Manual electric arc welding butt joint method suitable for 800MPa-grade high-strength steel plate

Through the manual arc welding butt method, including steel plate surface treatment, welding groove forming and pre-welding preheating, the problem of poor welding performance of 800MPa high-strength steel plates is solved, high-quality welding at the construction site is achieved, and the technical requirements of hydropower projects are met. .

CN118720358APending Publication Date: 2024-10-01BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410935632.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The welding performance of 800MPa-grade high-strength steel plates is poor, especially at construction sites where the environment is harsh and large-scale welding equipment is not easily equipped, making it difficult to achieve high-quality welding work.

Method used

The manual arc welding butt method is used, including steel plate surface pretreatment, welding groove processing and shaping, pre-welding preheating and welding. JQ.J807SD high-strength steel electrode is used to control the current, voltage, welding speed and post-heating system to ensure that the welding process is The mechanical properties and process performance meet the requirements of hydropower engineering.

Benefits of technology

The tensile strength of the steel plate after welding is not reduced, the low-temperature impact toughness is excellent, and the cold formability is good. It is suitable for high-quality welding at hydropower project construction sites, and the operation is simple and does not require large equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720358A_ABST
    Figure CN118720358A_ABST
Patent Text Reader

Abstract

The invention discloses a manual electric arc welding butt joint method suitable for 800MPa-grade high-strength steel plates, which comprises the following operation steps of steel plate surface pretreatment, steel plate welding groove processing and forming, steel plate pre-welding preheating treatment and welding, and in the welding step, the current is controlled to be 140-160A; the voltage is 22 to 25V; the welding speed ranges from 80 mm / min to 150 mm / min; the temperature between the channels is 100-200 DEG C; and the post-heating system is kept at 150-200 DEG C for more than 2 hours, so that the good post-welding mechanical property and process property of the steel plate can be ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of welding of low alloy high strength steel plates, and specifically relates to a manual arc welding butt joint method applicable to 800MPa grade high strength steel plates, and in particular to a manual arc welding butt joint method applicable to 800MPa grade high strength steel plates with a thickness of 10-60mm which is easy to implement on construction sites. Background Art

[0002] The construction of pumped storage power stations has led to an increase in the demand for 800MPa-grade high-strength hydropower steel, which is mainly used for the production of hydropower engineering pressure steel pipes, volutes, bifurcated pipes and other components. The steel plates are welded after rolling. As the installed capacity and head design of hydropower projects become larger and larger, the amount of 800MPa-grade high-strength steel plates used in hydropower projects is extremely large, and the welding workload has increased sharply. In particular, the welding environment at the construction site is worse than that at the factory workshop, and it is not easy to carry out welding methods that require large or large amounts of welding equipment. The composition design of 800MPa-grade steel plates for hydropower projects generally adopts low carbon + nickel-chromium-molybdenum-niobium-vanadium-titanium alloying, which makes the carbon equivalent (carbon equivalent CEV = C + Mn / 6 + (Cr + Mo + V) / 5 + (Ni + Cu) / 15) higher and the material weldability is poor. Therefore, it is necessary to develop a welding method for 800MPa-grade high-strength steel plates that is easy to implement at the construction site. Summary of the invention

[0003] The steel plate targeted by the present invention has high strength (tensile strength ≥ 800MPa) and large carbon equivalent (CEV can reach 0.52%), but poor welding performance (preheating treatment is required). At the same time, in order to facilitate the welding work on the construction site, a manual arc welding butt joint method suitable for 10-60mm thick 800MPa high-strength steel plates that is easy to implement on the construction site is invented and developed. The manual arc welding butt joint method provided by the present invention can ensure that the steel plate has good post-weld mechanical properties and process properties, the tensile strength of the steel plate after welding is not reduced, the low-temperature impact toughness of the weld and the heat-affected zone is excellent, and the cold formability is excellent, etc., and can be stably applied to welding on the construction site of hydropower projects.

[0004] The present invention is achieved through the following technical solutions.

