Electronic polycrystalline silicon multipurpose functional inner packaging material and preparation method thereof
By using conductive materials prepared by the crack template method and self-made cross-linking agents in electronic-grade polysilicon packaging materials, the problem of metal contamination and performance degradation caused by electrostatic field elimination is solved, efficient and low-cost static management is achieved, and the material is ensured stability and security.
Patent Information
- Application Number
- CN202411227092.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing electronic-grade polysilicon packaging materials can easily cause metal contamination when eliminating electrostatic fields, resulting in reduced performance, increased use of additives, increased processing difficulty, and poor material compatibility, resulting in high costs and environmental pollution.
The polyethylene film is prepared using the crack template method. Cracks are evenly distributed on the surface of the inner film and filled with conductive material prepared by self-made cross-linking agent. The conductive material is evenly distributed in the cracks to form a three-layer structure with high strength, high barrier properties and high conductivity. membrane to prevent electrostatic fields from accumulating on the inner membrane.
It achieves the rapid elimination of electrostatic interference, avoids metal pollution, reduces material costs, simplifies process difficulty, improves the overall performance of packaging materials, and ensures the safe storage of polysilicon.
Smart Images

Figure CN118721925A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of packaging materials and relates to a multi-purpose functional inner packaging material for electronic polysilicon and a preparation method thereof. Background Art
[0002] Electronic-grade polysilicon is an important electronic material. It is a product that uses industrial silicon as raw material and reaches a certain purity after a series of physical and chemical reactions. In the silicon product industry chain, electronic-grade polysilicon is an extremely important intermediate product, which is widely used in the manufacture of silicon polishing sheets, solar cells and high-purity silicon products. At the same time, it is also the most basic raw material for the information industry and new energy industry.
[0003] At present, the commonly used packaging materials for electronic-grade polysilicon are generally polyethylene (PE) or low-density polyethylene (LDPE) packaging bags. These materials have good corrosion resistance, oxidation resistance and heat resistance, and can effectively protect polysilicon from the influence of the external environment; electronic-grade polysilicon packaging materials not only need to have good corrosion resistance, oxidation resistance, heat resistance, high strength, etc., but also need to have excellent anti-static properties. Once static electricity is generated in the packaging material during use, polysilicon is easily adsorbed on the inner surface of the packaging bag, and additional operations are required to recover the polysilicon on the inner wall of the packaging bag, which not only increases the cost of transportation, material collection and other processing processes, but also causes polysilicon waste if the polysilicon cannot be completely recovered.
[0004] In order to make the packaging materials have excellent antistatic properties, the prior art generally introduces conductive materials such as metals, graphene, carbon black, etc. into the raw materials as antistatic agents. There are incompatibility issues between metals, graphene, carbon black, etc. and other materials in the packaging bag, especially metals. During use, the packaging bag is prone to precipitate metals, and the precipitated metals will cause metal pollution to the polysilicon. Although the antistatic function of the packaging bag is enhanced, it brings more serious metal pollution. In addition, after the addition of metals, graphene, carbon black and other materials, the transparency, fluidity, uniformity, etc. of the packaging material will decrease, and a large amount of additives will be needed to adjust the performance of the packaging material, which not only increases the material cost, environmental pollution risk, and process difficulty, but also makes the compatibility problem between the various substances more severe. The more substances there are, the greater the risk of incompatibility between the substances. If the substances are incompatible, high-quality packaging materials cannot be obtained. Summary of the invention
[0005] The purpose of the present invention is to provide a multi-purpose functional inner packaging material for electronic polysilicon and a preparation method thereof, which solves the problems that the current use of conductive materials such as metals, graphene, carbon black, etc. to eliminate the electrostatic field of packaging materials will bring about metal pollution, reduced performance of packaging materials, increased use of additives, increased processing difficulty, etc.
