Preparation method of Hastelloy X nickel-based superalloy based on selective laser melting technology

Through the comprehensive method of selective laser melting forming, hot isostatic pressing, solid solution treatment and stress relief annealing, the problems of residual stress and micro-cracks in Hastelloy X nickel-based superalloy were solved, and the microstructure and mechanical properties of the material were optimized. The comprehensive performance improvement of high-temperature alloys has been achieved.

CN118720168APending Publication Date: 2024-10-01SOUTHWEST JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410835401.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When traditional selective laser melting technology is used to prepare Hastelloy , leading to oxidation or carbide formation, further reducing performance.

Method used

Using a comprehensive method of selective laser melting, hot isostatic pressing, solid solution treatment and stress relief annealing, unmelted particles and dendrites are eliminated through high temperature and high pressure environment, grain boundary carbides are melted back, residual stress is removed, and uniform supersaturation is formed. Solid solution, optimizing material microstructure.

Benefits of technology

Effectively eliminate holes and cracks in the alloy, improve plasticity and strength, enhance high-temperature stability, improve mechanical properties, and ensure that the comprehensive performance of the material meets aerospace standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004913031140000091
    Figure BDA0004913031140000091
  • Figure HDA0004913031150000011
    Figure HDA0004913031150000011
  • Figure HDA0004913031150000012
    Figure HDA0004913031150000012
Patent Text Reader

Abstract

The invention discloses a preparation method of a Hastelloy X nickel-based superalloy based on a selective laser melting technology. The preparation method comprises the following steps: S1, selective laser melting molding: carrying out selective laser melting molding to obtain the Hastelloy X nickel-based superalloy; the process parameters are as follows: the light spot area is 2.5 to 3.5 mm, the layer thickness is 20 to 35 microns, the laser power is 150 to 190 W, the scanning speed is 1000 to 1100 mm / s, and the scanning distance is 0.07 to 0.11 mm; the Hastelloy X nickel-based high-temperature alloy powder is prepared from the following elements in percentage by mass: 20.0 to 23.0 percent of WCr, 6.5 to 10.0 percent of WMo, 17.0 to 20.0 percent of WFe, 0.5 to 2.5 percent of WCo, 0.2 to 1.0 percent of Ww and the balance of WNi; s2, hot isostatic pressing treatment is conducted, specifically, the hot isostatic pressing treatment temperature ranges from 1110 DEG C to 1130 DEG C, the time ranges from 100 min to 140 min, the pressure ranges from 140 MPa to 160 MPa, and furnace cooling is conducted to the room temperature after hot isostatic pressing treatment; s3, solution treatment is conducted, specifically, the solution treatment temperature ranges from 1110 DEG C to 1130 DEG C, the time ranges from 115 min to 125 min, and air cooling is conducted to the room temperature after solution treatment; s4, stress relief annealing treatment is conducted, specifically, the stress relief annealing temperature ranges from 750 DEG C to 770 DEG C, and the stress relief annealing time ranges from 20 min to 40 min; the preparation steps are carried out under the protection of an argon atmosphere. According to the preparation method disclosed by the invention, the Hastelloy X nickel-based high-temperature alloy with excellent comprehensive mechanical properties can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention provides a preparation method of Hastelloy X nickel-based high-temperature alloy based on selective laser melting technology, belonging to the technical field of additive manufacturing. Background Art

[0002] Hastelloy X alloy is a nickel-based high-temperature alloy mainly composed of solid solution strengthening elements Mo, W and Cr, with a melting point temperature range of 1260-1355℃. It is widely used in aerospace, petroleum, chemical and nuclear energy industries due to its excellent weldability and multifunctional properties (such as excellent corrosion resistance, high oxidation resistance and high strength). However, traditional manufacturing processes are difficult to meet the requirements of lightweight parts with complex structures and high precision. Additive manufacturing (AM) of metal components has been widely studied as the main means of manufacturing high-performance metal components because it can manufacture components with complex geometries.

[0003] The grains of nickel-based high-temperature alloy parts prepared by Selective Laser Melting (SLM) technology are mainly columnar crystals and some equiaxed crystals. Its basic phase composition is γ, γ′, Laves phase and some MC carbides. The presence of brittle phases causes the mechanical properties and creep properties of SLM directly formed parts to be far lower than the standards of aerospace forgings, so it is necessary to perform post-processing to improve its mechanical properties.

[0004] CN116586634A provides a heat treatment method for selective laser melting of nickel-based high-temperature alloy GH3536, which includes: preparing GH3536 nickel alloy samples; heating the heat treatment furnace and testing the actual temperature at the end of heating with a thermocouple; placing the GH3536 nickel alloy sample at the center of the heat treatment furnace and keeping it warm; after the insulation is completed, taking out the GH3536 nickel alloy sample and cooling it to room temperature with the furnace. However, the problem with this technical solution is that the selective laser melting technology will cause a large amount of residual stress inside the alloy due to its high cooling rate and large temperature gradient during the preparation process, thereby causing microcracks and a decrease in its mechanical properties.

[0005] CN113528992A provides a heat treatment method for optimizing the mechanical properties of additively manufactured GH3536 nickel-based high-temperature alloys, wherein the GH3536 nickel-based high-temperature alloy is prepared by additive manufacturing technology, the muffle furnace is heated to 1020-1080°C, the obtained additively manufactured GH3536 nickel-based high-temperature alloy is quickly placed in the muffle furnace for solid solution heat treatment, and then the obtained solid solution heat treated GH3536 nickel-based high-temperature alloy is cooled in the air. The problem with this technical solution is that the muffle furnace cannot ensure that the sample is treated in a vacuum or inert gas-filled environment, and atoms such as O and C will enter during the heat treatment process to form oxides or carbides, which will have an adverse effect on the mechanical properties of the material. Summary of the invention

[0006] The purpose of the present invention is to propose a preparation method of Hastelloy X nickel-based high-temperature alloy based on selective laser melting technology. The preparation method combines selective laser melting molding, hot isostatic pressing, solution treatment and stress relief annealing to solve the problem that defects such as microcracks and pores in the prior art cannot be closed. At the same time, the precipitated phases of the grains or grain boundaries are dispersed, the residual stress inside the matrix is ​​reduced, and the stress concentration disappears, thereby obtaining a Hastelloy X nickel-based high-temperature alloy with excellent comprehensive mechanical properties.

