Synthesis process of high-toughness CBN (cubic boron nitride) blade
By adding strong and heat-resistant materials to the CBN blade, and using high-temperature and high-pressure sintering and coating technology, the impact, heat resistance and oxidation problems of the CBN blade are solved, its toughness and heat resistance are improved, and the service life is extended. .
Patent Information
- Application Number
- CN202410773764.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-16
- Publication Date
- 2024-10-01
AI Technical Summary
CBN blades are prone to chipping or breaking under severe impact or extreme conditions, and when processing certain materials, high temperatures lead to insufficient heat resistance and chemical stability, and the surface is prone to oxidation and discoloration, which affects its service life.
By adding strong materials such as carbon, chromium, cobalt and ceramics to CBN micro-powder materials and binders, and adding heat-resistant materials such as zirconium, vanadium and molybdenum, through high-temperature and high-pressure sintering and coating spray technology to form wear-resistant and corrosion-resistant materials. , heat-resistant carbide substrate, and spray titanium nitride, chromium nitride and aluminum oxide coatings on the surface to improve oxidation resistance.
Significantly improves the toughness, heat resistance and oxidation resistance of CBN blades, avoids edge chipping or breakage, extends service life, and maintains high hardness and chemical stability.
Smart Images

Figure CN118720140A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of blade synthesis, and in particular to a synthesis process of a high-toughness CBN blade. Background Art
[0002] CBN tools are artificial cubic boron nitride tools that can maintain high hardness at high temperatures and are mainly used for processing iron parts. Cubic boron nitride CBN was first synthesized by General Electric Company of the United States in the 1950s using artificial methods under high temperature and high pressure conditions. Its hardness is second only to diamond and far higher than other materials. Therefore, it and diamond are collectively referred to as superhard materials. The synthesis process of CBN blades mainly involves compounding CBN micropowder with a binder and a cemented carbide matrix under high temperature and high pressure.
[0003] Patent No. CN111644627B discloses a synthesis process of a quenched steel polycrystalline blade, including raw materials for preparing the quenched steel polycrystalline blade, wherein the raw materials for preparing the quenched steel polycrystalline blade are composed of CBN micropowder and a binder. The synthesis process of the quenched steel polycrystalline blade adopts fine-grained CBN micropowder and a binder having both metal and ceramic composites, which improves the wettability of the binder and the CBN particles, promotes the formation of a dense bond between the CBN particles and maintains a uniform microstructure, improves the impact resistance and wear resistance of the polycrystalline blade, and thus greatly improves the service life of the polycrystalline blade.
[0004] After searching the above patents, it was found that the synthesis process of CBN blades has the following deficiencies: 1. Although the hardness of CBN material is very high, its toughness is not as good as that of some other cemented carbides, which may cause the blade to easily collapse or break under severe impact or extreme conditions; 2. Although CBN blades have good high-temperature stability, when processing some specific materials, such as hardened ferrous metals and super alloys, extremely high temperatures may be generated, which puts higher requirements on the heat resistance and chemical stability of the tool; 3. Since CBN blades need to maintain high hardness when in use, and after long-term use, the blade surface is prone to oxidation and discoloration, which affects the service life of the CBN blade.
[0005] Therefore, a synthesis process of a strong and tough CBN blade is proposed to solve the above problems. Summary of the invention
[0006] The main purpose of the present invention is to provide a synthesis process of a strong and tough CBN blade which has strong toughness, strong heat resistance and prevents surface oxidation and discoloration, and is applied to the synthesis process preparation of the CBN blade.
[0007] To achieve the above object, the technical solution adopted by the present invention is: a synthesis process of a strong and tough CBN blade, comprising the following steps:
[0008] Step 1: Prepare base material, CBN (cubic boron nitride) powder material and corresponding weight ratio binder;
[0009] Step 2: Prepare a mixed base material, mix the CBN (cubic boron nitride) powder material and the binder with a corresponding weight ratio, add a tough material, pour in a reinforcing material with a corresponding weight ratio, stir evenly, and obtain a mixed base material;
[0010] Step 3: prepare a base material mixture, pour the heat-resistant material with a corresponding weight ratio into the mixed base material, add the heat-resistant composite material, stir evenly, and obtain a base material mixture;
[0011] Step 4: Prepare the tool body, put the mixed base material mixture into a molybdenum cup, add a salt carbon tube shielding layer for isolation, and then perform heat treatment under ultra-high temperature and high pressure conditions to tightly combine the CBN micropowder with the cemented carbide matrix to obtain the tool body;
[0012] Step 5: Cooling and cutting. After the tool blank is cooled, it is cut and polished into a CBN blade of corresponding shape, and a coating spray is sprayed on the surface of the CBN blade to complete the synthesis process of the CBN blade.
