Preparation method of copper seal with high stamp-pad ink wettability
The copper seal body with a special pore structure is prepared through powder metallurgy near-net forming technology, which solves the problem of poor wettability of the printing oil on the surface of the copper seal, achieves clear and complete stamped images and text, and improves the clarity of multiple stampings. At the same time, the seal is prevented from falling off.
Patent Information
- Application Number
- CN202410941266.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-01
AI Technical Summary
The surface of the copper seal has poor wettability with printing oil, resulting in unclear and incomplete stamped images and text.
The powder metallurgy near-net forming technology is used to prepare the copper seal body with a special pore structure. The compact is formed through position limiting or constant pressure pressing, and the blank is formed by hydrogen sintering. It is then machining and shaping, sealing and grinding and polishing to improve the surface of the seal. The wettability of ink.
On the premise of maintaining high hardness, it increases the specific surface area of the seal surface, improves the wettability of the stamp oil, ensures that the stamped image and text are clear and complete, and has the functions of absorbing and storing oil to prevent the seal from falling off.
Smart Images

Figure CN118720134A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of copper seals, in particular to a method for preparing a copper seal with high printing oil wettability. Background Art
[0002] Seals have a long history in China, dating back to the Yao and Shun era more than 4,000 years ago. They are one of the representatives of Chinese traditional culture. At present, the mainstream products in the seal market include: photosensitive seals, ink-returning seals, atomic seals and copper seals. Compared with other types of seals, copper seals have the advantages of not easy to deform, wear-resistant, resistant to ink erosion, and long service life. They are ideal materials for official seals. However, due to the poor wettability of the copper seal surface to ink, the stamped images and texts are unclear and incomplete.
[0003] The Chinese invention patent with publication number CN115488343B discloses a method for preparing a gradient porous copper stamp head and a seal containing the stamp head, comprising the following steps: S1: screening copper powders of different particle sizes; S2: firstly placing copper powder in a mold to press a stamp oil layer, secondly placing copper powder on the stamp oil layer to press a transition layer, then placing copper powder on the transition layer and doping a mixed pore-forming agent to press an oil reservoir layer, then placing copper powder on the oil reservoir layer to press an annular transition layer, and finally placing copper powder on the annular transition layer to press an annular dense layer to obtain a stamp head compact; S3: performing oxygen-free sintering on the stamp head compact to obtain a stamp head sintered body; S4: performing fine treatment on the stamp head sintered body, and then engraving on the surface of the stamp oil layer to obtain a stamp head. This patent mainly prepares a stamp head from the perspective of self-storing stamp oil, which improves the efficiency of stamps, but it does not solve the technical problem that the copper stamp surface has poor wettability to the stamp oil, so there is still a need to improve the structure and preparation of the stamp. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a method for preparing a copper seal with high ink wettability, wherein a copper seal body with a special pore structure is prepared by powder metallurgy near-net forming technology, and the stamped image and text are clear and complete.
[0005] The purpose of the present invention is achieved through the following technical solutions: The present invention provides a method for preparing a copper seal with high printing oil wettability, comprising the following steps: Step 1: placing copper metal powder in a mold and pressing it to form a compact; Step 2: sintering the pressed green sheet in a hydrogen atmosphere to form a green sheet; Step 3: Machining and shaping the blank to form a chapter blank; Step 4: Choose one side of the seal blank as the bonding surface and perform sealing treatment; Step 5: Except for the bonding surface, select any side of the seal blank as the seal engraving surface, and perform grinding and polishing to form the seal body; Step 6: Carve the seal body to form images and texts, and assemble it with the seal shell to obtain a copper seal.
[0006] The present invention uses powder metallurgy near-net forming technology to prepare a copper seal body with a special pore structure. Under the premise of maintaining high hardness (compared to other seal body materials), the seal body mass is reduced, and the specific surface area of the seal surface is increased, and the wettability of the seal surface to the printing oil is improved. After the copper seal is stamped, the image and text are very clear and complete. At the same time, due to the existence of the pore structure, the copper seal also has the effect of absorbing and storing oil after stamping. Due to the improvement of the preparation process, the pore structure inside the copper seal also has better wettability for the printing oil, so it has better oil absorption and storage effects, and further improves the clarity of the seal for multiple stamping images and texts. In addition, the present invention can effectively prevent the printing oil from penetrating and contaminating the seal body and the adhesive surface of the seal shell by performing a special process sealing treatment on the non-engraved seal surface of the seal body, and avoid the phenomenon of the seal body falling off during the use of the seal. The present invention is mainly used in handle copper seals and ink-returning copper seals, and the preparation process involved is simple and efficient, and is suitable for industrial production.