[0005] The present invention provides a manual arc welding butt joint method applicable to 800MPa grade high-strength steel plates, which comprises the following operating steps: steel plate surface pretreatment - steel plate welding groove processing and forming - steel plate preheating treatment before welding - welding; wherein:

[0006] In the steel plate surface pretreatment step, before manual arc welding, various dirt and defects on the steel plate surface are deeply cleaned until they are invisible to the naked eye or the steel plate reveals metallic luster;

[0007] In the steel plate welding groove processing and forming step, an asymmetric X-shaped groove is processed according to standard technical requirements, and a blunt edge of 2-5 mm is reserved;

[0008] In the preheating treatment step before welding the steel plate, the preheating temperature is controlled to be ≥100°C, the preheating range is more than 100mm on each side of the weld, and the temperature is measured within a range of 30-50mm from the weld;

[0009] In the welding step, the welding material used is JQ.J807SD high-strength steel electrode with a specification of Ф4.0mm, and the following process parameters are controlled:

[0010] Current: 140-160A; Voltage: 22-25V; Welding speed: 80-150mm / min;

[0011] Interpass temperature 100-200°C; and

[0012] Post-heating system: 150-200℃ for more than 2 hours.

[0013] In some embodiments, the thickness specification of the 800 MPa grade high-strength steel plate is 10-60 mm.

[0014] In some embodiments, the chemical composition of the 800 MPa grade high-strength steel plate is calculated by mass percentage as follows: C≤0.10%, Si≤0.30%, Mn≤1.70%, P≤0.010%, S≤0.004%, Als: 0.020%~0.035%, Nb≤0.050%, Ti≤0.030%, V≤0.050%, Cr≤0.70%, Mo≤0.70%, Ni≤1.5%, Cu≤0.30%, B≤0.0020%, and the rest is Fe and unavoidable impurities.

[0015] In some embodiments, the chemical composition of the 800 MPa grade high-strength steel plate is calculated by mass percentage as follows: C: 0.07% to 0.09%, Si: 0.10% to 0.30%, Mn: 1.20% to 1.60%, P≤0.010%, S≤0.004%, Als: 0.020% to 0.035%, Nb: 0.030% to 0.050%, Ti: 0.015% to 0.030%, V: 0.030% to 0.050%, Cr≤0.70%, Mo≤0.70%, Ni: 0.70 to 1.5%, Cu≤0.30%, B≤0.0020%, and the rest is Fe and unavoidable impurities.

[0016] In some embodiments, the chemical composition of the 800 MPa grade high-strength steel plate is calculated by mass percentage as follows: C: 0.076% to 0.089%, Si: 0.19% to 0.23%, Mn: 1.31% to 1.37%, P≤0.010%, S≤0.004%, Als: 0.024% to 0.030%, Nb: 0.040% to 0.045%, Ti: 0.017% to 0.020%, V: 0.039% to 0.045%, Cr: 0.41 to 0.45%, Mo: 0.37 to 0.42%, Ni: 0.84 to 0.89%, Cu: 0.20 to 0.22%, B: 0 to 0.0014%, and the rest is Fe and unavoidable impurities.

[0017] In some embodiments, the steel plate surface pretreatment step includes: (1) wiping surface defects such as oil, moisture, dirt, etc. with alcohol; (2) grinding near-surface defects such as rust, iron oxide, fine cracks, etc. with an angle grinder.

[0018] In some embodiments, the manual arc welding butt welding method further includes observation and analysis of the metallographic structure of the weld and the heat affected zone after welding, and detection of mechanical properties and process properties.

[0019] In some embodiments, in the step of preheating the steel plate before welding, a flame spray gun is used to preheat the steel plate before welding, or a box-type resistance furnace is used to preheat the steel plate before welding.

[0020] The beneficial effects of the present invention are as follows: by selecting suitable welding materials and matching the best welding process parameters, especially controlling welding process parameters such as current, voltage, welding speed, interpass temperature and post-heating system, the present invention can ensure that the mechanical properties and process properties of the material after welding meet the technical requirements of steel plates for hydropower engineering, and provide data support for welding work at the construction site. At the same time, the method of the present invention is simple to operate and can be implemented at the construction site without the need for large or large amounts of welding equipment. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Schematic diagram of the welding groove (a) and welding pass arrangement (b) of Example 3 of the present invention.

[0022] Figure 2 These are metallographic structure photos of the weld and heat-affected zone of Example 3 of the present invention, wherein a represents the weld metallographic structure, b represents the overheating zone metallographic structure, c represents the normalizing zone metallographic structure, and d represents the incomplete normalizing zone structure. DETAILED DESCRIPTION

[0023] The present invention will be further described in detail below with reference to specific examples. The examples are merely descriptions of the best mode for carrying out the present invention and do not limit the scope of the present invention in any way.

