Machining method for arc-shaped plate and curved plate of three-dimensional curved surface multi-arch-limb structural steel arch shell

Through the methods of steel plate correction, surface pretreatment, lofting and typesetting, cutting and forming, the problem of long processing cycle and low precision of the three-dimensional curved multi-arch limb structure steel arch shell arc plate and curved plate is solved, and efficient and precise processing is achieved. , which promotes the application development of structures.

CN118720641APending Publication Date: 2024-10-01CHINA RAILWAY FIRST GROUP CO LTD +2
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410694044.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-30
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the existing technology, the processing of arc plates and curved panels of three-dimensional curved multi-arch limb structural steel arch shells has the problems of long cycle and low precision, which limits the application and development of the structure.

Method used

The methods of steel plate correction, surface pretreatment, lofting and layout, cutting and blanking and forming are adopted, including the use of mold surface forming and rounding machine forming, combined with tire frame assistance to ensure processing accuracy and efficiency.

Benefits of technology

It has shortened the processing cycle and improved the accuracy, provided a complete processing system, guaranteed the quality of later splicing, and facilitated the application of three-dimensional curved multi-arch limb structural steel arch shells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720641A_ABST
    Figure CN118720641A_ABST
Patent Text Reader

Abstract

The invention discloses a machining method for an arc-shaped plate and a curved plate of a three-dimensional curved surface multi-arch-limb structural steel arch shell, and relates to the technical field of bridge engineering. Comprising the following steps: S1, correcting a steel plate; s2, surface pretreatment; s3, lofting and typesetting; s4, cutting and blanking; and S5, forming. The invention provides a set of complete arc plate and curved plate processing system which can be completely completed in a factory, the processing period is greatly shortened, mold forming and jig frame assistance are adopted, the manufacturing precision is high, meanwhile, an effective guarantee is provided for later splicing, and application and development of the steel arch shell of the three-dimensional curved surface multi-arch-limb structure are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of bridge engineering, and in particular to a method for processing an arc plate and a curved plate of a three-dimensional curved surface multi-arch limb structure steel arch shell. Background Art

[0002] In recent years, the landscape effect of urban bridges has been improved by adding decorative structures to the main structure of the bridge. However, the decorative structure does not participate in the stress of the bridge structure, but increases the design load of the original bridge and reduces the safety of the structure. While improving the landscape of the bridge, the three-dimensional curved multi-arch limb steel arch shell participates in the overall stress of the bridge, improves the overall structural safety and economy, and has a trend of becoming a mainstream design. The three-dimensional curved multi-arch limb steel arch shell is completed by a multi-segment overall assembly method, and the processing of the curved plates and curved panels as unit components of each segment is particularly important. At present, the processing of curved plates and curved panels is mostly manual grinding, and there is no complete processing system. The processing cycle is long, the precision is low, and the splicing is time-consuming, which limits the application and development of the three-dimensional curved multi-arch limb steel arch shell. Summary of the invention

[0003] The main purpose of the present invention is to provide a method for processing an arc plate and a curved plate of a three-dimensional curved multi-arch limb structural steel arch shell to solve the above problems.

[0004] To achieve the above object, the present invention provides a method for processing an arc plate and a curved plate of a three-dimensional curved surface multi-arch structure steel arch shell, comprising the following steps:

[0005] S1, steel plate correction;

[0006] S2, surface pretreatment;

[0007] S3, layout and typesetting;

[0008] S4, cutting and blanking;

[0009] S5. Molding.

[0010] Furthermore, in step 1, the surface of the corrected steel plate should not have obvious concave surfaces or damage, and the scratch depth should not be greater than 0.5 mm, and should not be greater than 1 / 2 of the negative allowable deviation of the thickness of the steel plate.

[0011] Furthermore, in step 2, the steel plate surface is shot blasted and coated with epoxy zinc-rich primer.

[0012] Furthermore, in step three, nesting software is used to layout and cut materials, indicating the processing number, component number, part number, material and quantity; when layout, according to the project material collection plan, parts and components are cut as whole plates as possible to avoid splicing; plates with the same processing number, the same thickness and the same material must be laid out uniformly to improve material utilization.

[0013] Furthermore, in step four, the oil, rust and moisture on the surface of the parent material should be removed before cutting. After cutting, the gas-cut surface should be smooth and free of cracks, slag and spatter. The shear surface should be polished. After flame cutting, the part size should be self-checked, and then the component number and part number of the part should be marked. The quality inspector will then check the various indicators. Only after passing the inspection can it flow into the next process.

[0014] Furthermore, in step five, the curved plate is processed by mold surface forming; first, the cast steel mold is designed and manufactured according to the structural form of the part drawing, and then the part plate is formed by the mold pressing plate forming method; after the mold forming process, the steel surface should have no obvious concave surface or damage, and the scratch depth should be less than 0.5mm.