[0007] Preferably, in step 1, the copper metal powder is made of one of red copper, bronze and brass, and the powder particle size is 100-400 mesh.
[0008] If the powder particle size is too large, the pores of the sintered seal will be large, the engraved images will be intermittent, and the stamped images will also be discontinuous; if the powder particle size is too small, the pore size of the seal body will be too small, which will reduce the wettability of the surface to the printing oil and make the stamped images unclear.
[0009] Preferably, in step one, the pressing method is position-limited pressing or constant-pressure pressing.
[0010] Preferably, the compression ratio of the limited pressing is 1.8-2.5, and the holding time is 1-60s; the pressure of the constant pressure pressing is 150-500MPa, and the holding time is 1-60s; the shape of the pressed blank is round, oval or rectangular, and the thickness of the pressed blank is 2-15mm.
[0011] The pressing pressure is high, the porosity is low, the seal body is denser, the surface has poor wettability to printing oil, and the stamped image is unclear; if the pressing pressure is too low, the blank is difficult to form and is prone to cracking and breaking.
[0012] Preferably, in step 2, the sintering parameters are: sintering temperature is 0.75-0.95 times the melting point of copper metal powder, holding time is 2.5-5h, heating rate is 10-15°C / min; dew point of hydrogen is ≤-20°C.
[0013] Preferably, the melting point of the copper metal powder is 830-1050°C.
[0014] The original copper material powder will certainly be oxidized to varying degrees before sintering. Although it has little effect on its sintering activity, the surface oxidation will form an oxide film, causing the material to "not burn through", causing the sintering neck to stop or change direction when it grows to this point, ultimately affecting the pore morphology. The present invention needs to improve the wettability of the stamp surface to the printing ink, and the evenly distributed spherical pores help to better improve the surface wettability. By sintering for a long time at an appropriate sintering temperature and controlling the dew point of hydrogen for reduction protection, the material powder is allowed to fully grow its sintering neck during the sintering process, with more pore structures, and pore spheroidization, and a larger specific surface area, thereby improving the wettability to the printing ink.
[0015] Without adding pore-forming agents and other substances, the present invention achieves uniform spherical pore morphology at a relatively low sintering temperature. If the sintering temperature is too high, it is easy to cause sample densification. If the sintering temperature is too low, the sintering strength is not high, the surface is rough after post-processing, and it is not conducive to stamping. If the sintering time is too short, the sintering strength is low; if the sintering time is too long, it is easy to densify.
[0016] If the dew point of hydrogen is too high, the water content in the gas will be high. On the one hand, the reduction effect of hydrogen on the material is poor, and it is not easy to form a spherical pore morphology; on the other hand, due to the presence of water, the oxidation of the material is aggravated during the heating process. The final result is that it is difficult to form a sintering neck, the powder particles are in point contact, the surface is powdery after processing, and the engraved graphics will be rough. Reduction sintering is an integrated process. Usually, the heating process at a temperature below 500°C can be regarded as the reduction stage. By controlling the dew point of hydrogen, the heating rate can be increased while ensuring the reduction efficiency, shortening the time of the initial heating sintering, which is also conducive to extending the subsequent sintering insulation time. However, if the heating rate is too fast, the gas remaining in the blank will escape quickly during the pressing process, causing large holes in the blank or even cracks.
[0017] Preferably, in step three, the machining method is turning or milling; the thickness of the chapter blank is 70-90% of the thickness of the blank.
[0018] Preferably, in step 4, the sealing treatment is performed by sealing with a sealing agent, sealing by turning or sealing by milling.
[0019] Preferably, the sealing agent used in the sealing process is epoxy resin, polyurethane or silicone.
[0020] Preferably, the parameters of the turning and sealing hole are: spindle speed 700-1500rpm, feed speed 25-100mm / min, and tool material is one of high-speed steel, cemented carbide, and diamond.
[0021] Preferably, the parameters of the milling sealing are: spindle speed 2000-10000rpm, feed speed 100-1000mm / min, and tool material is one of high-speed steel, cemented carbide, and diamond.
[0022] Preferably, in step five, the grinding and polishing process is performed according to the method described in the patent applied for by the applicant (publication number: CN117124193A, invention name: A grinding and polishing method for porous metal materials).
[0023] Preferably, in step six, the copper seal is one of a handle copper seal, a patch copper seal, a light ink-returning copper seal, a heavy ink-returning copper seal, and a steel seal.