[0006] The technical solution adopted by the present invention is as follows: A multi-purpose functional inner packaging material for electronic polysilicon, comprising an inner film and an outer film laminated together, wherein the inner film is a polyethylene film, and the inner film is prepared based on a crack template method, and cracks are evenly distributed on the outer surface of the inner film, and a conductive material is filled between the inner film and the outer film, and the conductive material is evenly distributed between the inner film and the outer film, and the conductive material is filled in the cracks on the outer surface of the inner film; The conductive material is a conductive adhesive layer obtained by cross-linking polyvinyl alcohol under the action of a self-made cross-linking agent, and the self-made cross-linking agent is 4-(2-aminophenyl)-pyridine-3-oxacyclo-5-thiophene-2-acyl; The preparation method of the self-made cross-linking agent comprises the following steps: A. Under alkaline conditions, hydroquinone and benzaldehyde are subjected to Aldour condensation reaction to obtain dihydroxydiphenylmethane, and then, the dihydroxydiphenylmethane is converted into a benzene derivative by Bergmann cyclization reaction at 200°C; B. Using dimethyl sulfoxide as solvent, the prepared benzene derivative is subjected to condensation and cyclization reaction with 4-chloro-3-nitropyridine and 3-oxacyclo-5-thiophene-2-carboxaldehyde to obtain 4-(2-aminophenyl)-pyridine-3-oxacyclo-5-thiophene-2-acyl.
[0007] The present invention uses the method of slitting and filling to modify the polyethylene film. The present invention uses the crack template method to prepare the inner film. The outer surface of the inner film is evenly distributed with cracks, and the cracks cut off the movement path of the charges on the inner film. In order to ensure the integrity of the inner film and the strength of the overall packaging film, the present invention adheres the outer film to the outer side of the inner film, and fills the cracks with conductive materials. The conductive materials are filled in the cracks because they have good conductivity. When charges are generated on the surface of the inner film to form an electrostatic field, the conductive materials transfer the charges on the inner film to the outer film, so that no static electricity is generated on the inner film, and polysilicon will not be adsorbed. After the charges on the inner film come into contact with the conductive material, the charges will be absorbed by the conductive material and move along the path of the conductive material to the outer film. In this process, the conductive material acts as a bridge, realizing the transfer of charges from the inner film to the outer film.
[0008] The cracks in the present invention cut off the movement path of the charges on the inner film, which can eliminate electrostatic interference to a certain extent on the one hand; on the other hand, the cracks are filled with conductive materials, which will adsorb the charges on the inner film, so that a larger potential difference is generated between the position of the crack and other positions of the inner film. The larger the potential difference, the faster the charge movement speed and the larger the amount of charge transferred, which can quickly and efficiently transfer the charges on the inner film to the outer film, thereby eliminating the electrostatic interference of the inner film.
[0009] After cracks are opened on the inner film in the present invention, the integrity of the inner film is reduced and the comprehensive properties of the inner film such as barrier properties and strength will be reduced. Therefore, the present invention fills the cracks with conductive materials, and then uses the conductive materials as adhesives to adhere the outer film. The combination of the outer film and the conductive material avoids the adverse effects caused by the cracks in the inner film.
[0010] Commonly used conductive materials in the prior art are metals, graphene, carbon black and other materials. The above materials have poor compatibility with polymers. During use, the above substances will also be partially precipitated, causing metal pollution in the polysilicon inside the packaging bag. Therefore, the present invention prepares a new conductive material, using polyvinyl alcohol as the main film-forming and adhesive material, and then adding 4-(2-aminophenyl)-pyridine-3-oxacyclic-5-thiophene-2-acyl, 4-(2-aminophenyl)-pyridine-3-oxacyclic-5-thiophene-2-acyl as a crosslinker for polyvinyl alcohol, and amino groups, acyl groups and polyvinyl alcohol can be crosslinked under heating and stirring. Reaction, so that the cross-linked network between polyvinyl alcohol molecules is formed, and a stable three-dimensional network structure is obtained, which has high mechanical strength, thermal stability and chemical resistance after film formation; in addition, 4-(2-aminophenyl)-pyridine-3-oxacyclic-5-thiophene-2-acyl contains a benzene ring and a pyridine ring, providing the π electron system required by the present invention, and the introduction of amino and acyl groups enhances the polarity of the compound, and can undergo a cross-linking reaction with the polymer, and has high interfacial adhesion with the film surface; in the present invention, the thiophene unit is a conjugated system, and the introduction of the thiophene unit not only increases the π electron density of the molecule, but also helps to form a more effective electron transmission channel. The 4-(2-aminophenyl)-pyridine-3-oxacyclic-5-thiophene-2-acyl of the present invention combines a benzene ring, a pyridine ring and a conjugated system, and at the same time introduces a hydrogen bonding functional group through an amino group and an oxygen heterocycle, which not only has good chemical stability and thermal stability, but also exhibits excellent electrical properties.
