Nickel-aluminum-bronze alloy material for plastic mold and preparation method
By adjusting the element ratio of nickel-aluminum bronze alloy materials and using laser additive manufacturing technology, the problem of insufficient hardness and toughness of copper alloy materials was solved, and a high-performance nickel-aluminum bronze alloy material suitable for plastic molds was prepared, extending the mold life And improves production efficiency.
Patent Information
- Application Number
- CN202410894010.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-07-04
AI Technical Summary
The existing copper alloy materials have low hardness and insufficient toughness, which limits their application in the field of plastic molds.
Using nickel-aluminum bronze alloy material, by adjusting the mass percentage of Al, Ni, Fe, Mn, increasing the elements of Ti, La, Sr, combined with laser additive manufacturing technology and specific heat treatment processes, we can prepare high mechanical properties, corrosion resistance and Abrasion-resistant material.
It realizes the high strength, toughness and corrosion resistance of nickel-aluminum bronze alloy materials, extends the service life of plastic molds, and improves production efficiency.
Smart Images

Figure GDA0005128667430000041 
Figure GDA0005128667430000061
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of alloy material preparation, and in particular to a nickel-aluminum-bronze alloy material for plastic molds and a preparation method thereof. Background Art
[0002] Nickel aluminum bronze alloy is an alloy developed from aluminum bronze. Adding nickel, iron and manganese elements to aluminum bronze can not only refine the grains, but also inhibit the formation of harmful γ phase, so it has high comprehensive mechanical strength and good corrosion resistance. With the development of modern industry and the advancement of science and technology, the use and amount of polymer plastics in modern industry and people's daily life have grown rapidly, the variety of polymer plastic products has increased day by day, and people's requirements for the intrinsic quality, dimensional accuracy and appearance of plastic products have also increased day by day. The thermal conductivity, heat dissipation, service life, processability, geometric processing accuracy and surface finish of traditional iron alloy mold materials for making plastic product molding molds, as well as the precision, surface smoothness and beauty, and clear decorative patterns of plastic products made of iron alloy mold materials are far inferior to copper alloy mold materials. However, the existing copper alloy generally has a low hardness and is not suitable as a plastic mold material. Even if the copper alloy doped with other metal elements can achieve high strength and hardness, the corresponding toughness still cannot meet the requirements, thus limiting the application of copper alloys in the field of plastic molds. Existing copper alloys have been more widely used in the plastics and electronics industries. Therefore, studying a nickel-aluminum bronze alloy suitable for the preparation of plastic molds will greatly promote the development of related industries. Summary of the invention
[0003] In order to solve the above technical problems, a nickel-aluminum-bronze alloy material for plastic molds with good corrosion resistance, good wear resistance and high hardness is developed. The present application provides a nickel-aluminum-bronze alloy material for plastic molds and a preparation method thereof.
[0004] In a first aspect, the present application provides a nickel-aluminum bronze alloy material for a plastic mold, wherein the raw materials of the nickel-aluminum bronze alloy material contain the following elements and mass percentages: Al 8.3-8.8%, Ni 3.0-4.0%, Fe 3.5-4.5%, Mn 2.8-3.5%, and the balance is copper.
[0005] Furthermore, the elements and mass percentages contained in the raw materials of the nickel-aluminum bronze alloy material include: Al 8.3-8.8%, Ni 3.0-4.0%, Fe 3.5-4.5%, Mn 2.8-3.5%, Ti 1.1-1.6%, La 0.3-0.6%, Sr0.02-0.12%, and the balance is copper.
[0006] By adopting the above technical scheme, in this application, the mass percentage of the basic elements Al, Ni, Fe, and Mn in the nickel-aluminum bronze alloy material is fine-tuned, and the content of Al and Ni elements is appropriately reduced, which can reduce the content of κⅡ and κⅢ with higher strength in the alloy matrix material and increase the content of α phase and β' phase in the matrix material, thereby enhancing the elongation and plasticity of the nickel-aluminum bronze alloy material. The Fe and Mn elements have a certain promoting effect on grain refinement during the manufacturing process of the nickel-aluminum bronze alloy, and can improve the strength under the premise of maintaining the elongation of the alloy matrix material. Adding Ti, La and Sr elements to the alloy matrix material can, on the one hand, refine the grains to improve the mechanical properties, and on the other hand, promote the density of the surface alloy of the obtained nickel-aluminum bronze alloy material, thereby improving the corrosion resistance of the obtained nickel-aluminum bronze alloy material.
