Segment difference capillary, forming process thereof and vapor chamber
Through the profiling mold and metal powder sintering process, the problems of tedious operation and poor consistency of braided capillary are solved, stable installation of step capillary and efficient reflow effect are achieved, and the thermal conductivity performance of the vapor chamber is improved.
Patent Information
- Application Number
- CN202410943028.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-01
AI Technical Summary
The existing braided capillary is cumbersome to operate and has low efficiency when making step structures. Moreover, when combined with the vaporizing plate, the capillary structure has poor consistency, the reflow effect is unstable, and the scope of application is small.
The profiling mold and metal powder sintering process are used to control the sintering temperature and time to form a porous structure of step capillary to ensure the consistency of the shape, thickness and characteristics of the capillary. Different particle sizes and compounding of copper powder are used to design multi-level pores. structure to optimize the capillary reflow performance.
It realizes the convenient and stable installation of step capillary, improves the capillary reflow effect and heat conduction performance, expands the scope of application, and avoids the problem of reduced structural stability in the weaving process.
Smart Images

Figure CN118720135A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of step-difference capillaries, and in particular to a step-difference capillary and a molding process thereof, and a temperature balancing plate. Background Art
[0002] In the information age, AR, video shooting, live broadcasting, e-sports online games, 5G communications and other scenarios have increasingly higher requirements for the performance, user experience, device data transmission speed and processing power of electronic products, especially smartphones. Behind the smoothness of mobile phone operation and the comfort of use, there is a war about the heating and heat dissipation of electronic products. At present, the main heat dissipation methods for smartphones include graphene, heat pipes and VC heat sinks.
[0003] The interior of the VC heat spreader has a vacuum cavity with a microstructure. Its working principle is similar to that of a heat pipe, and both include four steps: conduction, evaporation, convection, and solidification. In different application scenarios, the thickness of each area of the heat spreader is different. Therefore, in order to meet its performance requirements, a capillary with a step difference is required to increase the liquid return capacity of the product in order to achieve a stable phase change cycle. At present, the common capillaries are mainly woven structures, such as copper wire weaving. When some special-shaped capillaries with step differences are needed, the step difference capillaries are generally obtained by removing one or more layers of the woven structure on the copper wire woven capillary, which is cumbersome and inefficient. In addition, when it is combined with the heat spreader shell, the consistency of the capillary structure is poor and the reflux effect is unstable. If the traditional capillary is not laid in a straight line on the heat spreader, a larger R angle is required for transition to avoid the capillary from being bent and affecting the reflux effect, but it has a greater impact on the design of the heat spreader support structure and has a small scope of application. Summary of the invention
[0004] The purpose of the present invention is to provide a step-difference capillary and its forming process, so as to solve the problems that the operation of making the step-difference structure of the existing braided capillary according to different needs is cumbersome and the design of the temperature equalizing plate support structure is greatly affected when the shape is an irregular structure and the application range is small.
[0005] The present invention also aims to provide a temperature equalizing plate, in which the step-difference capillary can be installed conveniently and stably in the housing.
[0006] The embodiments of the present invention are implemented by the following technical solutions:
[0007] A step-difference capillary forming process, characterized by comprising:
[0008] S100, making a contour mold according to a preset capillary structure shape;
[0009] S200, adding metal powder into the profiling mold, and forming the metal powder by sintering to obtain a step-difference capillary, wherein the step-difference capillary is a porous structure, the sintering temperature is 800-1000° C., and the sintering time is 2-4 hours.
[0010] The function and working principle of the temperature plate are consistent with those of the heat pipe. The evaporation and condensation cycle of the actuating fluid enclosed in the plate-shaped cavity makes it have the characteristics of rapid temperature uniformity, thus having the functions of rapid heat conduction and heat diffusion. The temperature plate is made of a metal shell, a capillary structure and an actuating fluid through annealing, vacuuming and sealing welding.