[0011] The 4-(2-aminophenyl)-pyridine-3-oxacyclo-5-thiophene-2-acyl prepared by the present invention is a new cross-linking agent. When acting on the cross-linking reaction of polyvinyl alcohol, only these two substances can be used to obtain a conductive colloid with strong conductivity, no precipitation of harmful substances, stable performance, strong viscosity, high barrier property after film formation and high strength. In the prior art, in order to prepare a colloid with the above functions, a mixed reaction of multiple substances is required, which not only increases the energy consumption, but also increases the compatibility difficulty between substances. In the reaction process, the more reactants there are, the more difficult it is to control the compatibility between the reactants, the greater the reaction difficulty, and the more by-products are generated. Therefore, the present invention uses Aldore condensation reaction, Bergmann cyclization reaction and the like to prepare a new cross-linking agent capable of cross-linking and modifying polyvinyl alcohol. The new cross-linking agent has excellent conductive properties and replaces existing conductive materials such as metals, carbon black, graphene, etc., which reduces the material use cost on the one hand and eliminates the risk of precipitation of conductive materials such as metals, carbon black, graphene, etc. on the other hand.
[0012] The conductive material of the present invention is a film-forming colloid material, which can form a film with high strength, high barrier property and high conductivity, and is combined with an inner film and an outer film to form a multifunctional film with a three-layer structure.
[0013] In summary, the principle of eliminating static electricity on the surface of the inner film of the present invention is as follows: the present invention first uses cracks to cut off the movement path of the charges on the surface of the inner film, and then uses a conductive material with better conductivity than the inner film as a filling material to change the movement path of the charges. The charges no longer move on the inner film, but are transferred from the inner film to the conductive material, and then from the conductive material to the outer film in contact with the conductive material; during the process of the conductive material transferring point charges, the charges on the inner film will continue to move from the inner film to the conductive material. In the present invention, the outer film can be an existing film, for example: one of polyamide film, polyvinyl alcohol film, and polyester film. Polyamide film, polyvinyl alcohol film, and polyester film have good compatibility with conductive materials and high interfacial adhesion strength. In the present invention, the outer film can also be a self-made new film.
[0014] Since polyethylene is a non-polar polymer, it has very weak interactions with other substances and stable chemical properties. Therefore, the present invention uses polyethylene film as the inner layer film. Polyethylene film is also a widely used film with low production cost and mature technology.
[0015] Polyvinyl alcohol has excellent barrier properties. Therefore, the present invention selects polyvinyl alcohol as the main film-forming substance in the conductor material. In addition, after the cross-linking reaction between polyvinyl alcohol and 4-(2-aminophenyl)-pyridine-3-oxacyclic-5-thiophene-2-acyl, the performance of the polyvinyl alcohol film can be enhanced without affecting the conductive properties of 4-(2-aminophenyl)-pyridine-3-oxacyclic-5-thiophene-2-acyl.
[0016] Furthermore, the mass ratio of polyvinyl alcohol to the homemade cross-linking agent in the conductive material is 7.2-7.5:1.
[0017] The present invention optimizes the mass ratio of polyvinyl alcohol to a self-made crosslinking agent. The amount of the crosslinking agent added will have a significant effect on the crosslinking of polyethanol. When the amount of the crosslinking agent added is insufficient, the number of crosslinking points between polymer chains will be reduced, resulting in a decrease in the mechanical properties of the material, which cannot meet the use requirements; when the crosslinking agent is excessive, the excessive crosslinking agent will lead to too many crosslinking points, causing the polymer to form a large number of crosslinked structures, which may affect the physical properties of the polymer, such as hardness and toughness, and may even cause the polymer to be unable to form a uniform structure, thereby affecting its application effect.