[0007] In a second aspect, the present application provides a method for preparing the above-mentioned nickel-aluminum bronze alloy material for plastic molds, comprising the following steps:
[0008] S1. Raw material pretreatment: placing the raw materials in a vacuum melting chamber for melting, heating, hot rolling, drawing, annealing, etching, cleaning, and drying to obtain nickel-aluminum bronze welding wire;
[0009] S2, start the laser additive manufacturing system, run the control program, convey the nickel-aluminum bronze welding wire obtained in step S1, deposit it layer by layer on the surface of the substrate, and obtain a nickel-aluminum bronze molded part. The process parameters of laser additive manufacturing using the laser additive manufacturing system are as follows: laser power: 2000-3000W, the angle between the welding wire and the horizontal substrate is 20-35°, the welding wire dry extension is 10-15mm, the wire output speed is 10-24mm / s, the laser beam scanning speed is 5-13mm / s, the layer height is 0.2-0.3mm, and the gas flow rate is 4-6L / min;
[0010] S3, heat-treating the nickel-aluminum bronze molded part obtained in step S2 to obtain a nickel-aluminum bronze alloy material, wherein the heat treatment comprises the following steps:
[0011] 1) Annealing treatment: keep at 600-640℃ for 2-3.5h, and cool with the furnace;
[0012] 2) Aging treatment: keep at 850-900℃ for 3.5-4.5h, quench; then keep at 400-450℃ for 1h, cool with the furnace.
[0013] By adopting the above technical scheme, the nickel-aluminum bronze molded parts produced by laser additive manufacturing technology are subjected to a specific process of heat treatment, so that the microstructure of the nickel-aluminum bronze alloy material presents a mixed structure of lamellar martensite and nano-precipitated Widmanstattenite α phase, and high-density κⅡ and κⅢ are dispersed, so that the nickel-aluminum bronze alloy material produced in this application has good toughness while retaining good strength, so that the produced plastic mold has a longer service life.
[0014] Optionally, in step S1, the raw material pretreatment includes the following steps:
[0015] a: Place the raw materials in a vacuum melting chamber and melt them at 1050-1150℃ for 40-60min to obtain alloy liquid;
[0016] b: heating the alloy liquid obtained in step a to 1100-1300° C., performing horizontal continuous casting to obtain a bar, hot rolling, pickling, and obtaining an alloy bar;
[0017] c: straightening the alloy rod obtained in step b, applying lubricating oil, drawing, annealing, furnace cooling, sizing, and scraping to obtain alloy wire;
[0018] d: etching the alloy wire obtained in step c, cleaning, drying, coating with a composite coating, and drying to obtain a nickel-aluminum bronze welding wire.
[0019] Optionally, in step d, the alloy wire is immersed in an etchant for etching, and the etchant comprises 5-8wt% of citric acid, 2-5wt% of sulfuric acid and 2-3wt% of triethanolamine.
[0020] Optionally, in step d, the composite coating comprises a binder and metal powder in a weight ratio of 2-5:2-3, wherein the metal powder comprises TiO 2 and CeO 2 .
[0021] By adopting the above technical solution, the nickel-aluminum bronze welding wire produced by a specific process in the present application has good processing performance, and the uniformity and stability of the welding wire composition are good, which is conducive to the preparation of a nickel-aluminum bronze alloy material with good property uniformity.
[0022] Optionally, in step S1, the raw materials include pure aluminum, pure iron, pure nickel, pure manganese and pure copper.
[0023] Optionally, in step S2, the substrate is surface treated by sequentially cleaning, polishing, cleaning and drying.
[0024] Optionally, in step S3, during the laser additive manufacturing process, the welding wire and the laser beam are controlled to start from a layer of the substrate and are reciprocatedly deposited layer by layer. The height of each layer of welding wire and laser beam is set to 3.0 mm, and the cooling time between layers is 10 s.
[0025] In summary, the present invention includes at least one of the following beneficial technical effects:
[0026] 1. Since the present invention adopts a specific element ratio and combines advanced laser additive manufacturing technology, the obtained nickel-aluminum bronze alloy material has good mechanical properties and excellent corrosion resistance and wear resistance, and is very suitable for the manufacture of plastic molds.
[0027] 2. In the present invention, a specific heat treatment process is preferably used to further improve the comprehensive performance of the material, extend the service life of the mold, and improve production efficiency. DETAILED DESCRIPTION
[0028] The present application is further described in detail below in conjunction with specific embodiments.