[0024] The present invention provides a manual arc welding butt joint method suitable for 800MPa grade high-strength steel plates, which comprises the following operation steps: steel plate surface pretreatment - steel plate welding groove processing and forming - steel plate preheating treatment before welding - welding; wherein

[0025] Steel plate surface pretreatment: Before manual arc welding, all dirt and defects on the steel plate surface should be cleaned up until they are no longer visible to the naked eye or the steel plate reveals its metallic luster; specifically: (1) Surface defects such as oil, water, dirt, etc. should be wiped with alcohol; (2) Near-surface defects such as rust, iron oxide, fine cracks, etc. can be polished with an angle grinder;

[0026] Steel plate welding groove processing and forming: Processing asymmetric X-shaped groove according to standard technical requirements, leaving a blunt edge of 2-5mm; exemplary (the following embodiment 3) welding groove such as Figure 1 As shown in panel a;

[0027] Preheating of steel plate before welding: control the preheating temperature to ≥100℃, the preheating range is more than 100mm on each side of the weld, and the temperature is measured within 30-50mm from the weld; the steel plate can be preheated by a flame spray gun, or by a box-type resistance furnace to achieve the effect of preheating the steel plate;

[0028] Welding: The welding material used is JQ.J807SD high-strength steel electrode with a specification of Ф4.0mm, and the following process parameters are controlled:

[0029] Current: 140-160A; Voltage: 22-25V; Welding speed: 80-150mm / min;

[0030] Interpass temperature 100-200°C; and

[0031] The post-heating system is 150-200°C for more than 2 hours; the exemplary (the following embodiment 3) welding pass arrangement schematic diagram is as follows Figure 1 As shown in panel b.

[0032] In addition, the manual arc welding butt-jointing method for 800MPa grade high-strength steel plates provided by the present invention may also include observing and analyzing the metallographic structure of the weld and the heat-affected zone after welding, and testing the mechanical properties and process performance; specifically, conducting tensile tests, cold bending tests, hardness tests and weld metallographic structure observations according to standard sampling.

[0033] The chemical composition and content of the 800 MPa grade high strength steel plate in the following Examples 1-5 are shown in Table 1 below.

[0034] Table 1: Chemical composition (wt%) of 800 MPa grade high strength steel plates for Examples 1-5 of the present invention

[0035] Example C Si Mn P S Als Nb Ti V Cr Mo Ni Cu B 1 0.076 0.23 1.33 0.010 0.002 0.030 0.042 0.020 0.045 0.42 0.37 0.84 0.21 0.00 2 0.078 0.20 1.31 0.008 0.003 0.025 0.042 0.019 0.045 0.44 0.37 0.87 0.20 0.00 3 0.080 0.19 1.36 0.009 0.001 0.026 0.044 0.020 0.045 0.41 0.42 0.89 0.22 0.00 4 0.087 0.20 1.33 0.008 0.001 0.025 0.045 0.017 0.040 0.45 0.40 0.85 0.20 0.0010 5 0.089 0.19 1.37 0.009 0.002 0.024 0.040 0.019 0.039 0.44 0.38 0.84 0.20 0.0014

[0036] The specific welding process parameters in the following Examples 1-5 and Comparative Example 1 are shown in Table 2. The only difference between Comparative Example 1 and Example 3 is the welding speed.

[0037] Table 2: Welding process parameters of Examples 1-5 and Comparative Example 1

[0038]

[0039] The metallographic structures of the welds and heat-affected zones obtained by the manual arc welding butt welding methods of Examples 1-5 and Comparative Example 1 were observed and analyzed, and the mechanical properties and process performance were tested. The results are as follows: Figure 2 As shown, the metallographic structure photos of the weld and the heat affected zone obtained by the manual arc welding butt method of Example 3 are exemplified, wherein a represents the metallographic structure of the weld, b represents the metallographic structure of the overheating zone, c represents the metallographic structure of the normalizing zone, and d represents the metallographic structure of the incomplete normalizing zone. The results show that the metallographic structures of the weld, overheating zone, normalizing zone and incomplete normalizing zone are normal, without abnormal structures, which conforms to the changes in the weld heat affected zone structure in metal materials science, and is consistent with the hardness test results in Table 3 and the mechanical properties and process performance results in Table 4. Table 3 below shows the results of the hardness value of the welding heat affected zone, and Table 4 below shows the results of the mechanical properties and process properties of the steel plate after welding, indicating that the mechanical properties and process properties of the weld and heat affected zone obtained by the manual arc welding butt method of Examples 1-5 meet the technical requirements of hydropower engineering, while the hardness value of the weld heat affected zone obtained by the manual arc welding butt method of Comparative Example 1 fails to meet the standard requirements in 4 of 15 measurements (accounting for 27%), and the results of the -40°C impact energy detection of the weld and heat affected zone obtained by the manual arc welding butt method of Comparative Example 1 can meet the standard requirements, but are significantly lower than Example 3. The above results show that the use of a higher welding speed in Comparative Example 1 will affect the mechanical properties and process properties after welding, and cause the hardness value of the weld heat affected zone to fail to meet the standard requirements.