[0018] Furthermore, the mass ratio of polyvinyl alcohol to the homemade cross-linking agent in the conductive material is 7.4:1.
[0019] In consideration of the cost of materials and the performance of packaging materials, the present invention optimizes the best ratio.
[0020] Furthermore, the outer film comprises component A and component B, and the mass of component B is 1-2% of the mass of component A; The component A comprises the following components: polyvinyl alcohol, furan-based copolyester, solvent, and photosensitive catalyst, wherein the solvent is dimethylformamide, the photosensitive catalyst is benzophenone, the mass ratio of polyvinyl alcohol to furan-based copolyester is 1.5:1, 10 ml of solvent is used for 1 g of the total amount of polyvinyl alcohol and furan-based copolyester, and the mass of the photosensitive catalyst is 1.2-1.4% of the total amount of polyvinyl alcohol and furan-based copolyester; The component B consists of the following components: 100 wt% of nano-layered silicate-modified PVA; The component A is used to prepare the base film of the outer film, and the component B is used to prepare the coating layer of the outer layer of the base film.
[0021] The outer film of the present invention does not use a single olefin structure, but uses a new polymer obtained by mixing polyvinyl alcohol and furan-based copolyester as a base film, and then uses nano-layered silicate-modified PVA with good compatibility with polyvinyl alcohol as a coating layer. The prepared outer film contains ether bonds, and the oxygen atoms in the ether bonds have high electronegativity, which makes the reactivity of the ether compounds low and not easy to chemically react. This stability enables the film material containing ether bonds to maintain a long service life and stable performance during use; in addition, the new polymer obtained by the reaction of polyvinyl alcohol and furan-based copolyester under photosensitive catalyst and light conditions has good transparency and water resistance.
[0022] Further, the mass of component B is 1.5% of the mass of component A; The component A comprises the following components: polyvinyl alcohol, furan-based copolyester, solvent, and photosensitive catalyst. The solvent is dimethylformamide, the photosensitive catalyst is benzophenone, the mass ratio of polyvinyl alcohol to furan-based copolyester is 1.5:1, 10 ml of solvent is used for 1 g of the total amount of polyvinyl alcohol and furan-based copolyester, and the mass of the photosensitive catalyst is 1.3% of the total amount of polyvinyl alcohol and furan-based copolyester.
[0023] Furthermore, the outer layer film is prepared by the following method: a. Prepare a base film with component A: use dimethylformamide as solvent, dissolve polyvinyl alcohol and furan-based copolyester in dimethylformamide, stir evenly, add benzophenone, continue stirring and heat to 40°C, and then irradiate the reactants with ultraviolet light. Under the irradiation of ultraviolet light, benzophenone induces an etherification reaction between polyvinyl alcohol and furan-based copolyester, combines the hydroxyl group in PVA with the hydroxyl group in furan-based copolyester to form an ether bond, and obtains a new copolymer containing an ether bond. The new copolymer is formed and cooled to obtain a base film; b. Coating: A coating machine is used to coat the nano-layered silicate-modified PVA on the outer surface of the base film to obtain an outer film, and the inner surface of the outer film is bonded to the inner film through a conductive material.
[0024] The present invention combines the two processes of photosensitization reaction and coating, and the obtained outer film has high barrier properties, high pressure resistance, high stability and other properties. After the charge on the inner film is transferred to the outer film, an electrostatic field will be formed on the outer film. The formation of the electrostatic field will have an adverse effect on the performance of the film to a certain extent. For example, the electrostatic field will cause the outer film to produce electrostatic adsorption on charged particles or particles in the surrounding environment. This adsorption may affect the surface properties of the film, such as wettability, air permeability, and permeability. In order to reduce the significant adverse effect of the electrostatic field on the outer film on the entire packaging material, the present invention improves the outer film, and the obtained outer film with superior comprehensive performance can withstand and buffer the adverse effects of the electrostatic field. The final obtained inner packaging material has good comprehensive performance.