[0011] The temperature equalizer has different thicknesses in different areas of the board in different application scenarios. Therefore, in order to meet its performance requirements, capillaries with step differences are needed to increase the liquid return capacity of the product in order to achieve a stable phase change cycle. Currently, common capillaries are mainly woven structures, such as those formed by copper wire weaving. When some special-shaped capillaries with step differences are needed, the step-difference capillaries are generally obtained by removing one or more layers of woven structures on the copper wire woven capillaries. The operation is cumbersome and inefficient. In addition, when it is combined with the temperature equalizer shell, the consistency of the capillary structure is poor and the reflux effect is unstable. If the traditional capillary is not laid in a straight line on the temperature equalizer, a larger R angle is required for transition to avoid the capillary from bending and affecting the reflux effect. However, it has a greater impact on the design of the temperature equalizer support structure and has a small scope of application.
[0012] The present invention provides a new capillary structure and forming process, in which step-difference capillaries are formed by sintering metal powders. The sintering conditions are limited so that the step-difference capillaries can achieve the best capillary reflux effect. The shape, thickness and step-difference characteristics of the step-difference capillaries are controlled by means of a contoured mold. Even if the capillaries are of a special shape, multiple thicknesses or multiple steps, their shapes have good stability. By limiting the sintering conditions, the metal powder will not melt completely. After the powder surface is slightly melted during the sintering process, adjacent powders are diffused and overlapped by molten metal to form pores. Therefore, in this case, the sintering temperature and sintering time are particularly important for the formation of pores and the control of the porosity size. The pore structure of the step-difference capillaries is crucial to the reflux performance of the capillaries. Therefore, during the process, it is necessary to pay attention to the sintering conditions within the numerical range of this case.
[0013] Preferably, the metal powder is copper powder, and the mesh size of the copper powder is 60-180 meshes.
[0014] The material and particle size of the metal powder particles will affect the structure and performance of the step-difference capillary after sintering. The particle size of the copper powder can be selected according to the performance requirements of each segment of the capillary. Under the sintering conditions of this case, the step-difference capillary formed by sintering coarse powder particles has the characteristics of large pores and high permeability, while the step-difference capillary formed by sintering fine powder particles has the characteristics of small pores and strong capillary ability. Copper has the advantages of good thermal conductivity, corrosion resistance and low cost.
[0015] For example, the capillary used in the condensing section of the heat spreader adopts a coarse powder design to reduce the reflux resistance, and the capillary used in the evaporating section of the heat spreader adopts a fine powder design to increase the capillary force and avoid burning out. In view of the high heat at the SOC, copper powders of different particle sizes can be compounded to obtain capillaries with special pore structures, which are easier to nucleate bubbles and accelerate the efficiency of heat removal.
[0016] Preferably, the copper powder used for the capillary of the evaporation section of the temperature equalizing plate includes: 15-35 parts of 80-mesh copper powder and 40-70 parts of 140-mesh copper powder; first add the 140-mesh copper powder into the profiling mold, and then add the 80-mesh copper powder, and obtain a step-difference capillary with a multi-level pore structure through sintering, the large pore end in the multi-level pore structure serves as the heat source end, and the small pore end in the multi-level pore structure serves as the steam outlet end.
[0017] If large-particle copper powder is added first and then small-particle copper powder is added, the small-particle copper powder may enter the gaps between the large-particle copper powders, and the pore structure is difficult to control. The multi-level pore structure has better diffusion and heat transfer properties. At the same time, the multi-level pore structure also has higher structural stability and can resist external stress and environmental changes. In this case, the large pore end with a suitable pore size can be used as the heat source end to increase the convection of the heat exchange medium and promote the evaporation of the liquid working fluid, while the small pore end can be used as the outlet end to avoid dry burning.
[0018] Preferably, the manufacturing process of the capillary for the evaporation section of the temperature equalizer includes: first adding a mixed powder of 15-35 parts of 80 mesh copper powder and 40-70 parts of 140 mesh copper powder into a contoured mold, and then adding 15-35 parts of 80 mesh copper powder, and obtaining a step-difference capillary with a multi-level pore structure by sintering.