[0007] The technical solution adopted by the present invention to achieve its invention object is: a preparation method of Hastelloy X nickel-based high-temperature alloy based on selective laser melting technology, the steps of which are as follows:

[0008] S1. Selective laser melting: A Hastelloy X nickel-based high-temperature alloy powder spread on a substrate is subjected to selective laser melting by a laser according to a preset scanning path to obtain a Hastelloy X nickel-based high-temperature alloy. The process parameters of the selective laser melting are: spot area 2.5-3.5 mm, layer thickness 20-35 μm, laser power 150-190 W, scanning speed 1000-1100 mm / s, and scanning spacing 0.07-0.11 mm. The Hastelloy X nickel-based high-temperature alloy powder is composed of the following alloy elements according to mass percentage: W Cr =20.0%-23.0%, W Mo =6.5%-10.0%, W Fe =17.0%-20.0%, W Co =0.5%-2.5%, W w =0.2%-1.0%, W Ni margin;

[0009] S2, hot isostatic pressing treatment: hot isostatic pressing treatment is performed on the Hastelloy X nickel-based high-temperature alloy formed by selective laser melting; the hot isostatic pressing treatment temperature is 1110° C.-1130° C., the time is 100-140 min, and the pressure is 140-160 MPa. After the hot isostatic pressing treatment, the Hastelloy X nickel-based high-temperature alloy is cooled to room temperature with the furnace;

[0010] S3, solution treatment: subjecting the Hastelloy X nickel-based high-temperature alloy subjected to hot isostatic pressing to solution treatment; the solution treatment temperature is 1110° C.-1130° C., and the time is 115-125 min. After the solution treatment, the Hastelloy X nickel-based high-temperature alloy is air-cooled to room temperature;

[0011] S4, stress relief annealing treatment: the Hastelloy X nickel-based high-temperature alloy that has undergone solid solution treatment is subjected to stress relief annealing treatment; the stress relief annealing temperature is 750° C.-770° C., and the time is 20-40 minutes;

[0012] The selective laser melting forming, hot isostatic pressing, solution treatment and stress relief annealing treatment are all carried out under the protection of argon atmosphere.

[0013] Furthermore, in the selective laser melting forming in step S1 of the present invention, the particle size distribution range of the Hastelloy X nickel-based high-temperature alloy powder is 15 to 53 μm, wherein D(10) is 21.77 μm, D(50) is 34.19 μm, D(90) is 53.0 μm, and D(95) is 61.20 μm.

[0014] Furthermore, in the selective laser melting molding in step S1 of the present invention, the scanning direction of each layer is rotated 67° based on the printing direction of the previous layer. This can optimize the microstructure of the material, ensure that each layer can be melted evenly, improve the density and surface roughness, and reduce the residual stress in the processing process to a certain extent.

[0015] Furthermore, the specific operation of the hot isostatic pressing treatment of the present invention is to place the Hastelloy X nickel-based high-temperature alloy formed by selective laser melting in a hot isostatic pressing furnace, heat it from room temperature to the hot isostatic pressing treatment temperature at a rate of 8-10°C / min, keep it warm and pressurize it, and the holding time is the hot isostatic pressing treatment time.

[0016] Furthermore, the specific operation of the solution treatment of the present invention is to place the Hastelloy X nickel-based high-temperature alloy that has undergone hot isostatic pressing in a heat treatment furnace, heat it to the solution treatment temperature at a heating rate of 8°C / min-10°C / min, and keep it warm. The insulation time is the solution treatment time.

[0017] Furthermore, the present invention performs a pre-insulation treatment before performing a solid solution treatment on the Hastelloy X nickel-based high-temperature alloy subjected to hot isostatic pressing. The specific operation of the pre-insulation treatment is to place the Hastelloy X nickel-based high-temperature alloy in a heat treatment furnace, heat it to 800° C. at a heating rate of 8° C. / min, and keep it warm for 30 minutes.

[0018] Furthermore, before the selective laser melting-molded Hastelloy X nickel-based high-temperature alloy is subjected to hot isostatic pressing, the Hastelloy X nickel-based high-temperature alloy is first cleaned. The specific cleaning method is to slightly grind the six surfaces of the Hastelloy X nickel-based high-temperature alloy with sandpaper to remove the surface oxide film generated by natural aging, and then use an ultrasonic cleaning machine to vibrate for 20-30 seconds to remove surface waste powder.

[0019] The principles and beneficial effects of the present invention are:

[0020] The manufacturing of Hastelloy X nickel-based high-temperature alloy is realized by selective laser melting, which can quickly and accurately manufacture alloys with complex shapes. However, due to the extremely fast cooling speed of rapid molding, the temperature gradient inside the sample after molding is very large, and the thermal stress inside the sample is extremely high, which will cause defects such as microcracks. To solve this problem, the present invention uses three steps for heat treatment. The first step is to perform hot isostatic pressing. Through the high temperature and high pressure environment, the unmelted particles inside the material are melted, the dendrite substructure inside the molten pool disappears, the molten pool line disappears, the grains tend to be uniform, the material tends to be isotropic, the microstructure of the material is improved, the holes and cracks are effectively eliminated, and the plasticity of the material is improved. However, the disappearance of the dendrite substructure of the alloy and the growth of the grains lead to a significant decrease in its strength and hardness, and a large amount of precipitated carbides will appear at the grain boundaries. Therefore, the second step is to perform solid solution treatment. A large amount of carbides at the grain boundaries of the alloy are formed. The carbides are dissolved back into the matrix, and the solid solution strengthening effect of the matrix is ​​increased. The solid solution treatment of the present invention adopts a furnace cooling process. After furnace cooling, there are many intermittent chain carbides precipitated at the grain boundaries, and the promotion effect of chain carbides on crack initiation is reduced. It can strengthen the grains and grain boundaries, prevent dislocation movement, and improve the high temperature strength and thermal stability of the alloy. The strength, hardness and plasticity of the alloy are further improved; the third step is to perform stress relief annealing treatment to remove the residual stress generated by the heat treatment, reduce the tendency of deformation and cracking, and dissolve the carbides inside the matrix to obtain a uniform supersaturated solid solution. The order of the three heat treatments cannot be reversed. The premise of the solid solution treatment is to be as uniform and dense as possible. Only in this way can the solute atoms be better dispersed in the matrix, so as to achieve the best solid solution effect. This heat treatment order can give full play to the advantages of hot isostatic pressing and solid solution treatment, so as to improve the overall performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a scanning electron microscope image of the Hastelloy X nickel-based high-temperature alloy obtained in Example 1 of the present invention.