[0024] Compared with the prior art, the present invention has the following beneficial effects: (1) The copper seal body with a special pore structure is prepared by powder metallurgy near-net forming technology. While maintaining high hardness (compared with other seal body materials), the specific surface area of the seal surface is increased, and the wettability of the seal surface to the printing ink is improved. After the copper seal is stamped, the image and text are very clear and complete; (2) The porous copper seal also has the function of absorbing and storing oil after stamping. Due to the improvement of the preparation process, the pore structure inside the copper seal also has better wettability for the printing oil, so it has better oil absorption and storage function, further improving the clarity of the seal after multiple stamping of images and texts; (3) By using a special process to seal the non-engraved surface of the seal, it is possible to effectively prevent ink from penetrating and contaminating the adhesive surface between the seal body and the seal shell, thereby avoiding the seal body from falling off during use. This allows better application in handle copper seals and ink-returning copper seals. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the macroscopic appearance of the copper seal body after carving in the present invention.
[0026] Figure 2 It is the stamped image and text of the copper seal in the present invention.
[0027] Figure 3 It is a traditional dense copper seal with images and texts printed on it.
[0028] Figure 4 This is a test diagram of the wettability of the copper seal surface to printing oil in the present invention.
[0029] Figure 5 This is a test chart of the wettability of traditional dense copper seal body to printing oil.
[0030] Figure 6 This is the SEM morphology of the spheroidized pores of the copper seal body in Example 1 of the present invention.
[0031] Figure 7 This is the SEM morphology of the irregular pores in the copper seal of Comparative Example 6 of the present invention. DETAILED DESCRIPTION
[0032] The technical solution of the present invention is described below with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0033] The preparation of a copper seal with high ink wettability comprises the following steps: Step 1: placing copper metal powder (including but not limited to flake, spherical, dendritic and irregular shapes) in a mold and pressing it, the pressing method is limited pressing or constant pressure pressing, to form a pressed green body, the shape of the pressed green body is round, oval or rectangular, and the thickness of the pressed green body is 2-15mm; Step 2: sintering the pressed green sheet in a hydrogen (dew point ≤ -20°C) atmosphere, the sintering temperature being 0.75-0.95 times the melting point of the copper metal powder, the holding time being 2.5-5h, the heating rate being 10-15°C / min, to form a green sheet, the pore structure in the green sheet being a spherical pore morphology, and the pore diameter being 10-30μm; Step 3: machining the blank by turning or milling to form a chapter blank, so that the thickness of the chapter blank is 70-90% of the thickness of the blank; Step 4: arbitrarily select one side of the chapter blank as the bonding surface and perform sealing treatment, wherein the sealing treatment method is sealing with a sealing agent, sealing by turning or sealing by milling; Step 5: Except for the bonding surface, select any side of the seal blank as the seal engraving surface, and perform grinding and polishing to form the seal body; Step 6: Carve the seal body to form images and texts, and assemble it with the seal shell to obtain a copper seal.
[0034] In a specific embodiment of the present invention, the copper metal powder is made of one of red copper, bronze and brass, and is sieved for use. The particle size of the sieved powder is 100-400 meshes.
[0035] In a specific embodiment of the present invention, when the pressing method is position-limited pressing, the compression ratio of the position-limited pressing is 1.8-2.5, and the holding time is 1-60s.
[0036] In a specific embodiment of the present invention, when the pressing method is constant pressure pressing, the constant pressure pressing pressure is 150-500 MPa, and the holding time is 1-60 s.
[0037] In a specific embodiment of the present invention, when the sealing treatment is performed by sealing with a sealing agent, the sealing agent used is epoxy resin, polyurethane or silicone.
[0038] In a specific embodiment of the present invention, when the sealing method is turning sealing, step three and step four can be combined into one step: while the blank is being machined and shaped (turned), one side of the blank is arbitrarily selected as the bonding surface, and the sealing treatment (turning sealing) is performed to form the blank. The parameters of turning sealing are: spindle speed 700-1500rpm, feed speed 25-100mm / min, and the tool material is one of high-speed steel, cemented carbide, and diamond.
[0039] In a specific embodiment of the present invention, when the sealing method is milling sealing, step three and step four can be combined into one step: while the blank is being machined and shaped (milling), one side of the blank is arbitrarily selected as the bonding surface, and the sealing treatment (milling sealing) is performed to form the blank. The parameters of milling sealing are: spindle speed 2000-10000rpm, feed speed 100-1000mm / min, and the tool material is one of high-speed steel, cemented carbide, and diamond.
[0040] In a specific embodiment of the present invention, the grinding and polishing process is performed according to the method described in the patent application (publication number: CN117124193A, invention name: A grinding and polishing method for porous metal materials) applied for by the applicant.