[0013] The total weight ratio of the CBN (cubic boron nitride) powder material and the binder to the grinding ball weight in step 1 is 2:7.
[0014] The strong and tough material in step 2 includes one or more of carbon (C), chromium (Cr), cobalt (Co) and ceramic materials, and the weight ratio of the strong and tough material is 10%-30% of the total mass;
[0015] The ceramic material is made of silicon nitride (Si3N4) or aluminum oxide (Al2O3).
[0016] The reinforcing material in step 2 includes one or both of tungsten carbide and nickel, and the weight ratio of the reinforcing material is 2%-10% of the total mass.
[0017] The heat-resistant material in step three includes one or more of zirconium, vanadium and molybdenum, and the weight ratio of the heat-resistant material is 2%-15% of the total mass.
[0018] The heat-resistant composite material in step three comprises zirconium oxide, titanium, hafnium and rhenium, and the weight ratio of the heat-resistant composite material is 2%-15% of the total mass.
[0019] The coating spray in step five includes one or more of titanium nitride coating (TiN), chromium nitride coating (CrN) and aluminum oxide (Al2O3).
[0020] The titanium nitride coating (TiN), chromium nitride coating (CrN) and aluminum oxide (Al2O3) in the coating spray are coated on the surface of the CBN insert of corresponding shape by physical vapor deposition (PVD) and chemical vapor deposition (CVD).
[0021] The heat treatment in step 4 is high temperature and high pressure sintering, which is used to vacuum dry the cemented carbide substrate at 200-400°C for 20-30 minutes, and then place the cemented carbide substrate in a six-sided top press for high temperature and high pressure sintering, with a temperature of 1200-1500°C and a pressure of 5-8GPA.
[0022] The hardness of the CBN blade made in step 5 is 48 GPa.
[0023] The present invention has the following beneficial effects:
[0024] 1. In the present invention, a strong and tough material is added after mixing a CBN (cubic boron nitride) powder material and a binder. The strong and tough material includes carbon (C), chromium (Cr), cobalt (Co) and a ceramic material. A reinforcing material is added to enhance the toughness after combining with the strong and tough material. The reinforcing material includes tungsten carbide and nickel. Since chromium combines with carbon to form chromium carbide, the tensile strength, hardness and heat resistance of the blade can be improved. Tungsten carbide or nickel and cobalt are combined to form a cemented carbide with extremely high hardness and excellent toughness. This material is not only wear-resistant, but also corrosion-resistant, and has high thermal stability and chemical stability, so that the prepared CBN blade can avoid edge collapse or breakage under severe impact or extreme conditions.
[0025] 2. In the present invention, by adding heat-resistant materials and heat-resistant composite materials, the heat-resistant materials include zirconium, vanadium and molybdenum, and the heat-resistant composite materials include zirconium oxide, titanium, hafnium and rhenium. Zirconium is combined with zirconium oxide, so that the heat resistance of the prepared CBN blade is enhanced. At the same time, vanadium is combined with titanium, and molybdenum is combined with hafnium and rhenium, so that the heat resistance of the prepared CBN blade is enhanced, ensuring that the CBN blade has good heat resistance and high temperature stability.
