Welding method for automatic flat welding of narrow groove of thick plate of ship
By combining the V-shaped narrow groove automatic flat welding method with flux-cored wire, the problems of multiple weld passes, stress concentration and precision in ship thick plate welding are solved, efficient and stable welding quality is achieved, and labor intensity and material consumption are reduced. Suitable for narrow gap welding of thick plates on large ships.
Patent Information
- Application Number
- CN202411100749.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-10-01
AI Technical Summary
The existing ship thick plate welding technology has many welding bead filling layers, stress concentration, and the interlayer temperature drops too quickly, resulting in high risk of cracks, low efficiency, high labor intensity, and cannot meet the accuracy requirements of narrow gap welding grooves. Especially in the crack arresting steel structure of large ships, there is a lack of matching solid welding wire.
Adopt V-shaped narrow groove automatic flat welding method, use flux-cored welding wire that matches the thick plate base material, conduct carbon dioxide gas shielded welding through predetermined welding parameters, set ceramic liners, use rotating arc and DC positive polarity welding, and control the interlayer temperature and welding speed, reducing the number of weld passes and improving molten pool stability, combined with magnetic particle and ultrasonic testing to ensure welding quality.
It improves welding efficiency, reduces labor intensity and material consumption, shortens the construction cycle, improves welding quality and precision, meets the needs of narrow gap welding of thick plates on large ships, and reduces the number of welding passes and the risk of cracks.
Smart Images

Figure CN118720341A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of shipbuilding, and in particular to a welding method for automatic flat welding of narrow grooves of thick plates of ships. Background Art
[0002] With the development of large-scale ships, 20,000-TEU container ships have become one of the mainstream products in the current ship market. The thickness of the high-strength steel thick plate EH47 / EH40 and high-strength crack arrest steel EH47CAS / EH40CAS of the torsion box of the box ship is 50-95mm, and its structural weight accounts for 12.5% of the total ship structure weight. This structure is the most critical force-bearing structure on the container ship, and the hatch coaming structure in the torsion box area is the area with the most concentrated structural stress distribution. The hatch coaming structure is made of thick high-strength steel and crack arrest steel, with the thickest plate thickness up to 100mm.
[0003] The welding method for thick plates in the assembly or loading stage is still mainly conventional welding methods such as mixed welding of carbon dioxide semi-automatic and carbon dioxide fully automatic welding. Figure 1 and Figure 2 As shown in the figure, the groove angle is 40-45°, so there are many weld fill layers, welding stress concentration, and too fast interlayer temperature drop, which increases the risk of weld cracks. In addition, carbon dioxide welding has low efficiency, large smoke and dust, and the welding quality is greatly affected by human factors.
[0004] At present, the thick plates of hatch coamings are welded by semi-automatic carbon dioxide welding. For welding operations with a plate thickness of 95mm and a weld length of 1 meter, one welder needs to weld for 2 to 3 days. There are problems such as high worker input, long welding cycle, high labor intensity and low efficiency.
[0005] In the prior art, narrow gap welding is used for welding thick plates. When performing narrow gap welding, the groove needs to adopt a U-shaped groove, such as Figure 3 As shown, the U-shaped groove processing is complex and requires many parameters to be set, so machining methods are required to meet the requirements. When welding thick plates in the assembly or loading stage of ship construction, the existing cutting and processing equipment cannot meet its requirements and cannot process U-shaped grooves. In addition, the assembly accuracy requirements are relatively stringent. The torsion box welding is in the stage of closing large sections of tens of tons. The assembly deviation is large and cannot meet the conventional narrow gap welding groove accuracy requirements. In addition, the conventional narrow gap welding uses solid welding wire. For large ships, especially crack arresting steel, the welding wire quality requirements are stable and crack resistance has crack resistance index requirements. At present, there is no matching solid welding wire for crack arresting steel on the market.
[0006] In summary, it is necessary to provide an improved technical solution to address the above-mentioned deficiencies in the prior art. Summary of the invention
[0007] The purpose of the embodiments of the present application is to provide a welding method for automatic flat welding of narrow grooves of thick plates for ships, which can complete narrow gap welding of thick plates under the premise of simple groove processing procedures.