[0025] Furthermore, the crack on the surface of the inner membrane is an inverted trumpet-shaped structure that expands inward and contracts outward, with the narrow end of the crack close to the outer membrane and the wide side of the crack close to the inner side of the inner membrane.
[0026] The structure of the crack in the present invention is a trumpet-shaped structure. The inside and outside of the crack are determined by referring to the inner and outer surfaces of the inner film. The side close to the inner surface of the inner film is the inner side of the crack, and the side close to the outer surface of the inner film is the outer side of the crack. The present invention utilizes the charge tip effect. The curvature of the conductor tip is large, and the number of charges per unit area is large, resulting in a particularly strong electric field intensity near this part. This strong electric field will attract charges and make them more likely to move to the conductor tip. Therefore, in order to increase the amount of charge transfer in the inner film, the present invention sets the gap structure to a trumpet-shaped structure. The width of the gap gradually decreases from the inside to the outside. The conductive structure formed after the conductive material in the gap is solidified also gradually decreases in diameter or width from the inside to the outside. The outer layer of the conductive structure is equivalent to a tip, so that the charge is concentrated here, so that the static elimination effect of the inner film is better and more efficient.
[0027] Furthermore, the wide side opening width d1 of the crack is 3-4 times the narrow side opening width d2.
[0028] The present invention combines the difficulty of the processing technology and the static elimination effect of the inner film, and optimizes the optimal width ratio of d1 to d2.
[0029] A method for preparing a multi-purpose functional inner packaging material for electronic polycrystalline silicon comprises the following steps: S1. preparing an inner layer film: using molten polyethylene resin to prepare a polyethylene inner layer film having cracks distributed on the surface based on a crack template method; S2. preparing a conductive material; S2.1 Preparation of homemade cross-linking agent A. Under alkaline conditions, hydroquinone and benzaldehyde are subjected to Aldour condensation reaction to obtain dihydroxydiphenylmethane, and then, the dihydroxydiphenylmethane is converted into a benzene derivative by Bergmann cyclization reaction at 200°C; B. Using dimethyl sulfoxide as solvent, the prepared benzene derivative is subjected to condensation and cyclization reaction with 4-chloro-3-nitropyridine and 3-oxacyclo-5-thiophene-2-carboxaldehyde to obtain 4-(2-aminophenyl)-pyridine-3-oxacyclo-5-thiophene-2-acyl; S2.2 Cross-linking reaction Under the protection of an inert gas (such as nitrogen), PVA and 4-(2-aminophenyl)-pyridine-3-oxacyclic-5-thiophene-2-acyl are dissolved in a solvent respectively. After dissolution, the PVA solution and the 4-(2-aminophenyl)-pyridine-3-oxacyclic-5-thiophene-2-acyl solution are mixed, and after mixing evenly, they are heated while stirring. After heating to 80° C., the reaction is carried out at a constant temperature. After reacting for 8-10 hours, the reaction is stopped, and the reaction mixture is cooled, filtered, and evaporated to remove the solvent to obtain a conductive material; S3, preparing outer membrane: The outer film comprises component A and component B; The component A comprises the following components: polyvinyl alcohol, furan-based copolyester, solvent, and photosensitive catalyst, wherein the solvent is dimethylformamide and the photosensitive catalyst is benzophenone; The component B consists of the following components: 100 wt% of nano-layered silicate-modified PVA; a. Prepare a base film with component A: use dimethylformamide as solvent, dissolve polyvinyl alcohol and furan-based copolyester in dimethylformamide, stir evenly, add benzophenone, continue stirring and heat to 40°C, and then irradiate the reactants with ultraviolet light. Under the irradiation of ultraviolet light, benzophenone induces an etherification reaction between polyvinyl alcohol and furan-based copolyester, combines the hydroxyl group in PVA with the hydroxyl group in furan-based copolyester to form an ether bond, and obtains a new copolymer containing an ether bond. The new copolymer is formed and cooled to obtain a base film; b. Coating: The nano-layered silicate-modified PVA is coated on the outer surface of the base film by a coating machine to obtain an outer film, and the inner surface of the outer film is bonded to the inner film by a conductive material; S4. Preparation of composite film: The conductive material prepared in step S2 is evenly sprayed on the outer surface of the inner film, the conductive material evenly covers the outer surface of the inner film and fills the cracks on the outer surface of the inner film with the conductive material, a conductive layer is formed after the conductive material is sprayed, and then the outer film is pressed on the conductive layer, the inner surface of the outer film is tightly fitted with the conductive layer, and then after pressing, cooling and forming, a multi-purpose functional inner packaging material for electronic polysilicon is prepared.