[0022] Figure 2 This is a scanning electron microscope image of the Hastelloy X nickel-based high-temperature alloy obtained in Example 2 of the present invention.

[0023] Figure 3 This is a scanning electron microscope image of the Hastelloy X nickel-based high-temperature alloy obtained in Example 3 of the present invention.

[0024] Figure 4 This is a scanning electron microscope image of the Hastelloy X nickel-based high-temperature alloy obtained in Comparative Example 1.

[0025] Figure 5 This is a scanning electron microscope image of the Hastelloy X nickel-based high-temperature alloy obtained in Comparative Example 2.

[0026] Figure 6 This is a scanning electron microscope image of the Hastelloy X nickel-based high-temperature alloy obtained in Comparative Example 3. DETAILED DESCRIPTION

[0027] Embodiment 1

[0028] A method for preparing Hastelloy X nickel-based high-temperature alloy based on selective laser melting technology, the steps of which are as follows:

[0029] S1. Selective laser melting: A Hastelloy X nickel-based high-temperature alloy powder spread on a substrate is subjected to selective laser melting by a laser according to a preset scanning path to obtain a Hastelloy X nickel-based high-temperature alloy. The process parameters of the selective laser melting are: spot area 3.0 mm, layer thickness 25 μm, laser power 170 W, scanning speed 1050 mm / s, and scanning spacing 0.09 mm. The Hastelloy X nickel-based high-temperature alloy powder is composed of the following alloy elements according to mass percentage: W Cr =20.61%, W Mo =6.54%, W Fe =17.92%, W Co =1.41%, W w =0.64%, W Ni margin;

[0030] S2. Hot isostatic pressing: The Hastelloy X nickel-based high-temperature alloy formed by selective laser melting is placed in a hot isostatic pressing furnace, and the temperature is raised from room temperature to a hot isostatic pressing temperature of 1120°C at a rate of 8°C / min. The temperature is kept and pressurized for 120 minutes at a pressure of 150MPa. After the hot isostatic pressing, the Hastelloy X nickel-based high-temperature alloy is cooled to room temperature along with the furnace;

[0031] S3, solution treatment: placing the Hastelloy X nickel-based high-temperature alloy that has undergone hot isostatic pressing in a heat treatment furnace, heating it to a solution treatment temperature of 1120°C at a heating rate of 8°C / min, and keeping it warm for 120 minutes. After the solution treatment, the Hastelloy X nickel-based high-temperature alloy is air-cooled to room temperature;

[0032] S4, stress relief annealing treatment: the Hastelloy X nickel-based high-temperature alloy that has undergone solid solution treatment is subjected to stress relief annealing treatment; the stress relief annealing temperature is 760° C. and the time is 30 minutes;

[0033] The selective laser melting forming, hot isostatic pressing, solution treatment and stress relief annealing treatment are all carried out under the protection of argon atmosphere.

[0034] In the selective laser melting forming in step S1 of this example, the particle size distribution range of the Hastelloy X nickel-based high-temperature alloy powder is 15-53 μm, wherein D(10) is 21.77 μm, D(50) is 34.19 μm, D(90) is 53.0 μm, and D(95) is 61.20 μm.

[0035] In the selective laser melting molding in step S1 of this example, the scanning direction of each layer is rotated by 67° based on the printing direction of the previous layer.

[0036] In this example, before the Hastelloy X nickel-based high-temperature alloy subjected to hot isostatic pressing is subjected to solution treatment, a pre-insulation treatment is first performed. The specific operation of the pre-insulation treatment is to place the Hastelloy X nickel-based high-temperature alloy in a heat treatment furnace, heat it to 800° C. at a heating rate of 8° C. / min, and keep it at that temperature for 30 minutes.

[0037] In this example, before the Hastelloy X nickel-based high-temperature alloy formed by selective laser melting is subjected to hot isostatic pressing, the Hastelloy X nickel-based high-temperature alloy is first cleaned. The specific cleaning method is to slightly grind the six surfaces of the Hastelloy X nickel-based high-temperature alloy with sandpaper to remove the surface oxide film generated by natural aging, and then use an ultrasonic cleaning machine to vibrate for 20-30s to remove surface waste powder.

[0038] Figure 1: This is a scanning electron microscope image of the Hastelloy X nickel-based high-temperature alloy obtained in this embodiment. Figure 1 It can be seen that there is no obvious precipitation phase inside the sample. With the increase of solution time and solution temperature, some precipitation phases in the material dissolve back into the matrix, the proportion of small-angle grain boundaries gradually decreases, the hindering effect on grain boundaries weakens, and the plastic deformation ability of the material increases. At high temperatures, the thermal motion of atoms is significantly enhanced, the lattice is distorted, and the lattice arrangement in some areas changes, thus forming twins. The appearance of twins can hinder the movement of dislocations, and the twin boundaries can play a role similar to that of grain boundaries, thereby limiting the slip of grains and increasing their tensile properties.

[0039] Embodiment 2

[0040] A method for preparing Hastelloy X nickel-based high-temperature alloy based on selective laser melting technology, the steps of which are as follows:

[0041] S1. Selective laser melting: A Hastelloy X nickel-based high-temperature alloy powder spread on a substrate is subjected to selective laser melting by a laser according to a preset scanning path to obtain a Hastelloy X nickel-based high-temperature alloy. The process parameters of the selective laser melting are: spot area 2.7 mm, layer thickness 20 μm, laser power 160 W, scanning speed 1000 mm / s, and scanning spacing 0.07 mm. The Hastelloy X nickel-based high-temperature alloy powder is composed of the following alloy elements according to mass percentage: W Cr =20.61%, W Mo =6.54%, W Fe =17.92%, W Co =1.41%, W w =0.64%, W Ni margin;

[0042] S2. Hot isostatic pressing: The Hastelloy X nickel-based high-temperature alloy formed by selective laser melting is placed in a hot isostatic pressing furnace, and the temperature is raised from room temperature to a hot isostatic pressing temperature of 1110°C at a rate of 8°C / min. The temperature is kept and pressurized for 120 minutes at a pressure of 150MPa. After the hot isostatic pressing, the Hastelloy X nickel-based high-temperature alloy is cooled to room temperature along with the furnace;

[0043] S3, solution treatment: placing the Hastelloy X nickel-based high-temperature alloy that has undergone hot isostatic pressing in a heat treatment furnace, heating it to a solution treatment temperature of 1110°C at a heating rate of 8°C / min, and keeping it warm for 115 minutes. After the solution treatment, the Hastelloy X nickel-based high-temperature alloy is air-cooled to room temperature;

[0044] S4, stress relief annealing treatment: the Hastelloy X nickel-based high-temperature alloy that has undergone solid solution treatment is subjected to stress relief annealing treatment; the stress relief annealing temperature is 760° C. and the time is 20 min;

[0045] The selective laser melting forming, hot isostatic pressing, solution treatment and stress relief annealing treatment are all carried out under the protection of argon atmosphere.