[0041] Example 1 The preparation of a copper seal with high ink wettability comprises the following steps: Step 1: Sieve brass powder (melting point 950°C) to a particle size of 200-350 mesh for later use; Step 2: Weigh an appropriate amount of the powder processed in step 1 and place it in a circular mold. Use limited compression with a compression ratio of 2.1 and hold the pressure for 15 seconds to form a circular compact with a thickness of 5 mm for later use. Step 3: Place the pressed green sheet in an atmosphere furnace, introduce hydrogen with a dew point of -25°C, heat to 780°C at 10°C / min and keep warm for 2.5h, cool with the furnace to form a green sheet for standby use; Step 4: Turn the blank and arbitrarily select one side of the blank as the bonding surface (non-carving surface) to seal the surface. The processing tool material is cemented carbide, the spindle speed is 1200rpm, the feed speed is 50mm / min, and a chapter blank with a thickness of 4mm is formed for standby use; Step 5: Select the opposite side of the bonding surface as the engraved surface of the seal blank, grind and polish the engraved surface to form a seal body with holes on the surface, and set it aside.
[0042] The grinding and polishing process is carried out according to the method described in the patent application of the applicant (publication number: CN117124193A, invention name: A grinding and polishing method for porous metal materials), including the following steps: (1) Place the seal blank on the HMP-1AE automatic grinding and polishing equipment and fix it with a fixture. Use 180-mesh water-abrasive sandpaper to rough-grind and level the surface to be processed. The rough-grinding conditions are: loading force 0.2 MPa, grinding disc speed 200 rpm, spindle speed 0 rpm, and grinding time 2.5 min.
[0043] (2) Then, the rough-ground surface is fine-ground with coarse water-abrasive sandpaper and fine water-abrasive sandpaper in turn until the scratches on the surface are shallow and in the same direction. The mesh number of the coarse water-abrasive sandpaper is 800 mesh, and the grinding conditions are: the loading force is 0.2MPa, the grinding disc speed is 550rpm, the spindle speed is 20rpm, and the grinding time is 10min. The mesh number of the fine water-abrasive sandpaper is 2000 mesh, and the grinding conditions are: the loading force is 0.15MPa, the grinding disc speed is 800rpm, the spindle speed is 35rpm, and the grinding time is 12min.
[0044] (3) Then, the polishing paste with a specification of W2.5 is evenly applied on the woolen polishing cloth, and the processed surface is finely polished; the conditions for fine polishing are: loading force is 0.25 MPa, grinding wheel speed is 1000 rpm, spindle speed is 75 rpm, and polishing time is 30 min.
[0045] (4) Then, ultrasonic cleaning was performed with deionized water and ethanol in turn. The ultrasonic cleaning parameters were the same each time, with a power density of 0.3 W / cm 2 , frequency of 40kHz, temperature of 35℃; vacuum drying to obtain the seal body, the vacuum degree of vacuum drying is -1×10 -5 Pa, temperature is 80℃, time is 30min.
[0046] Step six: Carve the seal body to form specific graphics and texts, which are "Zhejiang Metallurgical Research Institute and Happy Technology", and assemble it with a lightweight ink-returning seal shell to complete the copper seal production.
[0047] Example 2 Compared with Example 1, the copper metal powder material selected in step 1 is different, and the other process flows remain unchanged.
[0048] The preparation of a copper seal with high ink wettability comprises the following steps: Step 1: Sieve the bronze powder (melting point is 850°C) to a particle size of 200-350 mesh for later use; Step 2: Weigh an appropriate amount of the powder processed in step 1 and place it in a circular mold. Use limited compression with a compression ratio of 2.1 and hold the pressure for 15 seconds to form a circular compact with a thickness of 5 mm for later use. Step 3: Place the pressed green sheet in an atmosphere furnace, introduce hydrogen with a dew point of -25°C, heat to 780°C at 10°C / min and keep warm for 2.5h, cool with the furnace to form a green sheet for standby use; Step 4: Turn the blank and arbitrarily select one side of the blank as the bonding surface (non-carving surface) to seal the surface. The processing tool material is cemented carbide, the spindle speed is 1200rpm, the feed speed is 50mm / min, and a chapter blank with a thickness of 4mm is formed for standby use; Step 5: Select the opposite side of the bonding surface as the seal blank engraving surface, and perform grinding and polishing on the engraved surface (grinding and polishing according to the steps in Example 1) to form a seal body with holes on the surface for standby use; Step six: Carve the seal body to form specific graphics and texts, which are "Zhejiang Metallurgical Research Institute and Happy Technology", and assemble it with a lightweight ink-returning seal shell to complete the copper seal production.