[0008] The present application provides a method for automatic flat welding of a thick plate with a narrow groove, comprising the following steps:
[0009] S1. Cut the thick plate to a predetermined size and process the groove, wherein the root gap of the groove is 8-12 mm and the angle of the groove is 20-25°;
[0010] S2. Select a flux-cored welding wire that matches the thick plate base material as the welding material, and the diameter of the welding material is 1.2-1.4 mm;
[0011] S3. Welding thick plates according to predetermined welding parameters;
[0012] S4. Perform nondestructive testing after welding to ensure that the weld meets the welding requirements.
[0013] In one practicable manner, in step S3, at least the following contents are included:
[0014] S31, assembling an arc striking and extinguishing plate before welding, wherein the thickness and material of the arc striking and extinguishing plate are set corresponding to the thick plate base material, and the arc striking and extinguishing plate is set flush with the thick plate base material without a gap;
[0015] S32, preheating the thick plate base material to 100°C-120°C;
[0016] S33. The thick plate base material is welded by using carbon dioxide gas shielded welding according to predetermined welding parameters.
[0017] In one practicable manner, in step S33, at least the following contents are included:
[0018] When performing the first pass of backing welding, a rotating arc is used for welding, with a current of 190-210A, a voltage of 24-26V, a welding speed of 10-12cm / min, an arc left rotation angle of 25°-40°, an arc right rotation angle of 25°-40°, a rotation speed of 60-100r / min, a dwell time of 0.2S on each side, and a maximum wire swing width of 16mm;
[0019] When performing the second pass of backing welding, a rotating arc is used for welding, with a current of 190-210A, a voltage of 24-26V, a welding speed of 14-18cm / min, an arc left rotation angle of 25°-40°, an arc right rotation angle of 25°-40°, a rotation speed of 60-100r / min, a dwell time of 0.2S on each side, and a maximum wire swing width of 16mm;
[0020] From the third weld pass to the completion of the cap weld, the arc does not rotate or swing, the current is 220-240A, the voltage is 24-26V, and the welding speed is 25-40cm / min.
[0021] In one practicable manner, the carbon dioxide gas flow rate is 15-25 L / min, and the welding wire extension is 15-20 mm.
[0022] In one practicable manner, in step S33, a ceramic liner is provided on the reverse side of the groove, and positive current polarity is used for front welding, and multi-layer and multi-pass welding is used for the front welding.
[0023] In one practicable manner, when performing multi-layer and multi-pass welding, the interlayer temperature T should be controlled as follows: preheating temperature < T ≤ 200° C., and welding slag needs to be cleaned for each layer and each weld pass.
[0024] In an practicable manner, when the thickness of the thick plate base material is 80 mm and the material is EH47 crack-arresting steel, the length of the arc-extinguishing plate is greater than or equal to 150 mm, and the width is greater than or equal to 50 mm.
[0025] In an practicable manner, before step S31, the following contents are also included: grinding the inner surface and the outer surface of the groove with a grinding wheel.
[0026] In an practicable manner, in step S32, the following contents are also included: during the preheating process, a trolley is used to perform an idle travel to ensure that the welding path is accurate.
[0027] In one practicable manner, in step S4, the nondestructive testing at least includes magnetic particle testing and ultrasonic testing.
[0028] Compared with the prior art, the beneficial effects of this application are:
[0029] In the technical solution of the present application, narrow gap welding of thick plates is completed by setting a V-shaped narrow groove. The processing of the V-shaped groove is simple and easy to operate, which can reduce the workload of groove processing. By performing narrow gap welding on thick plates, the problem of side wall fusion of single-pass filling welding of large gap grooves is solved. By matching flux-cored wire as welding material, the problems of side wall fusion and molten pool stability are solved to ensure welding quality. By setting predetermined welding parameters for welding, the number of welds and the risk of weld cracks are reduced, and the problems of excessive weld filling, stress concentration, unstable welding quality, etc. in the prior art of carbon dioxide semi-automatic welding are solved. By setting a ceramic liner, single-sided welding and double-sided forming of narrow grooves can be achieved. The present application can improve production efficiency, save materials and energy, improve working conditions, reduce labor intensity, shorten the construction period of general assemblies and slipways, and facilitate promotion and use. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a structural schematic diagram of a V-shaped groove in the prior art.