[0046] In the selective laser melting forming in step S1 of this example, the particle size distribution range of the Hastelloy X nickel-based high-temperature alloy powder is 15-53 μm, wherein D(10) is 21.77 μm, D(50) is 34.19 μm, D(90) is 53.0 μm, and D(95) is 61.20 μm.

[0047] In the selective laser melting molding in step S1 of this example, the scanning direction of each layer is rotated by 67° based on the printing direction of the previous layer.

[0048] In this example, before the Hastelloy X nickel-based high-temperature alloy subjected to hot isostatic pressing is subjected to solution treatment, a pre-insulation treatment is first performed. The specific operation of the pre-insulation treatment is to place the Hastelloy X nickel-based high-temperature alloy in a heat treatment furnace, heat it to 800° C. at a heating rate of 8° C. / min, and keep it at that temperature for 30 minutes.

[0049] In this example, before the Hastelloy X nickel-based high-temperature alloy formed by selective laser melting is subjected to hot isostatic pressing, the Hastelloy X nickel-based high-temperature alloy is first cleaned. The specific cleaning method is to slightly grind the six surfaces of the Hastelloy X nickel-based high-temperature alloy with sandpaper to remove the surface oxide film generated by natural aging, and then use an ultrasonic cleaning machine to vibrate for 20-30s to remove surface waste powder.

[0050] Figure 2 : This is a scanning electron microscope image of the Hastelloy X nickel-based high-temperature alloy obtained in this embodiment. Figure 2 It can be seen that the organizational morphology of this embodiment is different from that of Embodiment 1 and Embodiment 3, and is an uneven equiaxed crystal, most of which are irregular elongated crystals. However, since its precipitated phase is distributed in the grain boundary in a chain shape, it can effectively hinder the dislocation movement during the deformation process, play the effect of grain boundary strengthening, and can maintain good tensile properties at room temperature. Although the yield strength and tensile strength are higher than those of Embodiment 1 and Embodiment 3, the elongation after fracture is reduced.

[0051] Embodiment 3

[0052] A method for preparing Hastelloy X nickel-based high-temperature alloy based on selective laser melting technology, the steps of which are as follows:

[0053] S1. Selective laser melting: A Hastelloy X nickel-based high-temperature alloy powder spread on a substrate is subjected to selective laser melting by a laser according to a preset scanning path to obtain a Hastelloy X nickel-based high-temperature alloy. The process parameters of the selective laser melting are: spot area 3.3 mm, layer thickness 30 μm, laser power 190 W, scanning speed 1100 mm / s, and scanning spacing 0.11 mm. The Hastelloy X nickel-based high-temperature alloy powder is composed of the following alloy elements according to mass percentage: W Cr =20.61%, W Mo =6.54%, W Fe =17.92%, W Co =1.41%, W w =0.64%, W Ni margin;

[0054] S2. Hot isostatic pressing: The Hastelloy X nickel-based high-temperature alloy formed by selective laser melting is placed in a hot isostatic pressing furnace, and the temperature is raised from room temperature to a hot isostatic pressing temperature of 1130°C at a rate of 8°C / min. The temperature is kept and pressurized for 120 minutes at a pressure of 150MPa. After the hot isostatic pressing, the Hastelloy X nickel-based high-temperature alloy is cooled to room temperature along with the furnace;

[0055] S3, solution treatment: placing the Hastelloy X nickel-based high-temperature alloy after hot isostatic pressing in a heat treatment furnace, heating it to a solution treatment temperature of 1130°C at a heating rate of 8°C / min, and keeping it warm for 125 minutes. After the solution treatment, the Hastelloy X nickel-based high-temperature alloy is air-cooled to room temperature;

[0056] S4, stress relief annealing treatment: the Hastelloy X nickel-based high-temperature alloy that has undergone solid solution treatment is subjected to stress relief annealing treatment; the stress relief annealing temperature is 750° C. and the time is 35 minutes;

[0057] The selective laser melting forming, hot isostatic pressing, solution treatment and stress relief annealing treatment are all carried out under the protection of argon atmosphere.

[0058] In the selective laser melting forming in step S1 of this example, the particle size distribution range of the Hastelloy X nickel-based high-temperature alloy powder is 15-53 μm, wherein D(10) is 21.77 μm, D(50) is 34.19 μm, D(90) is 53.0 μm, and D(95) is 61.20 μm.

[0059] In the selective laser melting molding in step S1 of this example, the scanning direction of each layer is rotated by 67° based on the printing direction of the previous layer.

[0060] In this example, before the Hastelloy X nickel-based high-temperature alloy subjected to hot isostatic pressing is subjected to solution treatment, a pre-insulation treatment is first performed. The specific operation of the pre-insulation treatment is to place the Hastelloy X nickel-based high-temperature alloy in a heat treatment furnace, heat it to 800° C. at a heating rate of 8° C. / min, and keep it at that temperature for 30 minutes.

[0061] In this example, before the Hastelloy X nickel-based high-temperature alloy formed by selective laser melting is subjected to hot isostatic pressing, the Hastelloy X nickel-based high-temperature alloy is first cleaned. The specific cleaning method is to slightly grind the six surfaces of the Hastelloy X nickel-based high-temperature alloy with sandpaper to remove the surface oxide film generated by natural aging, and then use an ultrasonic cleaning machine to vibrate for 20-30s to remove surface waste powder.