[0026] 3. In the present invention, a coating spray is sprayed on the surface of the formed CBN blade, and the coating spray includes a titanium nitride coating (TiN), a chromium nitride coating (CrN) and an aluminum oxide (Al2O3). The titanium nitride coating (TiN), the chromium nitride coating (CrN) and the aluminum oxide (Al2O3) are coated on the surface of the CBN blade of corresponding shape by physical vapor deposition (PVD) and chemical vapor deposition (CVD). When the chromium content exceeds 12%, the CBN blade can have good high-temperature oxidation resistance and resistance to corrosion by oxidizing media, so that the CBN blade can not only stably maintain high hardness, but also avoid oxidation discoloration on the surface of the CBN blade after long-term use, thereby extending the service life of the CBN blade. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The figure is a schematic diagram of the overall process of the synthesis process of a high-toughness CBN blade of the present invention. DETAILED DESCRIPTION
[0028] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.
[0029] Comparative Example
[0030] A synthesis process of a strong and tough CBN blade, the synthesis process of the strong and tough CBN blade comprising the following steps:
[0031] Step 1: Prepare base material, CBN (cubic boron nitride) powder material and corresponding weight ratio binder;
[0032] Step 2: Prepare a mixed base material, mix the CBN (cubic boron nitride) powder material and the binder with a corresponding weight ratio, stir evenly, and prepare a mixed base material;
[0033] Step 3: Prepare the tool embryo, put the mixed base material mixture into a molybdenum cup, add a salt carbon tube shielding layer for isolation, and then perform heat treatment under ultra-high temperature and high pressure conditions to tightly combine the CBN micropowder with the cemented carbide matrix to obtain the tool embryo;
[0034] Step 4: Cooling and cutting. After the tool blank is cooled, it is cut and polished into a CBN blade of corresponding shape to complete the synthesis process of the CBN blade.
[0035] Comparison 1:
[0036] S1: prepare CBN (cubic boron nitride) powder material and corresponding weight ratio binder, the total weight ratio of CBN (cubic boron nitride) powder material and binder to the weight of grinding ball is 2:7;
[0037] S2: Mix CBN (cubic boron nitride) powder material and binder with corresponding weight ratio, add one or more of carbon (C), chromium (Cr), cobalt (Co) or ceramic material in a ratio of 10%-30%, and pour tungsten carbide or nickel in a ratio of 2%-10%, stir evenly to obtain a mixed base material. Chromium and carbon combine to form chromium carbide, which can improve the tensile strength, hardness and heat resistance of the blade. Tungsten carbide or nickel and cobalt are combined to form a cemented carbide with extremely high hardness and excellent toughness. This material is not only wear-resistant, but also corrosion-resistant, and has high thermal stability and chemical stability;
[0038] S3: Put the mixed base material mixture into a molybdenum cup, add a salt carbon tube shielding layer for isolation, and then perform heat treatment under ultra-high temperature and high pressure conditions to tightly combine the CBN micropowder with the cemented carbide matrix to obtain a tool blank;
[0039] S4: Cooling and cutting: After the tool blank is cooled, it is cut and polished into a CBN blade of corresponding shape, completing the synthesis process of the CBN blade.
[0040] Comparison 2:
[0041] S1: Prepare CBN (cubic boron nitride) powder material and corresponding weight ratio binder;
[0042] S2: Mix the CBN (cubic boron nitride) powder material and the binder with the corresponding weight ratio, stir evenly, and prepare a mixed base material;
[0043] S3: preparing a base material mixture, pouring zirconium, vanadium or molybdenum with a weight ratio of 2%-15% into the mixed base material, and adding zirconium oxide, titanium, hafnium and rhenium with a weight ratio of 2%-15%, stirring evenly to obtain a base material mixture, zirconium is combined with zirconium oxide, so that the heat resistance of the prepared CBN blade is enhanced, and vanadium is combined with titanium, and molybdenum is combined with hafnium and rhenium, so that the heat resistance of the prepared CBN blade is enhanced;
[0044] S4: putting the mixed base material mixture into a molybdenum cup, adding a salt carbon tube shielding layer for isolation, and then heat treating it under ultra-high temperature and high pressure conditions to tightly combine the CBN micropowder with the cemented carbide matrix to obtain a tool blank;
[0045] S5: Cooling and cutting: After the tool blank is cooled, it is cut and polished into a CBN blade of corresponding shape, completing the synthesis process of the CBN blade.