[0019] Since the capillary also serves as a channel for the liquid to reflux at the condensation end, in order to reduce the resistance of fine powder to liquid reflux, this case uses a mixture of coarse and fine powders to reduce the reflux resistance while meeting the heat transfer requirements at the large hole end. In addition, due to the large surface energy of fine metal powder, a sintering neck will form at the contact point of the metal particles under certain pressure and temperature, reducing the system surface energy of the powder. The atoms undergo viscous flow in the neck, the radius of curvature at the sintering neck becomes larger, and the center distance between the two particles decreases under the action of surface tension. The sintered structure will shrink on a macro scale. Instead of directly using fine powder, a coarse and fine mixture is used to avoid structural defects and even cracks caused by different shrinkage rates in different parts during the step-difference capillary sintering process.
[0020] Preferably, during sintering, the temperature is firstly 900-1000° C. for 1-1.5 h, and then 800-850° C. for 1-2.5 h.
[0021] In order to promote the bonding of particles at contact and avoid the transitional shrinkage or even closure of pores, a two-stage sintering method is adopted. The first sintering promotes the connection of connected particles, and the second sintering temperature is lower, which can reduce the plastic flow of particles and mainly rely on viscous flow. It can also reduce the proximity of particles after connection, thereby avoiding excessive shrinkage of the embryo.
[0022] Preferably, during the process of adding the metal powder into the profiling die, the profiling die is shaken horizontally.
[0023] The shaking of the contoured mold can make the powder more compact and the powder layer more smooth.
[0024] Preferably, the profiling die is made of graphite. At the same time, since the step difference capillaries will shrink during the sintering process, the profiling die structure can also be modified according to the shrinkage rate.
[0025] Graphite material can effectively prevent copper powder from connecting with the contoured mold through atomic diffusion at high temperature, ensuring demoulding performance.
[0026] A step-difference capillary is produced by the step-difference capillary molding process.
[0027] A temperature equalizing plate comprises: a lower shell, an upper shell and a step-difference capillary; the upper shell is covered and connected with the lower shell, and the step-difference capillary is located between the upper shell and the lower shell.
[0028] Preferably, after the step-difference capillary is sintered in the profiling mold, the lower shell is covered on the surface of the step-difference capillary, and then the lower shell is connected to the step-difference capillary by sintering. The temperature plate shell is made of stainless steel, aluminum alloy, titanium alloy and other materials, and has good bonding performance with the copper step-difference capillary by sintering.
[0029] The present invention has at least the following beneficial effects:
[0030] The step-difference capillary forming process provided by the present invention improves the existing weaving forming process into a sintering forming process. Due to the use of a contoured mold, the process can be applicable to shapes and specifications of different step-difference capillaries, eliminating the operation of weaving the capillary for morphological changes and forming a step-difference structure, and also avoiding the reduction of structural stability after the braided capillary is deformed; reasonable sintering temperature and sintering time enable the step-difference capillary to form a porous structure, and the step-difference capillary has high consistency and stable capillary capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0032] Figure 1 This is an electron microscope image of the step-difference capillary;
[0033] Figure 2 Schematic diagram of the mechanism of the temperature equalizing plate;
[0034] Figure 3 It is a schematic diagram of the sintering of the step difference capillary and the lower shell;
[0035] Figure numerals: 11 - lower shell, 12 - profiling mold, 2 - step difference capillary, 3 - support column, 4 - heat source surface, 5 - heat dissipation surface. DETAILED DESCRIPTION
[0036] In order to make the purpose, method scheme and advantages of the embodiments of the present invention clearer, the method scheme in the embodiments of the present invention is clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0037] In order to facilitate understanding, this case first briefly explains the mechanism of the temperature equalization plate, such as Figure 2 As shown in the figure, the heat from the heat source is transferred to the liquid working medium in the shell through the heat source surface of the temperature equalizer. After absorbing heat, the liquid working medium evaporates and reaches the heat dissipation surface of the temperature equalizer. After releasing heat at the condensation end, it condenses into water and returns to the heat source end through capillaries. In this way, the heat can be continuously brought from the heat source to the condensation end. Therefore, in the treatment of the short-difference capillary structure, this case needs to pay attention to the pore structure to reduce its impact on the reflux performance and capillary capacity to avoid dry burning at the evaporation end.