[0049] Example 3 Compared with Example 1, the pressing method adopted in step 2 is different, and the other process flows remain unchanged.
[0050] The preparation of a copper seal with high ink wettability comprises the following steps: Step 1: Sieve brass powder (melting point 950°C) to a particle size of 200-350 mesh for later use; Step 2: Weigh an appropriate amount of the powder processed in step 1 and place it in a circular mold. Press it at a constant pressure of 350 MPa and hold the pressure for 15 seconds to form a circular compact with a thickness of 5 mm for later use. Step 3: Place the pressed green sheet in an atmosphere furnace, introduce hydrogen with a dew point of -25°C, heat to 780°C at 10°C / min and keep warm for 2.5h, cool with the furnace to form a green sheet for standby use; Step 4: Turn the blank and arbitrarily select one side of the blank as the bonding surface (non-carving surface) to seal the surface. The processing tool material is cemented carbide, the spindle speed is 1200rpm, the feed speed is 50mm / min, and a chapter blank with a thickness of 4mm is formed for standby use; Step 5: Select the opposite side of the bonding surface as the seal blank engraving surface, and perform grinding and polishing on the engraved surface (grinding and polishing according to the steps in Example 1) to form a seal body with holes on the surface for standby use; Step six: Carve the seal body to form specific graphics and texts, which are "Zhejiang Metallurgical Research Institute and Happy Technology", and assemble it with a lightweight ink-returning seal shell to complete the copper seal production.
[0051] Example 4 Compared with Example 1, the sintering process in step three is different, and the other process flows remain unchanged.
[0052] The preparation of a copper seal with high ink wettability comprises the following steps: Step 1: Sieve brass powder (melting point 950°C) to a particle size of 200-350 mesh for later use; Step 2: Weigh an appropriate amount of the powder processed in step 1 and place it in a circular mold. Use limited compression with a compression ratio of 2.1 and hold the pressure for 15 seconds to form a circular compact with a thickness of 5 mm for later use. Step 3: Place the pressed green sheet in an atmosphere furnace, introduce hydrogen with a dew point of -48°C, heat it to 725°C at a rate of 15°C / min and keep it at that temperature for 4 hours, cool it in the furnace to form a green sheet, and set it aside; Step 4: Turn the blank and arbitrarily select one side of the blank as the bonding surface (non-carving surface) to seal the surface. The processing tool material is cemented carbide, the spindle speed is 1200rpm, the feed speed is 50mm / min, and a chapter blank with a thickness of 4mm is formed for standby use; Step 5: Select the opposite side of the bonding surface as the seal blank engraving surface, and perform grinding and polishing on the engraved surface (grinding and polishing according to the steps in Example 1) to form a seal body with holes on the surface for standby use; Step six: Carve the seal body to form specific graphics and texts, which are "Zhejiang Metallurgical Research Institute and Happy Technology", and assemble it with a lightweight ink-returning seal shell to complete the copper seal production.
[0053] Example 5 Compared with Example 1, the turning process in step 4 is different, and the other process flows remain unchanged.
[0054] The preparation of a copper seal with high ink wettability comprises the following steps: Step 1: Sieve brass powder (melting point 950°C) to a particle size of 200-350 mesh for later use; Step 2: Weigh an appropriate amount of the powder processed in step 1 and place it in a circular mold. Use limited compression with a compression ratio of 2.1 and hold the pressure for 15 seconds to form a circular compact with a thickness of 5 mm for later use. Step 3: Place the pressed green sheet in an atmosphere furnace, introduce hydrogen with a dew point of -25°C, heat to 780°C at 10°C / min and keep warm for 2.5h, cool with the furnace to form a green sheet for standby use; Step 4: Turn the blank and arbitrarily select one side of the blank as the bonding surface (non-carving surface) to seal the surface. The processing tool material is diamond, the spindle speed is 800rpm, the feed speed is 100mm / min, and a chapter blank with a thickness of 4mm is formed for standby use; Step 5: Select the opposite side of the bonding surface as the seal blank engraving surface, and perform grinding and polishing on the engraved surface (grinding and polishing according to the steps in Example 1) to form a seal body with holes on the surface for standby use; Step six: Carve the seal body to form specific graphics and texts, which are "Zhejiang Metallurgical Research Institute and Happy Technology", and assemble it with a lightweight ink-returning seal shell to complete the copper seal production.
[0055] Comparative Example 1 Compared with Example 1, the particle size of the brass powder used in step 1 is 30-80 mesh, and the other process flows remain unchanged.
