Welding method suitable for nuclear power heat exchange tube and welding filling material thereof
By using specific welding filler materials and heat treatment technology, the stress and phase change problems in the welding of Incoloy-800H and SA-213T22 pipes are solved, the high-temperature performance and stability of the welded joints are improved, and the service life of the heat exchange tubes is extended.
Patent Information
- Application Number
- CN202411107813.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-10-01
AI Technical Summary
During the welding process between Incoloy-800H and SA-213T22 pipes, stress and deformation are caused by differences in thermal expansion coefficient and thermal conductivity, and different chemical compositions lead to complex phase changes and carbon diffusion phenomena, resulting in unstable weld quality and easy joints. Cracks, affecting welding performance.
The composition of a welding filler material is Cr: 15.0-18.0, Mn: 3.5-4.0, Nb: 3.0-3.5, Al: 1.5-1.8, Fe: ≤3.0, Si: ≤0.5, C : ≤0.1, P: ≤0.03, S: ≤0.015, the rest is Ni, Ni>67, used for welding of 800H/T22 dissimilar materials, surface treatment and TIG welding, heat treatment after welding is completed.
It reduces the driving force of carbon migration, reduces the risk of embrittlement and hardening, improves the toughness and crack resistance of the weld, enhances high-temperature performance, reduces welding defects, and improves the service life and performance of the welded joint.
Smart Images

Figure HDA0004991321960000011 
Figure HDA0004991321960000012
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nuclear power welding, and in particular relates to a welding method suitable for nuclear power heat exchange tubes and a welding filling material thereof. Background Art
[0002] The limited nature of fossil energy has aroused strong concern. Nuclear energy, as a clean, efficient and reliable new energy source, is a key research direction in the field of new energy. The heat exchange tube is the core component of the high-temperature gas-cooled reactor steam generator. While transmitting energy, it acts as a barrier to prevent the coolant and radioactive substances in the primary circuit from being released into the secondary circuit, which determines the service life of the steam generator. In order to save the construction cost of nuclear power plants, the heat exchange tube materials are divided into sections; the high-temperature section uses the high-temperature and corrosion-resistant Incoloy-800H pipe, while the preheating section and evaporation section of the heat exchange tube with a temperature below 440°C use the low-cost and high-performance low-alloy heat-resistant steel SA-213T22 pipe. The above two materials are connected by welding.
[0003] For the welding of the above heat exchange tubes, due to the significant differences in the thermal expansion coefficient, thermal conductivity and other physical properties of the tube materials on both sides of the welding part, stress and deformation are easily generated during the welding process; at the same time, due to the different chemical compositions of 800H and T22, complex phase changes and carbon diffusion phenomena are easily generated in the weld and heat-affected zone during welding; ultimately leading to unstable weld quality, easy joint cracks, and affecting the performance of the welded joint. At present, the commonly used welding filler material for 800H / T22 dissimilar material welding is ERNiCr-3, which cannot well improve the service performance of weld metal processing. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a welding method and welding filler material suitable for nuclear power heat exchange tubes, which are used to solve the welding quality defect problem between Incoloy-800H tubes and SA-213T22 tubes in the heat exchange tubes of high temperature gas-cooled reactor steam generators.
[0005] The present invention achieves the above technical objectives through the following technical means.
[0006] A welding filler material, whose components, by mass percentage, are: Cr: 15.0-18.0, Mn: 3.5-4.0, Nb: 3.0-3.5, Al: 1.5-1.8, Fe: ≤3.0, Si: ≤0.5, C: ≤0.1, P: ≤0.03, S: ≤0.015, and the rest is Ni.
[0007] Furthermore, Ni>67 in the composition.
[0008] Furthermore, it is used for welding 800H / T22 dissimilar materials.
[0009] A welding method suitable for nuclear power heat exchange tubes: using the above welding filler material as a melting ring.
[0010] Furthermore, surface treatment is performed before welding to remove the oxide film on the surface of the workpiece to be welded.
[0011] Furthermore, the surface treatment steps include: water washing, degreasing, polishing, and chemical cleaning.