[0038] Example 1
[0039] A step-difference capillary forming process includes: S100, making a profiling mold according to a preset capillary structure shape; S200, adding 60-mesh copper powder into the profiling mold, and sintering the copper powder to obtain a step-difference capillary; the sintering temperature is 800° C., and the sintering time is 2 hours. In the process of adding metal powder into the profiling mold, the profiling mold is shaken horizontally, and the profiling mold is made of graphite.
[0040] Example 2
[0041] A step-difference capillary forming process includes: S100, making a profiling mold according to a preset capillary structure shape; S200, adding 180-mesh copper powder into the profiling mold, and sintering the copper powder to obtain a step-difference capillary; the sintering temperature is 1000° C., and the sintering time is 4 hours. In the process of adding metal powder into the profiling mold, the profiling mold is shaken horizontally, and the profiling mold is made of graphite.
[0042] Example 3
[0043] A step-difference capillary forming process includes: S100, making a profiling mold according to a preset capillary structure shape; S200, adding 120-mesh copper powder into the profiling mold, and sintering the copper powder to obtain a step-difference capillary; the sintering temperature is 900° C., and the sintering time is 3 hours. In the process of adding metal powder into the profiling mold, the profiling mold is shaken horizontally, and the profiling mold is made of graphite.
[0044] Example 4
[0045] A step-difference capillary forming process comprises: S100, making a profiling mold according to a preset capillary structure shape; S200, adding 60-mesh copper powder into the profiling mold, and forming the copper powder by sintering to obtain the step-difference capillary; the sintering temperature is 800° C., and the sintering time is 2 hours;
[0046] The copper powder used for the capillary of the evaporation section of the temperature uniform plate includes: 15 parts of 80-mesh copper powder and 40 parts of 140-mesh copper powder; the 140-mesh copper powder is first added to the profiling mold, and then the 80-mesh copper powder is added, and a step-difference capillary with a multi-level pore structure is obtained by sintering, the large hole end in the multi-level pore structure is used as the heat source end, and the small hole end in the multi-level pore structure is used as the steam outlet end.
[0047] During the process of adding metal powder into the profiling die, the profiling die is shaken horizontally. The profiling die is made of graphite.
[0048] Example 5
[0049] A step-difference capillary forming process comprises: S100, making a profiling mold according to a preset capillary structure shape; S200, adding 60-mesh copper powder into the profiling mold, and forming the copper powder by sintering to obtain the step-difference capillary; the sintering temperature is 800° C., and the sintering time is 2 hours.
[0050] The copper powder used for the capillary of the evaporation section of the temperature uniform plate includes: 35 parts of 80-mesh copper powder and 70 parts of 140-mesh copper powder; the 140-mesh copper powder is first added to the profiling mold, and then the 80-mesh copper powder is added, and a step-difference capillary with a multi-level pore structure is obtained by sintering, the large hole end in the multi-level pore structure is used as the heat source end, and the small hole end in the multi-level pore structure is used as the steam outlet end.
[0051] During the process of adding metal powder into the profiling die, the profiling die is shaken horizontally. The profiling die is made of graphite.
[0052] Example 6
[0053] A step-difference capillary forming process comprises: S100, making a profiling mold according to a preset capillary structure shape; S200, adding 60-mesh copper powder into the profiling mold, and forming the copper powder by sintering to obtain the step-difference capillary; the sintering temperature is 800° C., and the sintering time is 2 hours.
[0054] The copper powder used for the capillary of the evaporation section of the temperature equalizing plate includes: 20 parts of 80-mesh copper powder and 55 parts of 140-mesh copper powder; the 140-mesh copper powder is first added to the profiling mold, and then the 80-mesh copper powder is added, and a step-difference capillary with a multi-level pore structure is obtained by sintering, the large hole end in the multi-level pore structure is used as the heat source end, and the small hole end in the multi-level pore structure is used as the steam outlet end.
[0055] During the process of adding metal powder into the profiling die, the profiling die is shaken horizontally. The profiling die is made of graphite.
