation modification on the surface under laser treatment and accelerated failure in a high temperature environment, the high temperature resistant nano-copper has good high temperature oxidation resistance (relative resistance increase trend is small) due to the formation of a coordination complex protective layer through laser induced surface passivation, and the high temperature and high humidity resistant nano-copper simultaneously introduces oleylamine for surface adsorption during the laser induced modification process, which is more conducive to blocking oxygen invasion in a hot environment, and thus has the best high temperature resistance.

[0132] Embodiment 7:

[0133] S1 to S11 are the same as in Example 1;

[0134] S12: Repeat S1 to S11 4 times, and finally obtain 5 nano copper electrodes resistant to high temperature and high humidity;

[0135] S13-S14 are the same as S12-S13 in Example 5;

[0136] S15: placing the high temperature and high humidity resistant nano copper electrode in a constant temperature blast drying oven, setting the temperature to 180°C / 190°C / 200°C / 210°C / 220°C in sequence, and recording the partial pressure change in real time through a data acquisition instrument;

[0137] S16: The data results under different high temperature environments are converted into the relative resistance change of the high temperature and high humidity resistant nano copper electrode through the voltage division formula.

[0138] Figure 6 The relative resistance changes of high temperature and high humidity resistant nano copper over time at 180℃, 190℃, 200℃, 210℃, and 220℃ respectively. It can be seen that when the high temperature environment is 180℃ and 190℃, the thermal stability of high temperature and high humidity resistant nano copper is equivalent, with no significant difference. When the temperature continues to rise to 200℃ and above, the electrical performance degradation of high temperature and high humidity resistant nano copper shows a trend of increasing. It can be considered that 190℃ is the upper temperature limit of high temperature and high humidity resistant nano copper.

[0139] Embodiment 8:

[0140] S1 to S37 are the same as in Example 6;

[0141] S38: placing the control nano-copper electrode, the high temperature resistant nano-copper electrode and the high temperature and high humidity resistant nano-copper electrode in an environmental test chamber, setting the temperature to 80° C. and the humidity to 90% RH, and recording the partial pressure changes in real time through a data acquisition instrument;

[0142] S39 is the same as Example 6.

[0143] Figure 7 The relative resistance changes of control nano-copper, high temperature resistant nano-copper and high temperature and high humidity resistant nano-copper over time at 80°C and 90% RH. It can be seen that the high temperature resistant nano-copper is not resistant to high humidity due to the hydrophobic modification of the surface without long-chain organic amines. In comparison, the high temperature and high humidity resistant nano-copper has the best high humidity resistance, and the relative resistance change rate is about 0.45 after 85 hours of continuous high humidity. The illustration shows that the hydrophobic angles of the control nano-copper, high temperature resistant nano-copper and high temperature and high humidity resistant nano-copper are 30°, 8° and 130° respectively.

[0144] Figure 8 The optical microscope photos of the control nano copper, high temperature resistant nano copper and high temperature and high humidity resistant nano copper before and after experiencing 80℃ and 90% RH. It can be seen that the surface of the high temperature resistant nano copper has been covered with dark green patina after continuous high humidity corrosion, and the surface of the control nano copper also shows some purple-red wet oxidation marks. In comparison, the surface of the high temperature and high humidity resistant nano copper has no obvious changes before and after high humidity.

[0145] Embodiment 9:

[0146] S1 to S37 are the same as in Example 6;

[0147] S38: placing the control nano-copper electrode, the high temperature resistant nano-copper electrode and the high temperature and high humidity resistant nano-copper electrode in an environmental test chamber, setting the temperature to 25°C, and the humidity to undergo 22 cycles between 30% RH and 90% RH (the duration of humidity climbing and falling is 1 hour, and the duration of humidity at 30% RH and 90% RH is 1 hour), and recording the partial pressure changes in real time through a data acquisition instrument;

[0148] S39 is the same as Example 6.

[0149] Fig. 9 The relative resistance changes of nano copper, high temperature resistant nano copper and high temperature and high humidity resistant nano copper over time during 22 cycles between 25°C, 30%RH and 90%RH are compared. It can be seen that after eliminating the high temperature interference (25°C), the high temperature and high humidity resistant nano copper under low and high humidity cycles still has excellent anti-corrosion stability (the relative resistance change rate after 74h is about 0.05).

[0150] Embodiment 10:

[0151] S1 to S37 are the same as in Example 6;

[0152] S38: placing the control nano-copper electrode, the high temperature resistant nano-copper electrode and the high temperature and high humidity resistant nano-copper electrode in an environmental test chamber, setting the humidity to 80% RH, and subjecting the temperature to 22 cycles between 20°C and 90°C (the duration of temperature rise and fall is 1 hour, and the duration of temperature at 20°C and 90°C is 1 hour), and recording the partial pressure changes in real time through a data acquisition instrument;

[0153] S39 is the same as Example 6.