[0062] Figure 3 : This is a scanning electron microscope image of the Hastelloy X nickel-based high-temperature alloy obtained in this embodiment. Figure 3 It can be seen that the grain structure is similar to that of Example 1, both of which are larger equiaxed crystals. There are also twin boundaries of different lengths inside the grains, and there are a small amount of precipitated phases inside the grains. Under appropriate layer width and scanning speed, there are no obvious microcracks and hole defects inside the grains, and the mechanical properties are similar to those of Example 1. Under this process parameter, the performance meets the standard use requirements and the technology is feasible.

[0063] Comparative Example 1

[0064] A method for preparing Hastelloy X nickel-based high-temperature alloy based on selective laser melting technology, the steps of which are as follows:

[0065] S1. Selective laser melting: A Hastelloy X nickel-based high-temperature alloy powder spread on a substrate is subjected to selective laser melting by a laser according to a preset scanning path to obtain a Hastelloy X nickel-based high-temperature alloy. The process parameters of the selective laser melting are: spot area 2.5 mm, layer thickness 35 μm, laser power 200 W, scanning speed 1150 mm / s, and scanning spacing 0.11 mm. The Hastelloy X nickel-based high-temperature alloy powder is composed of the following alloy elements according to mass percentage: W Cr =20.61%, W Mo =6.54%, W Fe =17.92%, W Co =1.41%, W w =0.64%, WNi margin;

[0066] S2. Hot isostatic pressing: The Hastelloy X nickel-based high-temperature alloy formed by selective laser melting is placed in a hot isostatic pressing furnace, and the temperature is raised from room temperature to a hot isostatic pressing temperature of 1100°C at a rate of 8°C / min. The temperature is kept and pressurized for 120 minutes at a pressure of 150MPa. After the hot isostatic pressing, the Hastelloy X nickel-based high-temperature alloy is cooled to room temperature along with the furnace;

[0067] S3, solution treatment: placing the Hastelloy X nickel-based high-temperature alloy that has undergone hot isostatic pressing in a heat treatment furnace, heating it to a solution treatment temperature of 1140°C at a heating rate of 8°C / min, and keeping it warm for 115 minutes. After the solution treatment, the Hastelloy X nickel-based high-temperature alloy is air-cooled to room temperature;

[0068] S4, stress relief annealing treatment: the Hastelloy X nickel-based high-temperature alloy that has undergone solid solution treatment is subjected to stress relief annealing treatment; the stress relief annealing temperature is 770° C. and the time is 25 minutes;

[0069] The selective laser melting forming, hot isostatic pressing, solution treatment and stress relief annealing treatment are all carried out under the protection of argon atmosphere.

[0070] In the selective laser melting forming in step S1 of this example, the particle size distribution range of the Hastelloy X nickel-based high-temperature alloy powder is 15-53 μm, wherein D(10) is 21.77 μm, D(50) is 34.19 μm, D(90) is 53.0 μm, and D(95) is 61.20 μm.

[0071] In the selective laser melting molding in step S1 of this example, the scanning direction of each layer is rotated by 67° based on the printing direction of the previous layer.

[0072] In this example, before the Hastelloy X nickel-based high-temperature alloy subjected to hot isostatic pressing is subjected to solution treatment, a pre-insulation treatment is first performed. The specific operation of the pre-insulation treatment is to place the Hastelloy X nickel-based high-temperature alloy in a heat treatment furnace, heat it to 800° C. at a heating rate of 8° C. / min, and keep it at that temperature for 30 minutes.

[0073] In this example, before the Hastelloy X nickel-based high-temperature alloy formed by selective laser melting is subjected to hot isostatic pressing, the Hastelloy X nickel-based high-temperature alloy is first cleaned. The specific cleaning method is to slightly grind the six surfaces of the Hastelloy X nickel-based high-temperature alloy with sandpaper to remove the surface oxide film generated by natural aging, and then use an ultrasonic cleaning machine to vibrate for 20-30s to remove surface waste powder.

[0074] Figure 4 : This is a scanning electron microscope image of the Hastelloy X nickel-based high-temperature alloy obtained in this comparative example. Figure 4 It can be seen that unevenly distributed precipitates appear at the grain boundaries. Although these precipitates will hinder the movement of dislocations, they are in block form and cannot play a strengthening role. They are prone to microcracks during the stretching process. In addition, due to the fast scanning speed and wide layer thickness, the powder cannot be completely melted during the printing process, thereby reducing the tensile strength of the sample. The high temperature process will make the dislocation movement more active. Due to the increase in the solution temperature, the number of dislocations is reduced, and the yield strength is also reduced. The increase in the content of precipitates will also hinder the slip between grains, causing the material's plastic deformation ability to decrease by about 25% of the embodiment.

[0075] Comparative Example 2

[0076] A method for preparing Hastelloy X nickel-based high-temperature alloy based on selective laser melting technology, the steps of which are as follows:

[0077] S1. Selective laser melting: A Hastelloy X nickel-based high-temperature alloy powder spread on a substrate is subjected to selective laser melting by a laser according to a preset scanning path to obtain a Hastelloy X nickel-based high-temperature alloy. The process parameters of the selective laser melting are: spot area 3.5 mm, layer thickness 20 μm, laser power 140 W, scanning speed 1000 mm / s, and scanning spacing 0.07 mm. The Hastelloy X nickel-based high-temperature alloy powder is composed of the following alloy elements according to mass percentage: W Cr =20.61%, W Mo =6.54%, W Fe =17.92%, W Co =1.41%, W w =0.64%, W Ni margin;

[0078] S2. Hot isostatic pressing: The Hastelloy X nickel-based high-temperature alloy formed by selective laser melting is placed in a hot isostatic pressing furnace, and the temperature is raised from room temperature to a hot isostatic pressing temperature of 1140°C at a rate of 8°C / min. The temperature is kept and pressurized for 110 minutes at a pressure of 150MPa. After the hot isostatic pressing, the Hastelloy X nickel-based high-temperature alloy is cooled to room temperature along with the furnace;

[0079] S3, solution treatment: placing the Hastelloy X nickel-based high-temperature alloy that has undergone hot isostatic pressing in a heat treatment furnace, heating it to a solution treatment temperature of 1100°C at a heating rate of 8°C / min, and keeping it warm for 130 minutes. After the solution treatment, the Hastelloy X nickel-based high-temperature alloy is air-cooled to room temperature;

[0080] S4, stress relief annealing treatment: the Hastelloy X nickel-based high-temperature alloy that has undergone solid solution treatment is subjected to stress relief annealing treatment; the stress relief annealing temperature is 780° C. and the time is 40 minutes;

[0081] The selective laser melting forming, hot isostatic pressing, solution treatment and stress relief annealing treatment are all carried out under the protection of argon atmosphere.