[0056] Example 7
[0057] A step-difference capillary forming process comprises: S100, making a profiling mold according to a preset capillary structure shape; S200, adding 60-mesh copper powder into the profiling mold, and forming the copper powder by sintering to obtain the step-difference capillary; the sintering temperature is 800° C., and the sintering time is 2 hours;
[0058] The manufacturing process of the capillary used in the evaporation section of the temperature equalizing plate includes: first adding a mixed powder of 15 parts of 80-mesh copper powder and 40 parts of 140-mesh copper powder into a contoured mold, and then adding 15 parts of 80-mesh copper powder, and sintering to obtain a step-difference capillary with a multi-level pore structure, wherein the large pore end in the multi-level pore structure serves as a heat source end, and the small pore end in the multi-level pore structure serves as a steam outlet end.
[0059] During the process of adding metal powder into the profiling die, the profiling die is shaken horizontally. The profiling die is made of graphite.
[0060] Example 8
[0061] A step-difference capillary forming process comprises: S100, making a profiling mold according to a preset capillary structure shape; S200, adding 60-mesh copper powder into the profiling mold, and forming the copper powder by sintering to obtain the step-difference capillary; the sintering temperature is 800° C., and the sintering time is 2 hours;
[0062] The manufacturing process of the capillary for the evaporation section of the temperature equalizing plate includes: first adding a mixed powder of 35 parts of 80-mesh copper powder and 70 parts of 140-mesh copper powder into a contoured mold, and then adding 35 parts of 80-mesh copper powder, and sintering to obtain a step-difference capillary with a multi-level pore structure, wherein the large pore end in the multi-level pore structure serves as a heat source end, and the small pore end in the multi-level pore structure serves as a steam outlet end.
[0063] During the process of adding metal powder into the profiling die, the profiling die is shaken horizontally. The profiling die is made of graphite.
[0064] Example 9
[0065] A step-difference capillary forming process comprises: S100, making a profiling mold according to a preset capillary structure shape; S200, adding 60-mesh copper powder into the profiling mold, and forming the copper powder by sintering to obtain the step-difference capillary; the sintering temperature is 800° C., and the sintering time is 2 hours;
[0066] The manufacturing process of the capillary for the evaporation section of the temperature equalizing plate includes: first adding a mixed powder of 25 parts of 80-mesh copper powder and 50 parts of 140-mesh copper powder into a contoured mold, and then adding 25 parts of 80-mesh copper powder, and sintering to obtain a step-difference capillary with a multi-level pore structure, wherein the large pore end in the multi-level pore structure serves as a heat source end, and the small pore end in the multi-level pore structure serves as a steam outlet end.
[0067] During the process of adding metal powder into the profiling die, the profiling die is shaken horizontally. The profiling die is made of graphite.
[0068] Example 10
[0069] A step-difference capillary forming process comprises: S100, making a profiling mold according to a preset capillary structure shape; S200, adding 60-mesh copper powder into the profiling mold, and forming the copper powder by sintering to obtain the step-difference capillary; during sintering, first sintering at a temperature of 900° C. for 1 hour, and then sintering at a temperature of 800° C. for 1 hour.
[0070] The manufacturing process of the capillary used in the evaporation section of the temperature equalizing plate includes: first adding a mixed powder of 15 parts of 80-mesh copper powder and 40 parts of 140-mesh copper powder into a contoured mold, and then adding 15 parts of 80-mesh copper powder, and sintering to obtain a step-difference capillary with a multi-level pore structure, wherein the large pore end in the multi-level pore structure serves as a heat source end, and the small pore end in the multi-level pore structure serves as a steam outlet end.
[0071] During the process of adding metal powder into the profiling die, the profiling die is shaken horizontally. The profiling die is made of graphite.
[0072] Embodiment 11
[0073] A step-difference capillary forming process comprises: S100, making a profiling mold according to a preset capillary structure shape; S200, adding 60-mesh copper powder into the profiling mold, and forming the copper powder by sintering to obtain the step-difference capillary; during sintering, first sintering at a temperature of 1000° C. for 1.5 hours, and then sintering at a temperature of 850° C. for 2.5 hours.