[0056] The preparation of the copper seal includes the following steps: Step 1: Sieve brass powder (melting point 950°C) to a particle size of 30-80 mesh for later use; Step 2: Weigh an appropriate amount of the powder processed in step 1 and place it in a circular mold. Use limited compression with a compression ratio of 2.1 and hold the pressure for 15 seconds to form a circular compact with a thickness of 5 mm for later use. Step 3: Place the pressed green sheet in an atmosphere furnace, introduce hydrogen with a dew point of -25°C, heat to 780°C at 10°C / min and keep warm for 2.5h, cool with the furnace to form a green sheet for standby use; Step 4: Turn the blank and arbitrarily select one side of the blank as the bonding surface (non-carving surface) to seal the surface. The processing tool material is cemented carbide, the spindle speed is 1200rpm, the feed speed is 50mm / min, and a chapter blank with a thickness of 4mm is formed for standby use; Step 5: Select the opposite side of the bonding surface as the seal blank engraving surface, and perform grinding and polishing on the engraved surface (grinding and polishing according to the steps in Example 1) to form a seal body with holes on the surface for standby use; Step six: Carve the seal body to form specific graphics and texts, which are "Zhejiang Metallurgical Research Institute and Happy Technology", and assemble it with a lightweight ink-returning seal shell to complete the copper seal production.
[0057] Comparative Example 2 Compared with Example 1, the compression ratio of the limited pressing in step 2 is 1.5, and the other process flows remain unchanged.
[0058] The preparation of the copper seal includes the following steps: Step 1: Sieve brass powder (melting point 950°C) to a particle size of 200-350 mesh for later use; Step 2: Weigh an appropriate amount of the powder processed in step 1 and place it in a circular mold. Use limited compression with a compression ratio of 1.5 and hold the pressure for 15 seconds to form a circular compact with a thickness of 5 mm for later use. Step 3: Place the pressed green sheet in an atmosphere furnace, introduce hydrogen with a dew point of -25°C, heat to 780°C at 10°C / min and keep warm for 2.5h, cool with the furnace to form a green sheet for standby use; Step 4: Turn the blank and arbitrarily select one side of the blank as the bonding surface (non-carving surface) to seal the surface. The processing tool material is cemented carbide, the spindle speed is 1200rpm, the feed speed is 50mm / min, and a chapter blank with a thickness of 4mm is formed for standby use; Step 5: Select the opposite side of the bonding surface as the seal blank engraving surface, and perform grinding and polishing on the engraved surface (grinding and polishing according to the steps in Example 1) to form a seal body with holes on the surface for standby use; Step six: Carve the seal body to form specific graphics and texts, which are "Zhejiang Metallurgical Research Institute and Happy Technology", and assemble it with a lightweight ink-returning seal shell to complete the copper seal production.
[0059] Comparative Example 3 Compared with Example 1, the dew point of the hydrogen introduced in step 3 is -10°C, the sintering temperature is 600°C, and the other process flows remain unchanged.
[0060] The preparation of the copper seal includes the following steps: Step 1: Sieve brass powder (melting point 950°C) to a particle size of 200-350 mesh for later use; Step 2: Weigh an appropriate amount of the powder processed in step 1 and place it in a circular mold. Use limited compression with a compression ratio of 2.1 and hold the pressure for 15 seconds to form a circular compact with a thickness of 5 mm for later use. Step 3: Place the pressed green sheet in an atmosphere furnace, introduce hydrogen with a dew point of -10°C, heat to 600°C at 10°C / min and keep warm for 2.5h, cool with the furnace to form a green sheet for standby use; Step 4: Turn the blank and arbitrarily select one side of the blank as the bonding surface (non-carving surface) to seal the surface. The processing tool material is cemented carbide, the spindle speed is 1200rpm, the feed speed is 50mm / min, and a chapter blank with a thickness of 4mm is formed for standby use; Step 5: Select the opposite side of the bonding surface as the seal blank engraving surface, and perform grinding and polishing on the engraved surface (grinding and polishing according to the steps in Example 1) to form a seal body with holes on the surface for standby use; Step six: Carve the seal body to form specific graphics and texts, which are "Zhejiang Metallurgical Research Institute and Happy Technology", and assemble it with a lightweight ink-returning seal shell to complete the copper seal production.
[0061] Comparative Example 4 Compared with Example 1, the dew point of the hydrogen introduced in step 3 is -25°C, the temperature is raised to 925°C at 5°C / min and kept for 1 hour, and the other process flows remain unchanged.