[0082] In the selective laser melting forming in step S1 of this example, the particle size distribution range of the Hastelloy X nickel-based high-temperature alloy powder is 15-53 μm, wherein D(10) is 21.77 μm, D(50) is 34.19 μm, D(90) is 53.0 μm, and D(95) is 61.20 μm.

[0083] In the selective laser melting molding in step S1 of this example, the scanning direction of each layer is rotated by 67° based on the printing direction of the previous layer.

[0084] In this example, before the Hastelloy X nickel-based high-temperature alloy subjected to hot isostatic pressing is subjected to solution treatment, a pre-insulation treatment is first performed. The specific operation of the pre-insulation treatment is to place the Hastelloy X nickel-based high-temperature alloy in a heat treatment furnace, heat it to 800° C. at a heating rate of 8° C. / min, and keep it at that temperature for 30 minutes.

[0085] In this example, before the Hastelloy X nickel-based high-temperature alloy formed by selective laser melting is subjected to hot isostatic pressing, the Hastelloy X nickel-based high-temperature alloy is first cleaned. The specific cleaning method is to slightly grind the six surfaces of the Hastelloy X nickel-based high-temperature alloy with sandpaper to remove the surface oxide film generated by natural aging, and then use an ultrasonic cleaning machine to vibrate for 20-30s to remove surface waste powder.

[0086] Figure 5: This is a scanning electron microscope image of the Hastelloy X nickel-based high-temperature alloy obtained in this comparative example. Figure 5 It can be seen that due to the increase in hot isostatic pressing temperature, the number of twin boundaries increases significantly, the grain boundaries become wider and deeper, and white precipitates appear at the grain boundaries, and there are also some unevenly distributed precipitates inside the grain boundaries. Twins, due to their specific orientation relationship, will hinder the movement of dislocations, thereby further improving the plasticity, and the elongation is increased by about 13% compared with Example 1, but the increase in the number of twins will be accompanied by the growth of recrystallized grains, and the proportion of large-angle grains will increase, thereby reducing the yield strength by about 20%.

[0087] Comparative Example 3

[0088] A method for preparing Hastelloy X nickel-based high-temperature alloy based on selective laser melting technology, the steps of which are as follows:

[0089] S1. Selective laser melting: A Hastelloy X nickel-based high-temperature alloy powder spread on a substrate is subjected to selective laser melting by a laser according to a preset scanning path to obtain a Hastelloy X nickel-based high-temperature alloy. The process parameters of the selective laser melting are: spot area 3.7 mm, layer thickness 40 μm, laser power 150 W, scanning speed 1050 mm / s, and scanning spacing 0.08 mm. The Hastelloy X nickel-based high-temperature alloy powder is composed of the following alloy elements according to mass percentage: W Cr =20.61%, W Mo =6.54%, W Fe =17.92%, W Co =1.41%, W w =0.64%, W Ni margin;

[0090] S2. Hot isostatic pressing: The Hastelloy X nickel-based high-temperature alloy formed by selective laser melting is placed in a hot isostatic pressing furnace, and the temperature is raised from room temperature to a hot isostatic pressing temperature of 1100°C at a rate of 8°C / min. The temperature is kept and pressurized for 130 minutes at a pressure of 150MPa. After the hot isostatic pressing, the Hastelloy X nickel-based high-temperature alloy is cooled to room temperature along with the furnace;

[0091] S3, solution treatment: placing the Hastelloy X nickel-based high-temperature alloy that has undergone hot isostatic pressing in a heat treatment furnace, heating it to a solution treatment temperature of 1120°C at a heating rate of 8°C / min, and keeping it warm for 120 minutes. After the solution treatment, the Hastelloy X nickel-based high-temperature alloy is air-cooled to room temperature;

[0092] S4, stress relief annealing treatment: the Hastelloy X nickel-based high-temperature alloy that has undergone solid solution treatment is subjected to stress relief annealing treatment; the stress relief annealing temperature is 740° C. and the time is 30 minutes;

[0093] The selective laser melting forming, hot isostatic pressing, solution treatment and stress relief annealing treatment are all carried out under the protection of argon atmosphere.

[0094] In the selective laser melting forming in step S1 of this example, the particle size distribution range of the Hastelloy X nickel-based high-temperature alloy powder is 15-53 μm, wherein D(10) is 21.77 μm, D(50) is 34.19 μm, D(90) is 53.0 μm, and D(95) is 61.20 μm.

[0095] In the selective laser melting molding in step S1 of this example, the scanning direction of each layer is rotated by 67° based on the printing direction of the previous layer.

[0096] In this example, before the Hastelloy X nickel-based high-temperature alloy subjected to hot isostatic pressing is subjected to solution treatment, a pre-insulation treatment is first performed. The specific operation of the pre-insulation treatment is to place the Hastelloy X nickel-based high-temperature alloy in a heat treatment furnace, heat it to 800° C. at a heating rate of 8° C. / min, and keep it at that temperature for 30 minutes.

[0097] In this example, before the Hastelloy X nickel-based high-temperature alloy formed by selective laser melting is subjected to hot isostatic pressing, the Hastelloy X nickel-based high-temperature alloy is first cleaned. The specific cleaning method is to slightly grind the six surfaces of the Hastelloy X nickel-based high-temperature alloy with sandpaper to remove the surface oxide film generated by natural aging, and then use an ultrasonic cleaning machine to vibrate for 20-30s to remove surface waste powder.

[0098] Figure 6 : This is a scanning electron microscope image of the Hastelloy X nickel-based high-temperature alloy obtained in this comparative example. Figure 6 It can be seen that, similar to comparative example 1, unevenly distributed precipitates are found at both the grain boundaries and within the grains, and the precipitates are scattered and scattered, with large differences in size. The presence of larger grains at the grain boundaries may cause stress concentration, and microcracks will preferentially initiate at these locations during the stretching process, thereby causing a reduction in mechanical properties.