[0074] The manufacturing process of the capillary used in the evaporation section of the temperature equalizing plate includes: first adding a mixed powder of 15 parts of 80-mesh copper powder and 40 parts of 140-mesh copper powder into a contoured mold, and then adding 15 parts of 80-mesh copper powder, and sintering to obtain a step-difference capillary with a multi-level pore structure, wherein the large pore end in the multi-level pore structure serves as a heat source end, and the small pore end in the multi-level pore structure serves as a steam outlet end.
[0075] During the process of adding metal powder into the profiling die, the profiling die is shaken horizontally. The profiling die is made of graphite.
[0076] Example 12
[0077] A step-difference capillary forming process comprises: S100, making a profiling mold according to a preset capillary structure shape; S200, adding 60-mesh copper powder into the profiling mold, and forming the copper powder by sintering to obtain the step-difference capillary; during sintering, first sintering at a temperature of 950° C. for 1.2 hours, and then sintering at a temperature of 830° C. for 1.8 hours.
[0078] The manufacturing process of the capillary used in the evaporation section of the temperature equalizing plate includes: first adding a mixed powder of 15 parts of 80-mesh copper powder and 40 parts of 140-mesh copper powder into a contoured mold, and then adding 15 parts of 80-mesh copper powder, and sintering to obtain a step-difference capillary with a multi-level pore structure, wherein the large pore end in the multi-level pore structure serves as a heat source end, and the small pore end in the multi-level pore structure serves as a steam outlet end.
[0079] During the process of adding metal powder into the profiling die, the profiling die is shaken horizontally. The profiling die is made of graphite.
[0080] test
[0081] The wettability test of the step-difference capillary obtained by the step-difference capillary molding process provided in Examples 1-12 is performed as follows:
[0082] One end of the step capillary is placed in water with a depth of 2.5 cm. The step capillary is kept tilted at 70°. The time required for water to climb from the bottom of the step capillary to the top of the step capillary is recorded. Five step capillaries are selected for each embodiment. The test result is the average of the time measured by the five step capillaries. The test results are shown in Table 1:
[0083] Table 1
[0084] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Time(s) 38.78 38.91 38.66 36.97 38.49 38.30 Example 7 Example 8 Example 9 Example 10 Embodiment 11 Example 12 Time(s) 33.68 33.42 33.57 31.29 31.23 31.17
[0085] It can be seen from Table 2 that the step-difference capillary produced by the molding process provided by the present invention has good wetting performance.
[0086] From the comparison between Example 4 and Example 1, it can be seen that after the capillary of the evaporation section of the temperature equalizer adopts a multi-level hole structure, the wetting performance of the step-difference capillary is effectively improved.
[0087] From the comparison between Example 7 and Example 4, it can be seen that after the mixed powder is used to make the evaporation section capillary of the temperature equalizing plate, the wetting performance of the step difference capillary is effectively improved.
[0088] From the comparison between Example 10 and Example 7, it can be seen that the multi-stage sintering method can provide the wetting performance of the capillary structure.
[0089] Embodiment 13
[0090] This embodiment provides a temperature equalizing plate structure using the step-difference capillary structure provided by the present invention.
[0091] like Figure 3 As shown, a temperature equalizing plate comprises a lower shell 11, an upper shell and the step capillary 2; the upper shell is covered and connected with the lower shell 11, and the step capillary is located between the upper shell and the lower shell 11. After the step capillary 2 is sintered in the profiling mold 12, the lower shell 11 is covered on the surface of the step capillary 2, and then the lower shell 11 is connected with the step capillary 2 by sintering.
[0092] In the specific implementation process, after the step-difference capillary 2 is sintered in the profiling mold 12, the step-difference capillary 2 is not taken out first, and the lower shell 11 is directly covered on the step-difference capillary 2, and sintered again. The sintering temperature can be 900°C. After the step-difference capillary 2 is connected to the lower shell 11 by sintering, the lower shell 11 can be taken out of the profiling mold together with the step-difference capillary 2, and then the upper shell and the lower shell 11 are covered and sealed, which can be sealed by welding. After sealing, the interior of the temperature-averaging plate is evacuated through the filling pipe reserved on the shell, and deionized water is filled, and then the filling pipe is cut off and sealed to obtain a finished temperature-averaging plate.