[0046] Comparison 3:
[0047] S1: Prepare CBN (cubic boron nitride) powder material and corresponding weight ratio binder;
[0048] S2: Mix the CBN (cubic boron nitride) powder material and the binder with the corresponding weight ratio, stir evenly, and prepare a mixed base material;
[0049] S3: Put the mixed base material mixture into a molybdenum cup, add a salt carbon tube shielding layer for isolation, and then perform heat treatment under ultra-high temperature and high pressure conditions to tightly combine the CBN micropowder with the cemented carbide matrix to obtain a tool blank;
[0050] S4: Cooling and cutting, cooling the tool blank, cutting and grinding it into a CBN blade of corresponding shape, and spraying titanium nitride coating (TiN), chromium nitride coating (CrN) or aluminum oxide (Al2O3) on the surface of the CBN blade to complete the synthesis process of the CBN blade. Titanium nitride coating (TiN), chromium nitride coating (CrN) and aluminum oxide (Al2O3) are coated on the surface of the CBN blade of corresponding shape by physical vapor deposition (PVD) and chemical vapor deposition (CVD). When the chromium content exceeds 12%, the CBN blade can have good high-temperature oxidation resistance and resistance to oxidizing medium corrosion, so that the CBN blade can not only stably maintain high hardness, but also avoid oxidation discoloration on the surface of the CBN blade after long-term use.
[0051] Embodiment 1
[0052] Please refer to Figure 1 As shown: A synthesis process of a strong and tough CBN blade includes the following steps:
[0053] Step 1: Prepare base material, CBN (cubic boron nitride) powder material and corresponding weight ratio binder;
[0054] Step 2: Prepare a mixed base material, mix the CBN (cubic boron nitride) powder material and the binder with a corresponding weight ratio, add a tough material, pour in a reinforcing material with a corresponding weight ratio, stir evenly, and obtain a mixed base material;
[0055] Step 3: prepare a base material mixture, pour the heat-resistant material with a corresponding weight ratio into the mixed base material, add the heat-resistant composite material, stir evenly, and obtain a base material mixture;
[0056] Step 4: Prepare the tool body, put the mixed base material mixture into a molybdenum cup, add a salt carbon tube shielding layer for isolation, and then perform heat treatment under ultra-high temperature and high pressure conditions to tightly combine the CBN micropowder with the cemented carbide matrix to obtain the tool body;
[0057] Step 5: Cooling and cutting. After the tool blank is cooled, it is cut and polished into a CBN blade of corresponding shape, and a coating spray is sprayed on the surface of the CBN blade to complete the synthesis process of the CBN blade.
[0058] The total weight ratio of the CBN (cubic boron nitride) powder material and the binder to the grinding ball weight in step 1 is 2:7.
[0059] The strong and tough material in step 2 includes one or more of carbon (C), chromium (Cr), cobalt (Co) and ceramic materials, and the weight ratio of the strong and tough material is 10%-30% of the total mass;
[0060] The ceramic material is made of silicon nitride (Si3N4) or aluminum oxide (Al2O3).
[0061] The reinforcing material in step 2 includes one or both of tungsten carbide and nickel, and the weight ratio of the reinforcing material is 2%-10% of the total mass.
[0062] Chromium combines with carbon to form chromium carbide, which can improve the tensile strength, hardness and heat resistance of the blade. Tungsten carbide or nickel and cobalt combine to form cemented carbide with extremely high hardness and excellent toughness. This material is not only wear-resistant, but also corrosion-resistant, with high thermal and chemical stability, so that the prepared CBN blade can avoid edge collapse or breakage under severe impact or extreme conditions.
[0063] Embodiment 2
[0064] Please refer to Figure 1 As shown: Based on the first embodiment, the heat-resistant material in step three includes one or more of zirconium, vanadium and molybdenum, and the weight ratio of the heat-resistant material is 2%-15% of the total mass.
[0065] The heat-resistant composite material in step three includes zirconium oxide, titanium, hafnium and rhenium, and the weight ratio of the heat-resistant composite material is 2%-15% of the total mass.
[0066] The combination of zirconium and zirconium oxide enhances the heat resistance of the prepared CBN blades. At the same time, the combination of vanadium and titanium, and molybdenum with hafnium and rhenium enhances the heat resistance of the prepared CBN blades, ensuring that the CBN blades have good high heat resistance and high temperature stability.