[0029] The present application designs a nickel-aluminum bronze alloy material for plastic molds. The raw materials of the nickel-aluminum bronze alloy material contain the following elements and mass percentages: Al 8.3-8.8%, Ni 3.0-4.0%, Fe 3.5-4.5%, Mn 2.8-3.5%, and the balance is copper.
[0030] The nickel-aluminum-bronze alloy material for the plastic mold of the present application is prepared by the following method, comprising the following steps:
[0031] S1. Raw material pretreatment: placing the raw materials in a vacuum melting chamber for melting, heating, hot rolling, drawing, annealing, etching, cleaning, and drying to obtain nickel-aluminum bronze welding wire;
[0032] S2, start the laser additive manufacturing system, run the control program, convey the nickel-aluminum bronze welding wire obtained in step S1, deposit it layer by layer on the surface of the substrate, and obtain a nickel-aluminum bronze molded part. The process parameters of laser additive manufacturing using the laser additive manufacturing system are as follows: laser power: 2000-3000W, the angle between the welding wire and the horizontal substrate is 20-35°, the welding wire dry extension is 10-15mm, the wire output speed is 10-24mm / s, the laser beam scanning speed is 5-13mm / s, the layer height is 0.2-0.3mm, and the gas flow rate is 4-6L / min;
[0033] S3, heat-treating the nickel-aluminum bronze molded part obtained in step S2 to obtain a nickel-aluminum bronze alloy material, wherein the heat treatment comprises the following steps:
[0034] 1) Annealing treatment: keep at 600-640℃ for 2-3.5h, and cool with the furnace;
[0035] 2) Aging treatment: keep at 850-900℃ for 3.5-4.5h, quench; then keep at 400-450℃ for 1h, cool with the furnace.
[0036] The technical problem solved by this application is that the existing copper alloys generally have low hardness and are not suitable as plastic mold materials. Even if the copper alloys doped with other metal elements can achieve high strength and hardness, the corresponding toughness still does not meet the requirements, thus limiting the application of copper alloys in the field of plastic molds. This application adopts a specific element ratio and combines it with advanced laser additive manufacturing technology to produce a nickel-aluminum bronze alloy material with good mechanical strength and excellent corrosion resistance and wear resistance, which is suitable for the manufacture of plastic molds. In addition, a specific heat treatment process is preferably used in this application to further improve the comprehensive performance of the material, extend the service life of the mold, and improve production efficiency.
[0037] Examples 1-6
[0038] Examples 1-6 are nickel-aluminum bronze alloy materials made from different raw material ratios, and the mass percentages of the elements of the raw materials are shown in Table 1.
[0039] surface
[0040]
[0041] It can be seen from Table 1 that Examples 1-3 are nickel-aluminum bronze alloy materials not doped with Ti, La and Sr elements, wherein the mass percentages of Al, Ni, Fe and Mn are as shown in Table 1, and the remainder is the copper content and unavoidable impurities, and the mass percentage of impurities is ≤0.1%.
[0042] Similarly, the contents of each element in the nickel-aluminum bronze alloy material raw materials in Examples 4-6 are the same as above.
[0043] The preparation process of the nickel-aluminum bronze alloy material obtained in Examples 1-6 comprises the following steps:
[0044] S1. Raw material pretreatment: The raw materials are made into nickel-aluminum bronze welding wire according to the ratio, which specifically includes the following steps:
[0045] Step a: placing the raw materials in a vacuum melting chamber and melting them at 1080° C. for 50 min to obtain a molten alloy;
[0046] Step b: heating the alloy liquid obtained in step a to 1180° C., performing horizontal continuous casting to obtain a bar, controlling the hot rolling temperature to 480° C. and performing hot rolling three times, wherein the total reduction rate of the outer diameter of the bar after hot rolling is 70%, and pickling to obtain an alloy bar;
[0047] Step c: straightening the alloy rod obtained in step b, applying lubricating oil, and performing multiple drawing. When the cold deformation reaches 60%, vacuum annealing is performed at 600° C. for 15 minutes, followed by furnace cooling, sizing, and scraping to obtain alloy wire.
[0048] Step d: etching the alloy wire obtained in step c, cleaning, drying, coating the composite coating, and drying to obtain the nickel-aluminum bronze welding wire; wherein the etching process is: immersing the alloy wire in an etchant for 30 seconds, the etchant comprising 5wt% citric acid, 2wt% sulfuric acid, 3wt% triethanolamine and the remainder water; the composite coating used in the composite coating is obtained by mixing a binder and a metal powder in a weight ratio of 3:2, the metal powder comprising TiO 2 and CeO 2 , the coating thickness of the composite coating is controlled at 0.2mm.