[0093] test
[0094] The step-difference capillary obtained by the step-difference capillary molding process provided in Examples 1-12 was used to make a temperature averaging plate according to Example 13 and the temperature difference test was performed on the temperature averaging plate. The temperature difference refers to the difference between the temperature at the heat source position of the temperature averaging plate and the temperature above the temperature averaging plate. When the temperature averaging plate was measured at 5 positions (center and four corners), the average of the temperature difference at each position was calculated. The test results are shown in Table 2:
[0095] Table 2
[0096] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Temperature difference (℃) 3.7 3.9 3.5 2.0 2.6 2.5 Example 7 Example 8 Example 9 Example 10 Embodiment 11 Example 12 Temperature difference (℃) 1.4 1.2 1.3 1.1 1.1 0.9
[0097] It can be seen from Table 2 that after the step-difference capillary produced by the molding process provided by the present invention is applied to the temperature averaging board, the temperature averaging board has good heat conduction and heat dissipation effects.
[0098] From the comparison between Example 4 and Example 1, it can be seen that after the capillary of the evaporation section of the temperature homogenizing plate adopts a multi-level hole structure, the heat conduction and heat dissipation effects are effectively improved.
[0099] From the comparison between Example 7 and Example 4, it can be seen that the capillary, heat conduction and heat dissipation effects of the evaporation section of the temperature equalizing plate made by using the mixed powder are effectively improved.
[0100] From the comparison between Example 10 and Example 7, it can be seen that the multi-stage sintering method can provide the capillary structure with thermal conductivity and heat dissipation performance.
[0101] from Figure 1 It can be seen that the step-difference capillary provided by the present invention has a good pore structure.
[0102] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A step-difference capillary forming process, characterized in that: include: S100, making a contour mold according to a preset capillary structure shape; S200, adding metal powder into the profiling mold, and forming the metal powder by sintering to obtain step-difference capillaries; the sintering temperature is 800-1000° C., and the sintering time is 2-4 hours.
2. The step-difference capillary forming process according to claim 1, characterized in that: The metal powder is copper powder, and the mesh size of the copper powder is 60-180 meshes.
3. The step-difference capillary forming process according to claim 2, characterized in that: The copper powder used for the capillary of the evaporation section of the temperature equalizing plate includes: 15-35 parts of 80-mesh copper powder and 40-70 parts of 140-mesh copper powder; the 140-mesh copper powder is first added to the profiling mold, and then the 80-mesh copper powder is added, and a step-difference capillary with a multi-level pore structure is obtained by sintering, the large hole end in the multi-level pore structure is used as the heat source end, and the small hole end in the multi-level pore structure is used as the steam outlet end.
4. The step-difference capillary forming process according to claim 2, characterized in that: The manufacturing process of the capillary for the evaporation section of the temperature uniform plate includes: first adding a mixed powder of 15-35 parts of 80-mesh copper powder and 40-70 parts of 140-mesh copper powder into a contoured mold, and then adding 15-35 parts of 80-mesh copper powder, and sintering to obtain a step-difference capillary with a multi-level pore structure.
5. The step-difference capillary forming process according to any one of claims 1 to 4, characterized in that: During sintering, firstly sinter at a temperature of 900-1000° C. for 1-1.5 hours, and then sinter at a temperature of 800-850° C. for 1-2.5 hours.
6. The step-difference capillary forming process according to claim 5, characterized in that: During the process of adding metal powder into the profiling die, the profiling die is shaken horizontally.
7. The step-difference capillary forming process according to claim 5, characterized in that: The profiling die is made of graphite.
8. A step-difference capillary obtained by the molding process of the step-difference capillary according to any one of claims 1 to 7.
9. A temperature equalizing plate, characterized in that: include: Lower housing; An upper shell, the upper shell is connected to the lower shell in a cover-shaped manner; The step-difference capillary according to claim 8 is located between the upper shell and the lower shell.
10. The temperature homogenizing plate according to claim 9, characterized in that: After the step-difference capillary is sintered in the profiling mold, the lower shell is covered on the surface of the step-difference capillary, and then the lower shell is connected to the step-difference capillary by sintering.