[0099] The Hastelloy X nickel-based high-temperature alloys obtained in various embodiments and comparative examples were subjected to tensile tests, and the tensile results are shown in Table 1. From Table 1, it can be seen that the elongation after fracture of the embodiment 1 and the embodiment 3 is higher than that of the embodiment 2 because the grains have twins and the proportion of high-angle grain boundaries is relatively large, which enhances the hindering effect on dislocations. However, the grain size of the embodiment 2 is smaller than that of the embodiment 1 and the embodiment 3. According to the Hall-Petch formula, the larger the grain size, the smaller the yield strength. Therefore, its yield strength is stronger than that of the embodiment 1 and the embodiment 3. In addition, the embodiment 2 has more chain-like precipitated phases, which will also hinder the movement of dislocations during the tensile process, so that its tensile strength is also stronger. In comparative example 1, the scanning speed is fast, the layer thickness is wide and the solid solution temperature is high, so that the precipitated phase is distributed in blocks and cannot play a strengthening role. In comparative example 2, the hot isostatic pressing temperature is too high, resulting in a significant increase in the number of twin boundaries, resulting in a higher tensile strength. In comparative example 3, the stress relief annealing is low and the annealing time is long, resulting in the precipitated phase being distributed in blocks similar to comparative example 1. The difference is that the precipitated phase in comparative example 3 is smaller, so the effect on the mechanical properties is not as obvious as that in comparative example 1.

[0100] Table 1 Room temperature tensile properties of Hastelloy X nickel-based high temperature alloy obtained in the above examples and comparative examples

[0101]

[0102] Embodiment 4

[0103] A method for preparing Hastelloy X nickel-based high-temperature alloy based on selective laser melting technology, the steps of which are as follows:

[0104] S1. Selective laser melting: A Hastelloy X nickel-based high-temperature alloy powder spread on a substrate is subjected to selective laser melting by a laser according to a preset scanning path to obtain a Hastelloy X nickel-based high-temperature alloy. The process parameters of the selective laser melting are: spot area 2.5 mm, layer thickness 20 μm, laser power 150 W, scanning speed 1000 mm / s, and scanning spacing 0.07 mm. The Hastelloy X nickel-based high-temperature alloy powder is composed of the following alloy elements according to mass percentage: W Cr =20%, W Mo =6.5%, W Fe =17%, W Co =2.5%, W w =1.0%,W Ni margin;

[0105] S2. Hot isostatic pressing: The Hastelloy X nickel-based high-temperature alloy formed by selective laser melting is placed in a hot isostatic pressing furnace, and the temperature is raised from room temperature to a hot isostatic pressing temperature of 1130°C at a rate of 10°C / min. The temperature is kept and pressurized for 100 minutes at a pressure of 140 MPa. After the hot isostatic pressing, the Hastelloy X nickel-based high-temperature alloy is cooled to room temperature along with the furnace;

[0106] S3, solution treatment: placing the Hastelloy X nickel-based high-temperature alloy after hot isostatic pressing in a heat treatment furnace, heating it to a solution treatment temperature of 1130°C at a heating rate of 10°C / min, and keeping it warm for 125 minutes. After the solution treatment, the Hastelloy X nickel-based high-temperature alloy is air-cooled to room temperature;

[0107] S4, stress relief annealing treatment: the Hastelloy X nickel-based high-temperature alloy that has undergone solid solution treatment is subjected to stress relief annealing treatment; the stress relief annealing temperature is 770° C. and the time is 40 minutes;

[0108] The selective laser melting forming, hot isostatic pressing, solution treatment and stress relief annealing treatment are all carried out under the protection of argon atmosphere.

[0109] In the selective laser melting forming in step S1 of this example, the particle size distribution range of the Hastelloy X nickel-based high-temperature alloy powder is 15-53 μm, wherein D(10) is 21.77 μm, D(50) is 34.19 μm, D(90) is 53.0 μm, and D(95) is 61.20 μm.

[0110] In the selective laser melting molding in step S1 of this example, the scanning direction of each layer is rotated by 67° based on the printing direction of the previous layer.

[0111] In this example, before the Hastelloy X nickel-based high-temperature alloy subjected to hot isostatic pressing is subjected to solution treatment, a pre-insulation treatment is first performed. The specific operation of the pre-insulation treatment is to place the Hastelloy X nickel-based high-temperature alloy in a heat treatment furnace, heat it to 800° C. at a heating rate of 8° C. / min, and keep it at that temperature for 30 minutes.

[0112] In this example, before the Hastelloy X nickel-based high-temperature alloy formed by selective laser melting is subjected to hot isostatic pressing, the Hastelloy X nickel-based high-temperature alloy is first cleaned. The specific cleaning method is to slightly grind the six surfaces of the Hastelloy X nickel-based high-temperature alloy with sandpaper to remove the surface oxide film generated by natural aging, and then use an ultrasonic cleaning machine to vibrate for 20-30s to remove surface waste powder.

[0113] Embodiment 5

[0114] A method for preparing Hastelloy X nickel-based high-temperature alloy based on selective laser melting technology, the steps of which are as follows:

[0115] S1. Selective laser melting: A Hastelloy X nickel-based high-temperature alloy powder spread on a substrate is subjected to selective laser melting by a laser according to a preset scanning path to obtain a Hastelloy X nickel-based high-temperature alloy. The process parameters of the selective laser melting are: spot area 3.5 mm, layer thickness 35 μm, laser power 190 W, scanning speed 1100 mm / s, and scanning spacing 0.11 mm. The Hastelloy X nickel-based high-temperature alloy powder is composed of the following alloy elements according to mass percentage: W Cr =23%, W Mo =10%,W Fe =20%, W Co =0.5%, W w =0.2%, W Ni margin;

[0116] S2. Hot isostatic pressing: The Hastelloy X nickel-based high-temperature alloy formed by selective laser melting is placed in a hot isostatic pressing furnace, and the temperature is raised from room temperature to a hot isostatic pressing temperature of 1130°C at a rate of 9°C / min. The temperature is kept and pressurized for 140 minutes at a pressure of 160 MPa. After the hot isostatic pressing, the Hastelloy X nickel-based high-temperature alloy is cooled to room temperature along with the furnace;

[0117] S3, solution treatment: placing the Hastelloy X nickel-based high-temperature alloy after hot isostatic pressing in a heat treatment furnace, heating it to a solution treatment temperature of 1130°C at a heating rate of 9°C / min, and keeping it warm for 125 minutes. After the solution treatment, the Hastelloy X nickel-based high-temperature alloy is air-cooled to room temperature;

[0118] S4, stress relief annealing treatment: the Hastelloy X nickel-based high-temperature alloy that has undergone solid solution treatment is subjected to stress relief annealing treatment; the stress relief annealing temperature is 770° C. and the time is 40 minutes;

[0119] The selective laser melting forming, hot isostatic pressing, solution treatment and stress relief annealing treatment are all carried out under the protection of argon atmosphere.