[0049] S2. Surface treatment of the substrate: using anhydrous ethanol to clean and remove oil stains, using sandpaper to increase the roughness of the substrate surface, thereby reducing the reflectivity of the substrate to the laser, and then using acetone to clean and dry; starting the laser additive manufacturing system, running the control program, conveying the nickel-aluminum bronze welding wire obtained in step S1, depositing layer by layer on the substrate to obtain a nickel-aluminum bronze molded part, and the process parameters for laser additive manufacturing using the laser additive manufacturing system are: laser power: 3000W, the angle between the welding wire and the horizontal substrate is 30°, the welding wire dry extension length is 10mm, the welding wire output speed is 15mm / s, the laser beam scanning speed is 10mm / s, the layer height is 0.2mm, and the gas flow rate is 6L / min; the height of each layer of welding wire and laser beam is set to 3.0mm, and the interlayer cooling time is 10s.
[0050] S3, heat treating the nickel-aluminum bronze molded part obtained in step S2 to obtain a nickel-aluminum bronze alloy material. The heat treatment comprises the following steps:
[0051] 1) Annealing treatment: keep at 600℃ for 3h, and cool with the furnace;
[0052] 2) Aging treatment: keep at 850℃ for 3.5h, quench; then keep at 400℃ for 1h, cool in the furnace.
[0053] Example 7
[0054] Example 7 is based on Example 2, except that in step d of step S1 in Example 7, the composite coating is not coated on the alloy wire.
[0055] Example 8
[0056] Example 8 is based on Example 2, except that: in step d of step S1 in Example 8, the composite coating used in the composite coating is obtained by mixing a binder and a metal powder in a weight ratio of 3:2, and the metal powder includes TiO 2 and Al 2 O 3 , the coating thickness of the composite coating is controlled at 0.2mm.
[0057] Examples 9-10
[0058] Example 9 is based on Example 2, with the difference that in step S2 of Example 9, during the laser additive manufacturing process, the laser beam scanning speed is changed to 13 mm / s.
[0059] Example 10 is based on Example 2, with the difference that in step S2 of Example 10, during the laser additive manufacturing process, the laser beam scanning speed is changed to 5 mm / s.
[0060] Comparative Example 1
[0061] Comparative Example 1 is based on Example 2, except that the elements and mass percentages contained in the raw materials of the nickel-aluminum bronze alloy material in Comparative Example 1 include: Al 9.5%, Ni 3.3%, Fe 4.4%, Mn 3.1%, and the balance is copper and unavoidable impurities.
[0062] Comparative Example 2
[0063] Comparative Example 2 is based on Example 2, with the difference that in Comparative Example 2, the nickel-aluminum-bronze molded part is not subjected to aging treatment after annealing treatment in step S3.
[0064] Performance Testing
[0065] 1. The tensile strength and elongation at break of the nickel-aluminum bronze alloy materials prepared in Examples 1-10 and Comparative Examples 1-2 were measured with reference to the standard GB / T228.1-2010 "Tensile test of metallic materials Part 1: Room temperature test method".
[0066] 2. The surface hardness of the nickel-aluminum bronze alloy materials prepared in Examples 1-10 and Comparative Examples 1-2 was measured with reference to the standard GB / T 4341-2009 "Metal Rockwell Hardness Test Method".
[0067] 3. The wear rates of the nickel-aluminum bronze alloy materials prepared in Examples 1-10 and Comparative Examples 1-2 were measured with reference to the standard GB / T 12444.1-2008 “Metallic material wear test methods Part 1: Wear test of rotating disks and contacting sliders”.
[0068] The measurement results are shown in Table 2.
[0069] Table 2
[0070]
[0071] By analyzing the data in Table 2 and comparing the performance test data of Examples 1-10 with those of Comparative Examples 1-2, it can be seen that the nickel-aluminum bronze alloy material in the present application has high tensile strength, hardness and wear resistance while maintaining a high elongation at break, and is very suitable for the manufacture of plastic molds.