[0030] Furthermore, the depth of the cracks on the surface of the inner film is 3 / 5-2 / 3 of the thickness of the inner film.
[0031] The crack in the present invention may penetrate both the inner and outer sides of the inner film, or may not penetrate through the inner film; the static elimination effect is better after the crack penetrates the inner film, but the inner surface of the inner film will become uneven after the inner film is penetrated, which may cause material jam; therefore, the present invention ensures the integrity of the inner film while ensuring a better static elimination effect, adopts a structure in which the crack does not penetrate through the inner film, and selects the optimal crack depth.
[0032] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are: 1. The crack of the multi-purpose functional inner packaging material for electronic polysilicon of the present invention cuts off the moving path of the charge on the inner film, which can eliminate electrostatic interference to a certain extent; on the other hand, the crack is filled with conductive material, which will absorb the charge on the inner film, so that a large potential difference is generated between the position where the crack is located and other positions of the inner film. The larger the potential difference, the faster the charge movement speed and the larger the amount of charge transferred, which can quickly and efficiently transfer the charge on the inner film to the outer film, thereby eliminating the electrostatic interference of the inner film; 2. The 4-(2-aminophenyl)-pyridine-3-oxacyclo-5-thiophene-2-acyl obtained from the multi-purpose functional inner packaging material of electronic polysilicon of the present invention is a new cross-linking agent, which acts on the cross-linking reaction of polyvinyl alcohol. Only these two substances can obtain a conductive colloid with strong conductivity, no precipitation of harmful substances, stable performance, strong viscosity, high barrier properties after film formation, and high strength. It is equivalent to one substance realizing multiple functions and replacing the existing additives for adjusting multiple functionalities.
[0033] 3. The preparation method of the multi-purpose functional inner packaging material of electronic polysilicon of the present invention modifies the polyethylene film by means of slitting and filling, thereby solving the problem that the current use of conductive materials such as metals, graphene, carbon black, etc. to eliminate the electrostatic field of packaging materials will bring about metal pollution, reduced performance of packaging materials, increased use of additives, increased processing difficulty, and other shortcomings. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative work, among which: Figure 1 Schematic diagram of the inner film structure of the present invention; Figure 2 is an enlarged view of part A of the present invention; Figure 3 is the infrared spectrum of the cross-linking agent of the present invention; Markings in the figure: 1-inner membrane, 2-gap. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all of the embodiments. The components of the embodiments of the present invention described and shown in the drawings herein can be arranged and designed in various different configurations.
[0036] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present invention.
[0037] It should be noted that relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0038] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0039] Example 1 A preferred embodiment of the present invention provides a multi-purpose functional inner packaging material for electronic polysilicon, comprising an inner film 1 and an outer film that are bonded together, wherein the conductivity of the outer film is better than that of the inner film; the inner film is a polyethylene film, and the inner film is prepared based on a crack template method, and cracks 2 are evenly distributed on the outer surface of the inner film 1, and a conductive material is filled between the inner film and the outer film, and the conductive material is evenly distributed between the inner film and the outer film and is filled in the cracks on the surface of the inner film; the depth of the cracks on the surface of the inner film is 2 / 3 of the thickness of the inner film; The conductive material is a conductive adhesive layer obtained by cross-linking polyvinyl alcohol under the action of a self-made cross-linking agent, and the self-made cross-linking agent is 4-(2-aminophenyl)-pyridine-3-oxacyclo-5-thiophene-2-acyl; The preparation method of the self-made cross-linking agent comprises the following steps: A. Under alkaline conditions, hydroquinone and benzaldehyde are subjected to Aldour condensation reaction to obtain dihydroxydiphenylmethane, and then, the dihydroxydiphenylmethane is converted into a benzene derivative by Bergmann cyclization reaction at 200°C; B. Using dimethyl sulfoxide as solvent, the prepared benzene derivative is subjected to condensation and cyclization reaction with 4-chloro-3-nitropyridine and 3-oxacyclo-5-thiophene-2-carboxaldehyde to obtain 4-(2-aminophenyl)-pyridine-3-oxacyclo-5-thiophene-2-acyl.