[0120] In the selective laser melting forming in step S1 of this example, the particle size distribution range of the Hastelloy X nickel-based high-temperature alloy powder is 15-53 μm, wherein D(10) is 21.77 μm, D(50) is 34.19 μm, D(90) is 53.0 μm, and D(95) is 61.20 μm.

[0121] In the selective laser melting molding in step S1 of this example, the scanning direction of each layer is rotated by 67° based on the printing direction of the previous layer.

[0122] In this example, before the Hastelloy X nickel-based high-temperature alloy subjected to hot isostatic pressing is subjected to solution treatment, a pre-insulation treatment is first performed. The specific operation of the pre-insulation treatment is to place the Hastelloy X nickel-based high-temperature alloy in a heat treatment furnace, heat it to 800° C. at a heating rate of 8° C. / min, and keep it at that temperature for 30 minutes.

[0123] In this example, before the Hastelloy X nickel-based high-temperature alloy formed by selective laser melting is subjected to hot isostatic pressing, the Hastelloy X nickel-based high-temperature alloy is first cleaned. The specific cleaning method is to slightly grind the six surfaces of the Hastelloy X nickel-based high-temperature alloy with sandpaper to remove the surface oxide film generated by natural aging, and then use an ultrasonic cleaning machine to vibrate for 20-30s to remove surface waste powder.

Claims

1. A method for preparing Hastelloy X nickel-based high-temperature alloy based on selective laser melting technology, the steps of which are as follows: S1. Selective laser melting: The Hastelloy X nickel-based high-temperature alloy powder spread on the substrate is subjected to selective laser melting by a laser according to a preset scanning path to obtain the Hastelloy X nickel-based high-temperature alloy. The process parameters of the selective laser melting are: spot area 2.5-3.5 mm, layer thickness 20-35 μm, laser power 150-190 W, scanning speed 1000-1100 mm / s, scanning spacing 0.07-0.11 mm. The Hastelloy X nickel-based alloy powder is composed of the following alloy elements according to mass percentage: W Cr = 20.0% - 23.0%, W Mo = 6.5% - 10.0%, W Fe = 17.0% - 20.0%, W Co = 0.5% - 2.5%, W w = 0.2% - 1.0%, W Ni the balance; S2, hot isostatic pressing treatment: hot isostatic pressing treatment is performed on the Hastelloy X nickel-based high-temperature alloy formed by selective laser melting; the hot isostatic pressing treatment temperature is 1110° C.-1130° C., the time is 100-140 min, and the pressure is 140-160 MPa. After the hot isostatic pressing treatment, the Hastelloy X nickel-based high-temperature alloy is cooled to room temperature with the furnace; S3, solution treatment: subjecting the Hastelloy X nickel-based high-temperature alloy subjected to hot isostatic pressing to solution treatment; the solution treatment temperature is 1110° C.-1130° C., and the time is 115-125 min. After the solution treatment, the Hastelloy X nickel-based high-temperature alloy is air-cooled to room temperature; S4, stress relief annealing treatment: the Hastelloy X nickel-based high-temperature alloy that has undergone solid solution treatment is subjected to stress relief annealing treatment; the stress relief annealing temperature is 750° C.-770° C., and the time is 20-40 minutes; The selective laser melting forming, hot isostatic pressing, solution treatment and stress relief annealing treatment are all carried out under the protection of argon atmosphere.

2. The method for preparing Hastelloy X nickel-based high-temperature alloy based on selective laser melting technology according to claim 1, characterized in that: In the selective laser melting forming in step S1, the particle size distribution range of the Hastelloy X nickel-based high-temperature alloy powder is 15-53 μm, wherein D(10) is 21.77 μm, D(50) is 34.19 μm, D(90) is 53.0 μm, and D(95) is 61.20 μm.

3. The method for preparing Hastelloy X nickel-based high-temperature alloy based on selective laser melting technology according to claim 1, characterized in that: In the selective laser melting molding in step S1, the scanning direction of each layer is rotated by 67° based on the printing direction of the previous layer.

4. The method for preparing Hastelloy X nickel-based high-temperature alloy based on selective laser melting technology according to claim 1, characterized in that: The specific operation of the hot isostatic pressing treatment is to place the HastelloyX nickel-based high-temperature alloy formed by selective laser melting in a hot isostatic pressing furnace, heat it from room temperature to the hot isostatic pressing treatment temperature at a rate of 8-10°C / min, keep it warm and pressurize it, and the holding time is the hot isostatic pressing treatment time.

5. The method for preparing Hastelloy X nickel-based high-temperature alloy based on selective laser melting technology according to claim 1, characterized in that: The specific operation of the solution treatment is to place the Hastelloy X nickel-based high-temperature alloy that has undergone hot isostatic pressing in a heat treatment furnace, heat it to the solution treatment temperature at a heating rate of 8°C / min-10°C / min, and keep it warm. The insulation time is the solution treatment time.

6. The method for preparing Hastelloy X nickel-based high-temperature alloy based on selective laser melting technology according to claim 1 or 5, characterized in that: Before the Hastelloy X nickel-based high-temperature alloy subjected to hot isostatic pressing is subjected to solution treatment, a pre-insulation treatment is first performed. The specific operation of the pre-insulation treatment is to place the Hastelloy X nickel-based high-temperature alloy in a heat treatment furnace, heat it to 800° C. at a heating rate of 8° C. / min, and keep it warm for 30 minutes.

7. The method for preparing Hastelloy X nickel-based high-temperature alloy based on selective laser melting technology according to claim 1, characterized in that: Before the selective laser melting-molded Hastelloy X nickel-based high-temperature alloy is subjected to hot isostatic pressing, the Hastelloy X nickel-based high-temperature alloy is first cleaned. Specifically, the six surfaces of the Hastelloy X nickel-based high-temperature alloy are slightly polished with sandpaper to remove the surface oxide film generated by natural aging, and then the surface waste powder is removed by vibrating with an ultrasonic cleaner for 20-30 seconds.