[0015] Furthermore, in step five, the curved panel is formed by rounding with a rounding machine; specifically, the steel plate is longitudinally placed in the rounding machine, the spacing between the three rollers of the rounding machine is adjusted, and the rotation speed of the rollers is controlled. The steel plate is first initially rounded, and the rounding is repeated to gradually form the curved panel. After forming, the curved panel is hoisted onto a special frame for comparison and fitting. If the forming is unqualified, the curved panel is corrected and rounded again until it passes the inspection.

[0016] Furthermore, the supporting material of the tire frame is determined according to the materials in stock in the factory, mainly rectangular square tubes, round tubes, H-shaped steel or steel plates, and the tire frame size control error is 3mm; using three-dimensional software, the outer contour shape of the lower side panel is taken out at intervals of 2 meters, and a CNC cutting machine is used to cut arc strips as tire frame supports.

[0017] The present invention has the following beneficial effects:

[0018] The present invention provides a complete arc plate and curved panel processing system, which can be completed entirely in the factory, greatly shortening the processing cycle. With mold forming and frame assistance, the manufacturing precision is high, while providing effective guarantee for later splicing, facilitating the application and development of three-dimensional curved multi-arch limb structural steel arch shells. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The present invention is a flow chart of a method for processing arc plates and curved panels of a three-dimensional curved surface multi-arch limb structure steel arch shell.

[0020] Figure 2 The present invention is a schematic diagram of a steel arch shell of a three-dimensional curved surface multi-arch structure and a method for processing an arc plate and a curved plate.

[0021] Figure 3 The present invention is a schematic diagram of arc plate forming of an arc plate and a method for processing an arc plate and a curved plate of a three-dimensional curved surface multi-arch limb structure steel arch shell.

[0022] Figure 4-5 The present invention is a schematic diagram of a tire frame for a method for processing an arc-shaped plate and a curved plate of a three-dimensional curved multi-arch-limb structural steel arch shell. DETAILED DESCRIPTION

[0023] In order to achieve the above-mentioned purpose and effect, the technical means and structures adopted by the present invention are described in detail with reference to the accompanying drawings for the features and functions of the preferred embodiments of the present invention.

[0024] like Figure 1 As shown, the present invention provides a method for processing an arc plate and a curved plate of a three-dimensional curved surface multi-arch limb structure steel arch shell, comprising the following steps:

[0025] S1, steel plate correction;

[0026] Before processing, the steel plate to be processed should be checked for any deformation that is harmful to the production (such as partial winding, bending, etc.). When heat correction is used, it should be noted that the heat correction heating temperature does not exceed 900℃, and water cooling is strictly prohibited during the correction process.

[0027] Low alloy structural steel should not be cold straightened when the ambient temperature is below -12℃.

[0028] The surface of the steel after correction should not have obvious concave surfaces or damage, the scratch depth should not be greater than 0.5mm, and should not be greater than 1 / 2 of the allowable deviation of the steel thickness.

[0029] The allowable deviation of steel after correction shall comply with the provisions of Table 4.4.5 of the "Railway Steel Bridge Manufacturing Specifications" (QCR9211-2015) on the local flatness of the steel plate.

[0030] S2, surface pretreatment;

[0031] Considering that the cross-sectional height of the project components is relatively small (800mm), and there are many stiffening plates and transverse partitions inside, it is difficult to remove rust in the box after the components are manufactured, and it is difficult to ensure the quality of rust removal; therefore, the steel plate surface is shot blasted before unloading. The construction environment: temperature 10-30℃, relative humidity 30-80%, and the shot blasting grade is required to reach Sa2.5. After the shot blasting is completed, epoxy zinc-rich primer must be sprayed within 4 hours. When spraying epoxy zinc-rich primer, the surface roughness of the steel is 40-70um; during assembly and welding, the paint on the welding part is polished, and after the segment manufacturing and welding is completed, the weld surface in the box is partially polished, and epoxy zinc-rich primer is applied, and then thick paste paint is applied together.

[0032] S3, layout and typesetting;

[0033] Use nesting software to layout and cut materials, and indicate the processing number, component number, part number, material and quantity; when layout, according to the project material collection plan, parts and components should be cut as whole plates as possible to avoid splicing; plates with the same processing number, thickness and material must be laid out uniformly to improve material utilization.

[0034] S4, cutting and blanking;

[0035] Before cutting, the oil, rust and moisture on the surface of the parent material should be removed. After cutting, the cut surface should be smooth without cracks, slag and spatter, and the shear surface should be polished.

[0036] The dimensions of the cut parts shall comply with the construction drawings, process documents and specifications. Unless otherwise specified, the allowable deviations are shown in the following table:

[0037]

[0038]

[0039] After flame cutting, the parts must be self-checked in size, and then marked with the component number and part number to which the parts belong. The quality inspector will then check all indicators. Only after passing the inspection can the parts enter the next process.

[0040] S5. Molding.

[0041] like Figure 3 As shown, the curved plate is processed by mold surface forming; first, the cast steel mold is designed and manufactured according to the structural form of the part drawing, and then the part plate is formed by the mold pressing plate forming method; after the mold forming process, the steel surface should have no obvious concave surface or damage, and the scratch depth should be less than 0.5mm.