[0067] Embodiment 3
[0068] Please refer to Figure 1 As shown: Based on Example 1, the coating spray in step five includes one or more of titanium nitride coating (TiN), chromium nitride coating (CrN) and aluminum oxide (Al2O3).
[0069] Titanium nitride coating (TiN), chromium nitride coating (CrN) and aluminum oxide (Al2O3) in the coating spray are coated on the surface of the corresponding shape of the CBN insert by physical vapor deposition (PVD) and chemical vapor deposition (CVD).
[0070] The heat treatment in step 4 is high temperature and high pressure sintering, which is used to vacuum dry the cemented carbide substrate at 200-400°C for 20-30 minutes, and then place the cemented carbide substrate in a six-sided top press for high temperature and high pressure sintering, with a temperature of 1200-1500°C and a pressure of 5-8GPA.
[0071] The hardness of the CBN blade made in step 5 is 48 GPa.
[0072] Titanium nitride coating (TiN), chromium nitride coating (CrN) and aluminum oxide (Al2O3) are coated on the surface of CBN blades of corresponding shapes by physical vapor deposition (PVD) and chemical vapor deposition (CVD). When the chromium content exceeds 12%, the CBN blades can have good high-temperature oxidation resistance and resistance to corrosion by oxidizing media, so that the CBN blades can not only stably maintain high hardness, but also avoid oxidation discoloration on the surface of the CBN blades after long-term use, thereby extending the service life of the CBN blades.
[0073] The test results of toughness and heat resistance are shown in Table 1 below:
[0074] Table 1: Tests of toughness and heat resistance
[0075] toughness(%) Heat resistance (%) Embodiment 1 45-70 700-1000 Embodiment 2 65-85 1000-1200 Embodiment 3 75-90 1200-1400
[0076] From the test results in the above table, it can be seen that the toughness and heat resistance of the prepared strong and tough CBN blades are significantly enhanced.
[0077] The present invention provides a synthesis process for a strong and tough CBN blade. When operating the method, a base material needs to be prepared first, a CBN (cubic boron nitride) powder material and a binder with a corresponding weight ratio are prepared, the CBN (cubic boron nitride) powder material and the binder with a corresponding weight ratio are mixed evenly, a strong and tough material is added, and a reinforcing material with a corresponding weight ratio is poured in, and stirred evenly to obtain a mixed base material. The strong and tough material is added after the CBN (cubic boron nitride) powder material and the binder are mixed. The strong and tough material includes carbon (C), chromium (Cr), cobalt (Co) and ceramic material, and a reinforcing material is added to enhance the toughness after combining with the strong and tough material. The reinforcing material includes tungsten carbide and nickel. Since chromium combines with carbon to form chromium carbide, the tensile strength, hardness and heat resistance of the blade can be improved. The tungsten carbide or nickel is combined with cobalt to form a cemented carbide with extremely high hardness and excellent toughness. This material is not only wear-resistant, but also corrosion-resistant, and has high thermal and chemical stability, so that the prepared CBN blades can avoid edge collapse or breakage under severe impact or extreme conditions; the heat-resistant material with a corresponding weight ratio is poured into the mixed mixed base material, and the heat-resistant composite material is added and stirred evenly to obtain a base material mixture, and the heat-resistant material and the heat-resistant composite material are added. The heat-resistant material includes zirconium, vanadium and molybdenum, and the heat-resistant composite material includes zirconium oxide, titanium, hafnium and rhenium. Zirconium is combined with zirconium oxide, so that the heat resistance of the prepared CBN blade is enhanced. At the same time, vanadium is combined with titanium, and molybdenum is combined with hafnium and rhenium, so that the heat resistance of the prepared CBN blade is enhanced, ensuring that the CBN blade has good high heat resistance and high temperature stability; the mixed base material mixture is placed in a molybdenum cup, and a salt carbon tube shielding layer is added for isolation, and then heat-treated under ultra-high temperature and high pressure conditions to tightly combine the CBN micropowder with the cemented carbide matrix. , obtain a tool blank; after cooling the tool blank, cut and grind it into a CBN blade of corresponding shape, and spray the coating spray on the surface of the CBN blade to complete the synthesis process of the CBN blade, spray the coating spray on the surface of the formed CBN blade, the coating spray includes titanium nitride coating (TiN), chromium nitride coating (CrN) and aluminum oxide (Al2O3), and the titanium nitride coating (TiN), chromium nitride coating (CrN) and aluminum oxide (Al2O3) are coated on the surface of the CBN blade of corresponding shape by physical vapor deposition (PVD) and chemical vapor deposition (CVD), and when the chromium content exceeds 12%, the CBN blade can have good high-temperature oxidation resistance and resistance to oxidative medium corrosion, so that the CBN blade can not only stably maintain high hardness, but also avoid oxidation discoloration on the surface of the CBN blade after long-term use, thereby extending the service life of the CBN blade. The synthesis process of the entire strong and tough CBN blade is simple and the blade has good use effect.