[0040] The mass ratio of polyvinyl alcohol to the homemade cross-linking agent in the conductive material is 7.4:1.
[0041] The outer film comprises component A and component B, wherein the mass of component B is 1.5% of the mass of component A; The component A comprises the following components: polyvinyl alcohol, furan-based copolyester, solvent, and photosensitive catalyst, wherein the solvent is dimethylformamide, the photosensitive catalyst is benzophenone, the mass ratio of polyvinyl alcohol to furan-based copolyester is 1.5:1, 10 ml of solvent is used for 1 g of the total amount of polyvinyl alcohol and furan-based copolyester, and the mass of the photosensitive catalyst is 1.3% of the total amount of polyvinyl alcohol and furan-based copolyester; The component B consists of the following components: 100 wt% of nano-layered silicate-modified PVA; The component A is used to prepare the base film of the outer film, and the component B is used to prepare the coating layer of the outer layer of the base film.
[0042] The outer layer membrane is prepared by the following method: a. Prepare a base film with component A: use dimethylformamide as solvent, dissolve polyvinyl alcohol and furan-based copolyester in dimethylformamide, stir evenly, add benzophenone, continue stirring and heat to 40°C, and then irradiate the reactants with ultraviolet light. Under the irradiation of ultraviolet light, benzophenone induces an etherification reaction between polyvinyl alcohol and furan-based copolyester, combines the hydroxyl group in PVA with the hydroxyl group in furan-based copolyester to form an ether bond, and obtains a new copolymer containing an ether bond. The new copolymer is formed and cooled to obtain a base film; b. Coating: A coating machine is used to coat the nano-layered silicate-modified PVA on the outer surface of the base film to obtain an outer film, and the inner surface of the outer film is bonded to the inner film through a conductive material.
[0043] A method for preparing a multi-purpose functional inner packaging material for electronic polycrystalline silicon, characterized in that it comprises the following steps: S1. preparing an inner layer film: using molten polyethylene resin to prepare a polyethylene inner layer film having cracks distributed on the surface based on a crack template method; S2. preparing a conductive material; S2.1 Preparation of homemade cross-linking agent A. Under alkaline conditions, hydroquinone and benzaldehyde are subjected to Aldour condensation reaction to obtain dihydroxydiphenylmethane, and then, the dihydroxydiphenylmethane is converted into a benzene derivative by Bergmann cyclization reaction at 200°C; B. Using dimethyl sulfoxide as solvent, the prepared benzene derivative is subjected to condensation and cyclization reaction with 4-chloro-3-nitropyridine and 3-oxacyclo-5-thiophene-2-carboxaldehyde to obtain 4-(2-aminophenyl)-pyridine-3-oxacyclo-5-thiophene-2-acyl; S2.2 Cross-linking reaction Under the protection of an inert gas (such as nitrogen), PVA and 4-(2-aminophenyl)-pyridine-3-oxacyclic-5-thiophene-2-acyl are dissolved in a solvent respectively. After dissolution, the PVA solution and the 4-(2-aminophenyl)-pyridine-3-oxacyclic-5-thiophene-2-acyl solution are mixed, and after mixing evenly, they are heated while stirring. After heating to 80° C., the reaction is carried out at a constant temperature. After reacting for 8-10 hours, the reaction is stopped, and the reaction mixture is cooled, filtered, and evaporated to remove the solvent to obtain a conductive material; S3, preparing outer membrane: The outer film comprises component A and component B; The component A comprises the following components: polyvinyl alcohol, furan-based copolyester, solvent, and photosensitive catalyst, wherein the solvent is dimethylformamide and the photosensitive catalyst is benzophenone; The component B consists of the following components: 100 wt% of nano-layered silicate-modified