[0154] Fig.10 The relative resistance changes of nano copper, high temperature resistant nano copper and high temperature and high humidity resistant nano copper over time during 22 cycles between 80% RH, 20°C and 90°C are compared. It can be seen that after the introduction of temperature cycling in a continuous high humidity environment, although the high temperature and high humidity resistant nano copper will respond slightly to temperature changes, it still has good thermal stability and corrosion resistance overall (the relative resistance change rate after 72h is about 0.44).

Claims

1. A high temperature and high humidity resistant nano copper, characterized in that: The high temperature and high humidity resistant nano copper is nano copper with formate-copper ion complex and alkyl hydrophobic layer modified on the surface.

2. The method for preparing high temperature and humidity resistant nano copper according to claim 1, characterized in that: include: The alcohol solvent, the organic dispersant, the organic additive 1, the organic additive 2, the long-chain organic amine and the formic acid are mixed and heated and stirred to obtain a functional precursor solution; the nano copper oxide is added to the functional precursor solution and fully ultrasonically dispersed to obtain a functional nano copper oxide ink; The functional nano copper oxide ink is applied on the pretreated substrate, and heated and dried to obtain a functional nano copper oxide film; The functional nano copper oxide film is modified by laser direct writing / reduction sintering to obtain high temperature and high humidity resistant nano copper.

3. The method for preparing high temperature and humidity resistant nano copper according to claim 2, characterized in that: The alcohol solvent is selected from one or more of monohydric alcohol, dihydric alcohol and polyhydric alcohol.

4. The method for preparing high temperature and humidity resistant nano copper according to claim 2, characterized in that: The organic dispersant is selected from one or more of polyacrylamide organic polymers, polyethylene oxide organic polymers, hexadecyltrimethylammonium bromide, tannin, and lignin.

5. The method for preparing high temperature and humidity resistant nano copper according to claim 2, characterized in that: The organic auxiliary agent 1 is an organic amide, and the organic auxiliary agent 2 is an organic alcohol amine.

6. The method for preparing high temperature and high humidity resistant nano copper according to claim 2, characterized in that: The long-chain organic amine is selected from one or more of dodecylamine, tetradecylamine, hexadecylamine, octadecylamine, eicosylamine, behenylamine, dodecylbenzylamine, hexadecylbenzylamine, eicosylbenzylamine, dodecyldimethylamine, dodecyltrimethylamine, tetradecyldimethylamine, hexadecyldimethylamine, octadecylmethylamine, octadecyldimethylamine, octadecylethylamine, octadecyldiethylamine, octadecylaniline, eicosyldimethylamine, behenyltrimethylamine, N-methyloctadecylamine, N,N-dimethyldodecylamine, N,N-dimethylhexadecylamine, N,N-dimethyloctadecylamine, N-ethyldodecylamine, N-butyldodecylamine, diethylenetriamine, and oleylamine.

7. The method for preparing high temperature and humidity resistant nano copper according to claim 2, characterized in that: The functional nano copper oxide ink comprises 34.8-45.1wt% nano copper oxide, 38.6-43.5wt% alcohol solvent, 5.9-8.5wt% organic dispersant, 0.0-2.5wt% organic auxiliary agent 1, 0.0-5.2wt% organic auxiliary agent 2, 4.5-5.0wt% long-chain organic amine, and 3.4-4.0wt% formic acid.

8. The method for preparing high temperature and high humidity resistant nano copper according to claim 2, characterized in that: The pretreatment is oxygen plasma surface treatment, and the treatment time is 60s to 150s.

9. The method for preparing high temperature and high humidity resistant nano copper by laser direct writing according to claim 2, characterized in that: The substrate is a flexible substrate or a rigid substrate; the flexible substrate is selected from one or more of polyimide (PI), polyethylene terephthalate (PET), polyvinyl alcohol (PVA), polyethylene naphthalate (PEN), and the rigid substrate is selected from one or more of polyetheretherketone (PEEK), polyphenylene sulfide (PPS), polysulfone (PSF), liquid crystal polymer (LCP), glass, silicon wafer, and ceramic.

10. The method for preparing high temperature and high humidity resistant nano copper according to claim 2, characterized in that: The laser is a continuous green light with a wavelength of 532nm, the power of the laser direct writing modification / reduction sintering is 100-300mW, the speed is 20-200mm / s, and the scanning period is 20-40μm.

Citation Information

Patent Citations

  • Novel oxidizing-resistant nanometer copper soldering paste and preparation method and application thereof

    CN107267938A

  • Preparation method of antioxidant copper-based conductive ink

    CN107337965A

  • Surface processing method for copper-containing material

    CN107460464A

  • Preparation method of anti-oxidation micro-nano copper material

    CN109954876A

  • Method for preparing nanocarbon coated copper powder

    CN110000373A

Cited By

  • Antioxidant nano-copper powder, preparation method thereof and nano-copper soldering paste

    CN119634742A