[0012] Furthermore, a TIG welding system is used for welding, wherein: the peak welding current is 80A, the base current is 40A, the arc voltage is 12.4V, the pulse duty cycle is 60%, the pulse frequency is 1Hz, the welding speed is 12cm / min, the welding shielding gas composition outside the tube is 80% He and 20% Ar, the welding shielding gas flow rate is 22L / min, the shielding gas composition inside the tube is Ar, and the back shielding gas flow rate is 5L / min.
[0013] Furthermore, after welding is completed, the welded joint is heat treated.
[0014] Furthermore, the heat treatment steps are: preheating at 150-250°C first, then uniformly heating to 650°C and keeping warm for 40 minutes, and finally slowly cooling in the furnace.
[0015] The beneficial effects of the present invention are:
[0016] (1) The present invention provides a welding method and welding filler material suitable for nuclear power heat exchange tubes, wherein the welding filler material proposed reduces the content of Cr, which has a high affinity for carbon. Reducing Cr can reduce the driving force of carbon migration; adding a proper amount of Nb can combine with C to form a stable carbide, reduce the precipitation and migration of carbides, reduce the risk of embrittlement hardening, and can also refine the grains and improve the high-temperature strength; adding a proper amount of Al can reduce the oxygen content of the weld and effectively reduce pores and inclusions; while adding a proper amount of Mn, it can be used as a desulfurizer to improve the toughness and crack resistance of the weld. In summary, its high-temperature performance can be enhanced, the generation of welding defects can be reduced, and its service life can be improved.
[0017] (2) The welding method proposed in the present invention adds a heat treatment process after welding is completed, which can reduce the residual internal stress of welding, optimize the structure, improve the overall performance of the joint, make it more compatible with the performance of the parent material, and improve the service performance and service life of the heat exchange tube. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is the tensile fracture morphology formed by using conventional ERNiCr-3 welding filler material;
[0019] Figure 2This is a tensile fracture morphology diagram formed after adopting the welding method and welding filling material of the present invention. DETAILED DESCRIPTION
[0020] The following embodiments of the present invention are described in detail. The following embodiments are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.
[0021] Aiming at the welding problem between Incoloy-800H pipe and SA-213T22 pipe, this embodiment provides the following new welding filler material, the composition of which is as follows by mass percentage:
[0022] Cr: 15.0-18.0, Mn: 3.5-4.0, Nb: 3.0-3.5, Al: 1.5-1.8, Fe: ≤3.0, Si: ≤0.5, C: ≤0.1, P: ≤0.03, S: ≤0.015, and the rest is Ni, and the Ni content is >67.
[0023] Before welding, the welding filler material is cast into a melting ring according to the above composition requirements; after the casting is completed, the oil stains on the surface of the melting ring are first cleaned with an ethanol solution, and then ultrasonically cleaned with anhydrous ethanol and air-dried, and finally sealed in a dehumidification box for standby use;
[0024] For the welding of Incoloy-800H pipe and SA-213T22 pipe, follow the steps below:
[0025] Step 1, surface treatment: The pipe to be welded is subjected to water washing, degreasing, grinding, chemical cleaning and other processes to remove the oxide film on the surface of the workpiece to be welded.
[0026] Step 2, welding is performed using a TIG welding system and the above-mentioned melting ring, wherein:
[0027] 1) Before welding, check whether the welding equipment is working properly, check whether the gas cylinder has gas, and check whether the mechanical walking mechanism is operating normally;
[0028] 2) Set the welding process parameters as follows: peak welding current is 80A, base current is 40A, arc voltage is 12.4V, pulse duty cycle is 60%, pulse frequency is 1Hz, welding speed is 12cm / min, welding shielding gas composition outside the tube is 80% He and 20% Ar, welding shielding gas flow rate is 22L / min, shielding gas composition inside the tube is Ar, and back shielding gas flow rate is 5L / min.