[0031] Figure 2 It is a structural schematic diagram of a weld in the prior art.
[0032] Figure 3 It is a structural schematic diagram of a U-shaped groove in the prior art.
[0033] Figure 4 The present invention is a flow chart of a welding method for automatic flat welding of narrow grooves of thick plates for ships according to an embodiment of the present invention.
[0034] Figure 5 The invention is a schematic structural diagram of a groove in a welding method for automatic flat welding of a narrow groove of a thick ship plate according to an embodiment of the present invention.
[0035] Figure 6 The present invention is a schematic structural diagram of a weld bead in a welding method for automatic flat welding of a narrow groove of a thick ship plate according to an embodiment of the present invention.
[0036] Figure 7 It is a macroscopic metallographic diagram of a weld in a welding method for automatic flat welding of a ship thick plate with a narrow groove according to an embodiment of the present invention.
[0037] Figure 8 It is a schematic diagram of the number of welding passes in traditional gas shielded welding.
[0038] Fig. 9 The present invention is a schematic diagram of the number of welding passes in the welding method for automatic flat welding of narrow grooves of thick plates for ships according to an embodiment of the present invention.
[0039] Fig.10 The figure is a comparison chart of welding efficiency between the welding method for automatic flat welding of narrow groove of thick ship plate in an embodiment of the present invention and the conventional gas shielded welding.
[0040] Fig.11 The figure is a comparison chart of welding material consumption in the welding method for automatic flat welding of narrow groove of thick plate of ship in an embodiment of the present invention and that in conventional gas shielded welding. DETAILED DESCRIPTION
[0041] The specific embodiments of the present invention are further described in detail below in conjunction with the accompanying drawings. These embodiments are only used to illustrate the present invention, but not to limit the present invention.
[0042] In the description of the present invention, it should be noted that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.
[0043] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0044] Furthermore, in the description of the present invention, unless otherwise specified, “plurality” means two or more.
[0045] See also Figures 4 to 6 The present application provides a method for automatic flat welding of narrow grooves of thick plates for ships, comprising the following steps:
[0046] S1. Cut the thick plate to a predetermined size and process the groove. The root gap C of the groove is 8-12mm, leaving no root, which is convenient for slag removal, ensuring welding quality, improving production efficiency and saving welding materials. The groove angle α is 20-25°, such as Figure 5 shown.
[0047] S2. Matching welding materials. The welding materials are flux-cored wires that match the thick plate base material. The diameter of the welding materials is 1.2-1.4 mm. They have excellent welding performance and good crack sensitivity resistance.
[0048] S3. Weld the thick plate according to the predetermined welding parameters.
[0049] In one practicable manner, in step S3, at least the following contents are included:
[0050] S31. Assemble an arc striking and extinguishing plate before welding. The thickness and material of the arc striking and extinguishing plate are set corresponding to the thick plate base material. The arc striking and extinguishing plate is set flush with the thick plate base material without a gap.
[0051] Specifically, in this embodiment, when the thickness t of the thick plate base material is 80 mm and the material is EH47 crack-arresting steel, the length of the arc-extinguishing plate is greater than or equal to 150 mm, and the width of the arc-extinguishing plate is greater than or equal to 50 mm.
[0052] In one practicable manner, step S31 also includes the following: before welding, the inner surface and the outer surface of the groove are ground with a grinding wheel to remove oil, rust, scale and other substances harmful to welding on and near the groove.
[0053] It should be noted that when grinding the outer surface of the groove, ensure that the groove and the outer surface within 20mm outside are ground clean.
[0054] S32. Preheat the thick plate base material to 100°C-120°C.
[0055] It should be noted that during the preheating process, the trolley is used for idling travel to ensure that the welding path is accurate and to avoid biased welding during formal welding.
[0056] S33. The thick plate base material is welded by using carbon dioxide gas shielded welding according to predetermined welding parameters.
[0057] Specifically, a special welding machine of model NJUST-NG-001 and a flat gun head are used for automatic flat welding with oxygen shielding gas. Before welding, a ceramic liner is set on the reverse side of the groove to achieve single-sided welding and double-sided forming.