[0040] Table 3: Hardness values ​​of weld heat affected zone

[0041]

[0042] Table 4: Mechanical properties and process properties after welding

[0043]

[0044] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A manual arc welding butt welding method suitable for 800MPa grade high-strength steel plates, comprising the following steps: steel plate surface pretreatment - steel plate welding groove processing and forming - steel plate preheating treatment before welding - welding; wherein: In the steel plate surface pretreatment step, before manual arc welding, various dirt and defects on the steel plate surface are deeply cleaned until they are invisible to the naked eye or the steel plate reveals metallic luster; In the steel plate welding groove processing and forming step, an asymmetric X-shaped groove is processed according to standard technical requirements, and a blunt edge of 2-5 mm is reserved; In the preheating treatment step before welding the steel plate, the preheating temperature is controlled to be ≥100°C, the preheating range is more than 100mm on each side of the weld, and the temperature is measured within a range of 30-50mm from the weld; In the welding step, the welding material used is JQ.J807SD high-strength steel electrode with a specification of Ф4.0mm, and the following process parameters are controlled: Current: 140-160A; Voltage: 22-25V; Welding speed: 80-150mm / min; Interpass temperature 100-200°C; and Post-heating system: 150-200℃ for more than 2 hours.

2. The manual arc welding butt welding method according to claim 1, wherein the thickness specification of the 800MPa grade high-strength steel plate is 10-60mm.

3. The manual arc welding butt welding method according to claim 1 or 2, wherein the chemical composition of the 800MPa grade high-strength steel plate is calculated by mass percentage as follows: C≤0.10%, Si≤0.30%, Mn≤1.70%, P≤0.010%, S≤0.004%, Als: 0.020%~0.035%, Nb≤0.050%, Ti≤0.030%, V≤0.050%, Cr≤0.70%, Mo≤0.70%, Ni≤1.5%, Cu≤0.30%, B≤0.0020%, and the rest is Fe and unavoidable impurities.

4. The manual arc welding butt welding method according to claim 3, wherein the chemical composition of the 800MPa grade high-strength steel plate is calculated by mass percentage as follows: C: 0.07% to 0.09%, Si: 0.10% to 0.30%, Mn: 1.20% to 1.60%, P≤0.010%, S≤0.004%, Als: 0.020% to 0.035%, Nb: 0.030% to 0.050%, Ti: 0.015% to 0.030%, V: 0.030% to 0.050%, Cr≤0.70%, Mo≤0.70%, Ni: 0.70 to 1.5%, Cu≤0.30%, B≤0.0020%, and the rest is Fe and unavoidable impurities.

5. The manual arc welding butt welding method according to claim 4, wherein the chemical composition of the 800MPa grade high-strength steel plate is calculated by mass percentage as follows: C: 0.076% to 0.089%, Si: 0.19% to 0.23%, Mn: 1.31% to 1.37%, P≤0.010%, S≤0.004%, Als: 0.024% to 0.030%, Nb: 0.040% to 0.045%, Ti: 0.017% to 0.020%, V: 0.039% to 0.045%, Cr: 0.41% to 0.45%, Mo: 0.37% to 0.42%, Ni: 0.84% ​​to 0.89%, Cu: 0.20% to 0.22%, B: 0 to 0.0014%, and the rest is Fe and unavoidable impurities.

6. The manual arc welding butt welding method according to any one of claims 1 to 5, wherein the steel plate surface pretreatment step comprises: (1) Surface defects such as oil, water, dirt, etc. should be wiped with alcohol; (2) Near-surface defects such as rust, iron oxide, and fine cracks should be polished away with an angle grinder.

7. The manual arc welding butt welding method according to any one of claims 1 to 6, further comprising observation and analysis of the metallographic structure of the weld and the heat affected zone after welding, and detection of mechanical properties and process properties.

8. The manual arc welding butt-jointing method according to any one of claims 1 to 7, wherein in the step of preheating the steel plate before welding, a flame spray gun is used to preheat the steel plate before welding, or a box-type resistance furnace is used to preheat the steel plate before welding.