[0042] The curved panel is formed by rounding with a rounding machine. Specifically, the steel plate is placed longitudinally in the rounding machine, the spacing between the three rollers of the rounding machine is adjusted, and the speed of the rollers is controlled. The steel plate is first rounded slowly, and then the rounding is repeated to gradually form the curved panel. After forming, the curved panel is hoisted to a special frame for comparison and fitting. If the forming is unqualified, it is corrected and rounded again until it passes the inspection.

[0043] like Figure 4-5 As shown, the support material of the tire frame is determined according to the inventory materials in the factory, mainly rectangular square tubes, round tubes, H-shaped steels, and steel plates, and the tire frame size control error is 3mm; using three-dimensional software, the outer contour shape of the lower side panel is taken out at intervals of 2 meters, and a CNC cutting machine is used to cut arc strips as tire frame supports.

[0044] The above descriptions are only preferred embodiments of the present invention, not all embodiments. Anyone should be aware that any structural changes made under the inspiration of the present invention, and any technical solutions that are the same or similar to the present invention, belong to the protection scope of the present invention.

Claims

1. A method for processing arc plates and curved plates of a three-dimensional curved multi-arch structure steel arch shell, characterized in that: The following steps are involved: S1, steel plate correction; S2, surface pretreatment; S3, layout and typesetting; S4, cutting and blanking; S5. Molding.

2. The method for processing the arc-shaped plate and the curved plate of the three-dimensional curved surface multi-arch limb structure steel arch shell according to claim 1, characterized in that: In step 1, the surface of the corrected steel plate should not have obvious concave surfaces or damage, the scratch depth should not be greater than 0.5mm, and should not be greater than 1 / 2 of the negative allowable deviation of the steel plate thickness.

3. The method for processing the arc-shaped plate and the curved plate of the three-dimensional curved surface multi-arch limb structure steel arch shell according to claim 2, characterized in that: In step 2, the steel plate surface is shot blasted and coated with epoxy zinc-rich primer.

4. The method for processing the arc-shaped plate and the curved plate of the three-dimensional curved surface multi-arch limb structure steel arch shell according to claim 3, characterized in that: In step three, use nesting software to layout and cut materials, indicating the processing number, component number, part number, material and quantity; when layout, according to the project material plan, parts and components should be cut as whole plates as possible to avoid splicing; plates with the same processing number, thickness and material must be laid out uniformly to improve material utilization.

5. The method for processing the arc-shaped plate and the curved plate of the three-dimensional curved surface multi-arch limb structure steel arch shell according to claim 4, characterized in that: In step 4, the oil, rust and moisture on the surface of the parent material should be removed before cutting. After cutting, the gas-cut surface should be smooth and free of cracks, slag and spatter. The shear surface should be polished. After flame cutting, the part size should be self-checked, and then the component number and part number of the part should be marked. The quality inspector will then check the various indicators. Only after passing the inspection can it flow into the next process.

6. The method for processing the arc-shaped plate and the curved plate of the three-dimensional curved surface multi-arch structure steel arch shell according to claim 5, characterized in that: In step five, the curved plate is processed by mold surface forming; first, the cast steel mold is designed and manufactured according to the structural form of the part drawing, and then the part plate is formed by the mold pressing plate forming method; after the mold forming process, the steel surface should have no obvious concave surface or damage, and the scratch depth should be less than 0.5mm.

7. The method for processing the arc-shaped plate and the curved plate of the three-dimensional curved surface multi-arch limb structure steel arch shell according to claim 6, characterized in that: In step five, the curved panel is formed by rounding with a rounding machine; specifically, the steel plate is placed longitudinally in the rounding machine, the spacing between the three rollers of the rounding machine is adjusted, and the roller speed is controlled. The steel plate is first rounded slowly, and the rounding is repeated to gradually form the curved panel. After forming, the curved panel is hoisted onto a special frame for comparison and fitting. If the forming is unqualified, the curved panel is corrected and rounded again until it passes the inspection.

8. The method for processing the arc-shaped plate and the curved plate of the three-dimensional curved surface multi-arch structure steel arch shell according to claim 7, characterized in that: The supporting material of the tire frame is determined according to the materials in stock in the factory, mainly rectangular square tubes, round tubes, H-shaped steel or steel plates, and the tire frame size control error is 3mm; using three-dimensional software, the outer contour shape of the lower side panel is taken out at intervals of 2 meters, and a CNC cutting machine is used to cut arc strips as tire frame supports.

Citation Information

Patent Citations

  • Manufacture method for curve plate of steel case girder

    CN103028914A

  • Manufacturing method of spatial multi-curved-surface special shaped steel bridge arch

    CN107745227A

  • Manufacturing method of box type steel structure streamline steel arch with special-shaped section

    CN112342922A

  • Multi-span asymmetric bridge special-shaped steel arch manufacturing and construction method

    CN114960450A

  • Special-shaped curved plate unit forming and control method

    CN116140438A