[0058] In this embodiment, the positive polarity of the current is used for front welding, and the front welding adopts multi-layer multi-pass welding. The weld bead arrangement is as follows: Figure 6 During the welding process, the predetermined welding parameters include at least:
[0059] When performing the first pass of backing welding, a rotating arc is used for welding, with a current of 190-210A, a voltage of 24-26V, a welding speed of 10-12cm / min, an arc left rotation angle of 25°-40°, an arc right rotation angle of 25°-40°, a rotation speed of 60-100r / min, a dwell time of 0.2S on each side, and a maximum wire swing width of 16mm;
[0060] When performing the second pass of backing welding, a rotating arc is used for welding, with a current of 190-210A, a voltage of 24-26V, a welding speed of 14-18cm / min, an arc left rotation angle of 25°-40°, an arc right rotation angle of 25°-40°, a rotation speed of 60-100r / min, a dwell time of 0.2S on each side, and a maximum wire swing width of 16mm;
[0061] From the third weld pass to the completion of the cap weld, the arc does not rotate or swing, the current is 220-240A, the voltage is 24-26V, and the welding speed is 25-40cm / min.
[0062] In one practicable manner, during welding, the carbon dioxide gas flow rate is 15-25 L / min, and the welding wire is extended by 15-20 mm.
[0063] It should be noted that during the welding process, the interlayer temperature T is controlled as follows: preheating temperature < T ≤ 200°C, and welding slag is cleaned for each layer and each pass.
[0064] S4. Perform nondestructive testing after welding to ensure that the weld meets the welding requirements.
[0065] Specifically, non-destructive testing is performed 48 hours after welding is completed, and the non-destructive testing at least includes magnetic particle testing and ultrasonic testing.
[0066] The test results of magnetic particle testing must meet the ISO-23278 qualification level; the test results of ultrasonic testing must meet the ISO-11666 qualification level.
[0067] The weld seam welded by the welding method provided in this embodiment is well-formed, with a smooth and clean overall appearance. The final test result of the weld seam surface through magnetic particle testing meets the ISO-23278 2X grade; the test result of the internal ultrasonic testing of the weld seam meets the ISO-11666 2X grade. The joint tensile and bending tests are qualified, and the macroscopic metallographic inspection of the weld seam is as follows. Figure 7 As shown in the figure, no defects such as lack of fusion, pores, inclusions, etc. were found in the heat affected zone. The low temperature -20℃ impact test meets the requirements of classification society regulations, and the Vickers hardness HV10 test value ≤350 meets the requirements.
[0068] This application effectively improves the welding quality of thick high-strength crack arrest steel in the 50-100mm torsion box area of large box ships, reduces the number of welding layers and passes, and takes a thick plate with a thickness of 80mm as an example to compare the number of welding passes. The comparison results of the number of welding passes are as follows: Figure 8 and Fig. 9 As shown, the welding deformation can be reduced due to the reduction in the number of welding passes.
[0069] This application applies narrow groove welding to the flat butt weld of the thick plate of the torsion box in the overall assembly or loading stage of the hull structure, which can increase the welding efficiency by 30% and save 40% of the welding material cost. The comparison results of welding efficiency are as follows: Fig.10 As shown, the comparative structure of welding material consumption is as follows Fig.11 shown.
[0070] In summary, the present application completes the narrow gap welding of thick plates by setting a V-shaped narrow groove. The processing of the V-shaped groove is simple and easy to operate, which can reduce the workload of groove processing. By performing narrow gap welding on thick plates, the side wall fusion problem of single-pass filling welding of large gap grooves is solved. By matching flux-cored wire as the welding material, the side wall fusion and molten pool stability problems are solved to ensure the welding quality. By setting predetermined welding parameters for welding, the number of welds and the risk of weld cracks are reduced, and the problems of excessive weld filling, stress concentration, unstable welding quality, etc. in the prior art of carbon dioxide semi-automatic welding are solved. By setting a ceramic liner, single-sided welding and double-sided forming of narrow grooves can be achieved. The present application can improve production efficiency, save materials and energy, and can also improve working conditions, reduce labor intensity, shorten the construction period of general assemblies and slipways, and facilitate promotion and use.