[0078] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A synthesis process for a tough CBN blade, characterized in that: The synthesis process of the tough CBN blade comprises the following steps: Step 1: Prepare base material, CBN (cubic boron nitride) powder material and corresponding weight ratio binder; Step 2: Prepare a mixed base material, mix the CBN (cubic boron nitride) powder material and the binder with a corresponding weight ratio, add a tough material, pour in a reinforcing material with a corresponding weight ratio, stir evenly, and obtain a mixed base material; Step 3: prepare a base material mixture, pour the heat-resistant material with a corresponding weight ratio into the mixed base material, add the heat-resistant composite material, stir evenly, and obtain a base material mixture; Step 4: Prepare the tool body, put the mixed base material mixture into a molybdenum cup, add a salt carbon tube shielding layer for isolation, and then perform heat treatment under ultra-high temperature and high pressure conditions to tightly combine the CBN micropowder with the cemented carbide matrix to obtain the tool body; Step 5: Cooling and cutting. After the tool blank is cooled, it is cut and polished into a CBN blade of corresponding shape, and a coating spray is sprayed on the surface of the CBN blade to complete the synthesis process of the CBN blade.
2. The method according to claim 1, characterized in that The total weight ratio of the CBN (cubic boron nitride) powder material and the binder to the grinding ball weight in step 1 is 2:
7.
3. The method according to claim 1, characterized in that The strong and tough material in step 2 includes one or more of carbon (C), chromium (Cr), cobalt (Co) and ceramic materials, and the weight ratio of the strong and tough material is 10%-30% of the total mass; The ceramic material is made of silicon nitride (Si3N4) or aluminum oxide (Al2O3).
4. The method according to claim 1, characterized in that: The reinforcing material in step 2 includes one or both of tungsten carbide and nickel, and the weight ratio of the reinforcing material is 2%-10% of the total mass.
5. The method according to claim 1, characterized in that: The heat-resistant material in step three includes one or more of zirconium, vanadium and molybdenum, and the weight ratio of the heat-resistant material is 2%-15% of the total mass.
6. The method according to claim 1, characterized in that The heat-resistant composite material in step three comprises zirconium oxide, titanium, hafnium and rhenium, and the weight ratio of the heat-resistant composite material is 2%-15% of the total mass.
7. The method according to claim 1, characterized in that The coating spray in step five includes one or more of titanium nitride coating (TiN), chromium nitride coating (CrN) and aluminum oxide (Al2O3).
8. The method according to claim 7, characterized in that The titanium nitride coating (TiN), chromium nitride coating (CrN) and aluminum oxide (Al2O3) in the coating spray are coated on the surface of the CBN insert of corresponding shape by physical vapor deposition (PVD) and chemical vapor deposition (CVD).
9. The method according to claim 1, characterized in that: The heat treatment in step 4 is high temperature and high pressure sintering, which is used to vacuum dry the cemented carbide substrate at 200-400°C for 20-30 minutes, and then place the cemented carbide substrate in a six-sided top press for high temperature and high pressure sintering, with a temperature of 1200-1500°C and a pressure of 5-8GPA.
10. The method according to claim 1, characterized in that The hardness of the CBN blade made in step 5 is 48 GPa.