[0062] The preparation of the copper seal includes the following steps: Step 1: Sieve brass powder (melting point 950°C) to a particle size of 200-350 mesh for later use; Step 2: Weigh an appropriate amount of the powder processed in step 1 and place it in a circular mold. Use limited compression with a compression ratio of 2.1 and hold the pressure for 15 seconds to form a circular compact with a thickness of 5 mm for later use. Step 3: Place the pressed green sheet in an atmosphere furnace, introduce hydrogen with a dew point of -25°C, heat it to 925°C at 5°C / min and keep it at that temperature for 1h, cool it with the furnace to form a green sheet, and set it aside; Step 4: Turn the blank and arbitrarily select one side of the blank as the bonding surface (non-carving surface) to seal the surface. The processing tool material is cemented carbide, the spindle speed is 1200rpm, the feed speed is 50mm / min, and a chapter blank with a thickness of 4mm is formed for standby use; Step 5: Select the opposite side of the bonding surface as the seal blank engraving surface, and perform grinding and polishing on the engraved surface (grinding and polishing according to the steps in Example 1) to form a seal body with holes on the surface for use.
[0063] Step six: Carve the seal body to form specific graphics and texts, which are "Zhejiang Metallurgical Research Institute and Happy Technology", and assemble it with a lightweight ink-returning seal shell to complete the copper seal production.
[0064] Comparative Example 5 Compared with Example 1, in step 4, the blank is only shaped without sealing, and the other process flows remain unchanged.
[0065] The preparation of the copper seal includes the following steps: Step 1: Sieve brass powder (melting point 950°C) to a particle size of 200-350 mesh for later use; Step 2: Weigh an appropriate amount of the powder processed in step 1 and place it in a circular mold. Use limited compression with a compression ratio of 2.1 and hold the pressure for 15 seconds to form a circular compact with a thickness of 5 mm for later use. Step 3: Place the pressed green sheet in an atmosphere furnace, introduce hydrogen with a dew point of -25°C, heat to 780°C at 10°C / min and keep warm for 2.5h, cool with the furnace to form a green sheet for standby use; Step 4: Turn the blank to shape it, the machining tool material is cemented carbide, the spindle speed is 1200rpm, the feed speed is 50mm / min, and a chapter blank with a thickness of 4mm is formed for standby use; Step 5: Select the opposite side of the bonding surface as the seal blank engraving surface, and perform grinding and polishing on the engraved surface (grinding and polishing according to the steps in Example 1) to form a seal body with holes on the surface for standby use; Step six: Carve the seal body to form specific graphics and texts, which are "Zhejiang Metallurgical Research Institute and Happy Technology", and assemble it with a lightweight ink-returning seal shell to complete the copper seal production.
[0066] Comparative Example 6 Compared with Example 1, the sintering time in step 3 is 0.5 h, and the other process flows remain unchanged.
[0067] The preparation of the copper seal includes the following steps: Step 1: Sieve brass powder (melting point 950°C) to a particle size of 200-350 mesh for later use; Step 2: Weigh an appropriate amount of the powder processed in step 1 and place it in a circular mold. Use limited compression with a compression ratio of 2.1 and hold the pressure for 15 seconds to form a circular compact with a thickness of 5 mm for later use. Step 3: Place the pressed green sheet in an atmosphere furnace, introduce hydrogen with a dew point of -25°C, heat to 780°C at 10°C / min and keep warm for 0.5h, cool with the furnace to form a green sheet for standby use; Step 4: Turn the blank and arbitrarily select one side of the blank as the bonding surface (non-carving surface) to seal the surface. The processing tool material is cemented carbide, the spindle speed is 1200rpm, the feed speed is 50mm / min, and a chapter blank with a thickness of 4mm is formed for standby use; Step 5: Select the opposite side of the bonding surface as the seal blank engraving surface, and perform grinding and polishing on the engraved surface (grinding and polishing according to the steps in Example 1) to form a seal body with holes on the surface for standby use; Step six: Carve the seal body to form specific graphics and texts, which are "Zhejiang Metallurgical Research Institute and Happy Technology", and assemble it with a lightweight ink-returning seal shell to complete the copper seal production.
[0068] The seal bodies prepared in the above embodiments and comparative examples were tested for wettability to printing ink and stamping conditions, and the results are shown in Table 1.
[0069] Table 1 Note: 1. The specific graphics and texts engraved on the copper seal are "Zhejiang Metallurgical Research Institute and Happy Technology", where "Zhejiang Metallurgical Research Institute" is the abbreviation of the applicant's unit name, and "Happy Technology" means that scientific researchers are happy to engage in scientific and technological work; 2. The "traditional dense copper seal" is an ink-returning dense copper seal purchased by Changzhou Jintan Cultural Seal Material Co., Ltd.; 3. The liquid used in the wettability test of the seal surface is the same oily printing ink.