[0071] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and substitutions can be made without departing from the technical principles of the present invention. These improvements and substitutions should also be regarded as the scope of protection of the present invention.
Claims
1. A welding method for automatic flat welding of narrow grooves of thick ship plates, characterized in that: The following steps are involved: S1. Cut the thick plate to a predetermined size and process the groove, wherein the root gap of the groove is 8-12 mm and the angle of the groove is 20-25°; S2. Select a flux-cored welding wire that matches the thick plate base material as the welding material, and the diameter of the welding material is 1.2-1.4 mm; S3. Welding thick plates according to predetermined welding parameters; S4. Perform nondestructive testing after welding to ensure that the weld meets the welding requirements.
2. The welding method for automatic flat welding of ship thick plate narrow groove according to claim 1 is characterized in that: In step S3, at least the following contents are included: S31, assembling an arc striking and extinguishing plate before welding, wherein the thickness and material of the arc striking and extinguishing plate are set corresponding to the thick plate base material, and the arc striking and extinguishing plate is set flush with the thick plate base material without a gap; S32, preheating the thick plate base material to 100°C-120°C; S33. The thick plate base material is welded by using carbon dioxide gas shielded welding according to predetermined welding parameters.
3. The welding method for automatic flat welding of ship thick plate narrow groove according to claim 2 is characterized in that: In step S33, at least the following contents are included: When performing the first pass of backing welding, a rotating arc is used for welding, with a current of 190-210A, a voltage of 24-26V, a welding speed of 10-12cm / min, an arc left rotation angle of 25°-40°, an arc right rotation angle of 25°-40°, a rotation speed of 60-100r / min, a dwell time of 0.2S on each side, and a maximum wire swing width of 16mm; When performing the second pass of backing welding, a rotating arc is used for welding, with a current of 190-210A, a voltage of 24-26V, a welding speed of 14-18cm / min, an arc left rotation angle of 25°-40°, an arc right rotation angle of 25°-40°, a rotation speed of 60-100r / min, a dwell time of 0.2S on each side, and a maximum wire swing width of 16mm; From the third weld pass to the completion of the cap weld, the arc does not rotate or swing, the current is 220-240A, the voltage is 24-26V, and the welding speed is 25-40cm / min.
4. The welding method for automatic flat welding of narrow groove of thick ship plate according to claim 3 is characterized in that: The carbon dioxide gas flow rate is 15-25L / min, and the welding wire extension is 15-20mm.
5. The welding method for automatic flat welding of ship thick plate narrow groove according to claim 1 is characterized in that: In step S33, a ceramic liner is arranged on the reverse side of the groove, and positive current polarity is used for front welding, and multi-layer and multi-pass welding is used for the front welding.
6. The welding method for automatic flat welding of ship thick plate narrow groove according to claim 5 is characterized in that: When performing multi-layer and multi-pass welding, the interlayer temperature T should be controlled as follows: preheating temperature <T≤200℃, and the welding slag must be cleaned for each layer and each weld pass.
7. The welding method for automatic flat welding of ship thick plate narrow groove according to claim 2 is characterized in that: When the thickness of the thick plate base material is 80 mm and the material is EH47 crack-arresting steel, the length of the arc-extinguishing plate is greater than or equal to 150 mm, and the width of the arc-extinguishing plate is greater than or equal to 50 mm.
8. The welding method for automatic flat welding of ship thick plate narrow groove according to claim 2 is characterized in that: Before step S31, the following contents are also included: grinding the inner surface and the outer surface of the groove with a grinding wheel.
9. The welding method for automatic flat welding of ship thick plate narrow groove according to claim 2 is characterized in that: In step S32, the following contents are also included: during the preheating process, the trolley is used to perform an idle travel to ensure that the welding path is accurate.
10. The welding method for automatic flat welding of ship thick plate narrow groove according to claim 1, characterized in that: In step S4, the nondestructive testing at least includes magnetic particle testing and ultrasonic testing.
Citation Information
Cited By
Single-side welding process for processing marine sanitary unit
CN120715459A
Turnover-free tailor-welding process for thick plate U-shaped groove of offshore wind power barrel-shaped structure
CN122787532A