[0072] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing a nickel-aluminum bronze alloy material for a plastic mold, characterized in that: The elements and mass percentages contained in the raw materials of the nickel-aluminum bronze alloy material include: Al 8.3-8.8%, Ni 3.0-4.0%, Fe 3.5-4.5%, Mn 2.8-3.5%, and the balance is copper; The preparation method comprises the following steps: S1. Raw material pretreatment: placing the raw materials in a vacuum melting chamber for melting, heating, hot rolling, drawing, annealing, etching, cleaning, and drying to obtain nickel-aluminum bronze welding wire; S2, start the laser additive manufacturing system, run the control program, convey the nickel-aluminum bronze welding wire obtained in step S1, deposit it layer by layer on the surface of the substrate, and obtain a nickel-aluminum bronze molded part. The process parameters of laser additive manufacturing using the laser additive manufacturing system are: laser power: 2000-3000W, the angle between the welding wire and the horizontal substrate is 20-35°, the welding wire dry extension is 10-15mm, the wire output speed is 10-24mm / s, the laser beam scanning speed is 5-13mm / s, the layer height is 0.2-0.3 mm, and the gas flow rate is 4-6L / min; S3, heat-treating the nickel-aluminum bronze molded part obtained in step S2 to obtain a nickel-aluminum bronze alloy material, wherein the heat treatment comprises the following steps: 1) Annealing treatment: keep at 600-640℃ for 2-3.5h, and cool with the furnace; 2) Aging treatment: keep at 850-900℃ for 3.5-4.5h, quench; then keep at 400-450℃ for 1h, cool with the furnace.
2. The method for preparing the nickel-aluminum-bronze alloy material for plastic mold according to claim 1, characterized in that: The elements and mass percentages contained in the raw materials of the nickel-aluminum bronze alloy material include: Al 8.3-8.8%, Ni 3.0-4.0%, Fe3.5-4.5%, Mn 2.8-3.5%, Ti 1.1-1.6%, La 0.3-0.6%, Sr 0.02-0.12%, and the balance is copper.
3. The method for preparing the nickel-aluminum-bronze alloy material for plastic mold according to claim 1, characterized in that: In step S1, the raw material is pretreated The following steps are involved: a: Place the raw materials in a vacuum melting chamber and melt them at 1050-1150℃ for 40-60 min to obtain alloy liquid; b: heating the alloy liquid obtained in step a to 1100-1300° C., performing horizontal continuous casting to obtain a bar, hot rolling, pickling, and obtaining an alloy bar; c: straightening the alloy rod obtained in step b, applying lubricating oil, drawing, annealing, furnace cooling, sizing, and scraping to obtain alloy wire; d: etching the alloy wire obtained in step c, cleaning, drying, coating with a composite coating, and drying to obtain a nickel-aluminum bronze welding wire.
4. The method for preparing the nickel-aluminum bronze alloy material for plastic mold according to claim 3, characterized in that: In the step d, the alloy wire is immersed in an etchant for etching, wherein the etchant comprises 5-8wt% of citric acid, 2-5wt% of sulfuric acid and 2-3wt% of triethanolamine.
5. The method for preparing the nickel-aluminum-bronze alloy material for plastic mold according to claim 3, characterized in that: In the step d, the composite coating comprises a binder and metal powder in a weight ratio of 2-5:2-3, and the metal powder comprises TiO2 and CeO2.
6. The method for preparing the nickel-aluminum-bronze alloy material for plastic mold according to claim 1, characterized in that: In the step S1, the raw materials include pure aluminum, pure iron, pure nickel, pure manganese and pure copper.
7. The method for preparing the nickel-aluminum-bronze alloy material for plastic mold according to claim 1, characterized in that: In step S2, the substrate is surface treated by sequentially cleaning, grinding, cleaning and drying.
8. The method for preparing the nickel-aluminum-bronze alloy material for plastic mold according to claim 1, characterized in that: In the step S2, during the laser additive manufacturing process, the welding wire and the laser beam are controlled to start from a layer of the substrate and to be reciprocated layer by layer. The height of each layer of welding wire and laser beam is set to 3.0 mm, and the cooling time between layers is 10 seconds.
Citation Information
Patent Citations
Zirconium and strontium compound micro-alloyed nickel-aluminum bronze and preparation method thereof
CN102899523A
Nickel-aluminum bronze alloy and preparation method thereof
CN104862522A
Ultra-short period high-strength and high-ductility nickel-aluminum-bronze alloy and preparing method
CN109628772A
Nickel-aluminum bronze laser additive manufacturing method
CN114855015A
Cavitation-corrosion-resistant high-manganese aluminum bronze welding wire for repairing propeller and manufacturing method of cavitation-corrosion-resistant high-manganese aluminum bronze welding wire
CN115213584A