[0070] like Figure 1 The figure shows the macroscopic appearance of the copper seal body after engraving in the present invention, and the copper seal body obtained by the present invention and the traditional dense copper seal body of the same specification are compared. Figure 2 and Figure 3 The figures show the stamped texts of the copper seal body obtained by the present invention and the traditional dense copper seal body. It can be clearly seen that the stamped texts of the copper seal body of the present invention are clear, while the stamped texts of the traditional dense copper seal body are not clear. Figure 4 and Figure 5 The figures shown are respectively the wettability test graphs of the copper seal body obtained by the present invention and the traditional dense copper seal body to printing oil, Figure 5 The contact angle shown is significantly greater than Figure 4 The contact angles shown indicate that the copper seal surface of the present invention has better wettability to the printing ink. There are oily, water-based and neutral printing inks, and different printing inks have different wettability to the seal surface. The test results of the three types of printing inks are all better for the present invention. In addition, for the copper seal body of the present invention, the wettability effects on oily, water-based and neutral printing inks decrease in turn.
[0071] As shown in Table 1, the wettability of the ink and the stamping test data in Examples 1-5 are better than those of the traditional dense copper seal body. Comparative Examples 1-4 show that the particle size selection, pressing and sintering parameters in the process of preparing the powder material into the seal body will affect the pore structure and strength, and thus affect the wettability and stamping effect. Comparative Example 5 shows that the failure to perform the pore sealing treatment will affect the bonding surface adhesive, which is not conducive to the application of the seal body. Comparative Example 6 shortens the sintering and heat preservation time relative to Example 1. Figure 6 The SEM morphology of the spheroidized pores of the copper seal of Example 1 is shown. Figure 7 The figure shows the SEM morphology of irregular pores of the copper seal body of comparative example 6 of the present invention. The data in Table 1 also show that the stamping effect of comparative example 6 is poor, and the contact angle is significantly increased relative to that of embodiment 1. The results show that the sintering process parameters and hydrogen work together to obtain a better pore morphology, and thus a better stamping effect.
[0072] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the specification of the present invention, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a copper seal with high ink wettability, characterized in that: The steps include: Step 1: placing copper metal powder in a mold and pressing it to form a compact; Step 2: sintering the pressed green sheet in a hydrogen atmosphere to form a green sheet; Step 3: Machining and shaping the blank to form a chapter blank; Step 4: Choose one side of the seal blank as the bonding surface and perform sealing treatment; Step 5: Except for the bonding surface, select any side of the seal blank as the seal engraving surface, and perform grinding and polishing to form the seal body; Step 6: Carve the seal body to form images and texts, and assemble it with the seal shell to obtain a copper seal.
2. The method for preparing a copper stamp with high ink wettability according to claim 1, characterized in that: In step 1, the copper metal powder is made of one of red copper, bronze and brass, and the powder particle size is 100-400 meshes.
3. The method for preparing a copper stamp with high ink wettability according to claim 1, characterized in that: In step 1, the pressing method is position limiting pressing or constant pressure pressing.
4. The method for preparing a copper stamp with high ink wettability according to claim 3, characterized in that: The compression ratio of the limited pressing is 1.8-2.5, and the holding time is 1-60s; the pressure of the constant pressure pressing is 150-500 MPa, and the holding time is 1-60s; the shape of the pressed green body is round, oval or rectangular, and the thickness of the pressed green body is 2-15 mm.
5. The method for preparing a copper stamp with high ink wettability according to claim 1, characterized in that: In step 2, the sintering parameters are: the sintering temperature is 0.75-0.95 times the melting point of the copper metal powder, the holding time is 2.5-5 h, the heating rate is 10-15 °C / min; the dew point of the hydrogen is ≤-20 °C.
6. The method for preparing a copper stamp with high ink wettability according to any one of claims 1 to 5, characterized in that: In step three, the machining method is turning or milling; the thickness of the chapter blank is 70-90% of the thickness of the blank.
7. The method for preparing a copper stamp with high ink wettability according to any one of claims 1 to 5, characterized in that: In step 4, the sealing treatment is carried out by sealing with a sealing agent, sealing by turning or sealing by milling.
8. The method for preparing a copper seal with high ink wettability according to claim 7, characterized in that: The sealing agent used in the sealing of the holes is epoxy resin, polyurethane or silicone.
9. The method for preparing a copper seal with high ink wettability according to claim 7, characterized in that: The parameters of the turning and sealing hole are: spindle speed 700-1500 rpm, feed speed 25-100 mm / min.
10. The method for preparing a copper seal with high ink wettability according to claim 7, characterized in that: The parameters of the milling sealing are: spindle speed 2000-10000 rpm, feed speed 100-1000 mm / min.