[0029] Step 3, heat treatment: After welding is completed, the welded joint is heat treated; specifically, it is preheated at 150-250°C, then evenly heated to 650°C and kept warm for 40 minutes, and finally slowly cooled with the furnace;
[0030] After all welding steps are completed, the welding parts are inspected accordingly, including:
[0031] 1) Nondestructive testing: X-ray or ultrasonic testing of welded joints to detect the process quality and sealing of welded joints;
[0032] 2) Performance testing: Testing the mechanical properties of welded joints, including hardness testing, tensile testing and impact testing.
[0033] The corresponding comparative test results are shown in Table 1, Table 2 and Figure 1 , Figure 2 shown.
[0034] Table 1: Comparative test of mechanical properties of welded joints
[0035] No melting ring ERCrNi-3 The present invention Tensile strength / Mpa 486 503 509 Yield strength / Mpa 363 210 150 Elongation after break / % 5.5 17.54 25.09 Microhardness of weld / HV 143.8 145.2 147.2
[0036] Table 2 Comparison of EDS spectrum analysis of tissues near the joint
[0037] C Si Mo Cl Cr Mn Fe Ni Nb Al ERCrNi-3 3.25 0.26 0.71 0.58 3.93 0.47 87.68 3.11 The present invention 2.58 2.73 0.68 19.58 20.13 8.76 1.72
[0038] As shown in Table 1, after adopting the welding method of the present invention and the melting ring filling material thereof, the mechanical properties of the welded structure are significantly improved compared with the welding method without melting ring and the melting ring made of ERCrNi-3 material.
[0039] like Figure 1 and Figure 2 The tensile fracture morphology shown in the figure Figure 1 To use ERCrNi-3 filler material, Figure 2 The filler material proposed in the present invention is used. By comparison, it can be seen that the size and number of dimples using the welding filler material of the present invention are reduced, and the number of second phase particles and pores in the reaction welded parts is reduced. Combined with the EDS analysis of the welded joint in Table 2, it can be concluded that the weld of the present invention contains Nb elements, which can form carbonitrides with C, reduce the migration of C elements, and disperse strengthen, thereby improving the strength and toughness of the joint.
[0040] The present invention is not limited to the above-mentioned embodiments. Any obvious improvement, substitution or deformation that can be made by those skilled in the art without departing from the essential content of the present invention belongs to the protection scope of the present invention.
Claims
1. A welding filler material, characterized in that: In terms of mass percentage, its composition is: Cr: 15.0-18.0, Mn: 3.5-4.0, Nb: 3.0-3.5, Al: 1.5-1.8, Fe: ≤3.0, Si: ≤0.5, C: ≤0.1, P: ≤0.03, S: ≤0.015, and the rest is Ni.
2. The welding filler material according to claim 1, characterized in that: Ni>67 in the composition.
3. The welding filler material according to claim 1, characterized in that: Used for 800H / T22 dissimilar material welding.
4. A welding method suitable for nuclear power heat exchange tubes, characterized in that: The welding filler material as claimed in any one of claims 1 to 3 is used as the melting ring.
5. The welding method for nuclear power heat exchange tubes according to claim 4 is characterized in that: Before welding, surface treatment is performed to remove the oxide film on the surface of the workpiece to be welded.
6. The welding method for nuclear power heat exchange tubes according to claim 5, characterized in that: The surface treatment steps include: water washing, degreasing, polishing and chemical cleaning.
7. The welding method for nuclear power heat exchange tubes according to claim 4 is characterized in that: TIG welding system is used for welding, in which: peak welding current is 80A, base current is 40A, arc voltage is 12.4V, pulse duty cycle is 60%, pulse frequency is 1Hz, welding speed is 12cm / min, welding shielding gas composition outside the tube is 80% He and 20% Ar, welding shielding gas flow rate is 22L / min, shielding gas composition inside the tube is Ar, and back shielding gas flow rate is 5L / min.
8. The welding method for nuclear power heat exchange tubes according to claim 4 is characterized in that: After welding is completed, the weld joint is heat treated.
9. The welding method for nuclear power heat exchange tubes according to claim 8, characterized in that: The heat treatment steps are: preheating at 150-250° C., then uniformly heating to 650° C. and keeping the temperature for 40 minutes, and finally slowly cooling in the furnace.