PVA; a. Prepare a base film with component A: use dimethylformamide as solvent, dissolve polyvinyl alcohol and furan-based copolyester in dimethylformamide, stir evenly, add benzophenone, continue stirring and heat to 40°C, and then irradiate the reactants with ultraviolet light. Under the irradiation of ultraviolet light, benzophenone induces an etherification reaction between polyvinyl alcohol and furan-based copolyester, combines the hydroxyl group in PVA with the hydroxyl group in furan-based copolyester to form an ether bond, and obtains a new copolymer containing an ether bond. The new copolymer is formed and cooled to obtain a base film; b. Coating: The nano-layered silicate-modified PVA is coated on the outer surface of the base film by a coating machine to obtain an outer film, and the inner surface of the outer film is bonded to the inner film by a conductive material; S4. Preparation of composite film: The conductive material prepared in step S2 is evenly sprayed on the outer surface of the inner film, the conductive material evenly covers the outer surface of the inner film and fills the cracks on the outer surface of the inner film with the conductive material, a conductive layer is formed after the conductive material is sprayed, and then the outer film is pressed on the conductive layer, the inner surface of the outer film is tightly fitted with the conductive layer, and then after pressing, cooling and forming, a multi-purpose functional inner packaging material for electronic polysilicon is prepared.
[0044] Figure 3 The infrared spectrum of 4-(2-aminophenyl)-pyridine-3-oxacyclo-5-thiophene-2-yl of the present invention is shown in the figure. The 500-1500 cm -1 There are multiple absorption peaks in the thiophene ring, corresponding to the vibration mode of the thiophene ring; at 1700-1800 cm -1 There is a strong absorption peak in the range of 1500-1600 cm -1 There are multiple absorption peaks in the range of 1150-1350 cm -1 CN stretching vibration peaks appear in the region; at 2850-3000 cm- 1 CH stretching vibration appears in the region; in the range of 3300-3500 cm- 1 An absorption peak appears in the region, which corresponds to the characteristic absorption peak of the amino group. In summary, the present invention successfully prepares a compound named 4-(2-aminophenyl)-pyridine-3-oxacyclo-5-thiophene-2-yl.
[0045] like Figure 1 , Figure 2 As shown, the crack on the surface of the inner film 1 is a trumpet-shaped structure that expands inward and contracts outward, the narrow end of the crack 2 is close to the outer film, and the wide side of the crack is close to the inner side of the inner film. The wide side opening width d1 of the crack is 4 times the narrow end opening width d2.
[0046] Example 2 Based on Example 1, the difference from Example 1 is that the mass ratio of polyvinyl alcohol to the homemade cross-linking agent in the conductive material is 7.2:1.
[0047] Example 3 Based on Example 1, the difference from Example 1 is that the mass ratio of polyvinyl alcohol to the homemade cross-linking agent in the conductive material is 7.5:1.
[0048] Example 4 Based on Example 1, the difference from Example 1 is that: the outer layer film includes component A and component B, and the mass of component B is 1% of the mass of component A.
[0049] Example 5 Based on Example 1, the difference from Example 1 is that: the outer layer film includes component A and component B, and the mass of component B is 2% of the mass of component A.
[0050] Example 6 Based on Example 1, the difference from Example 1 is that the component A includes the following components: polyvinyl alcohol, furan-based copolyester, solvent, and photosensitive catalyst, the solvent is dimethylformamide, the photosensitive catalyst is benzophenone, the mass ratio of polyvinyl alcohol and furan-based copolyester is 1.5:1, 10 ml of solvent is used for 1 g of the total amount of polyvinyl alcohol and furan-based copolyester, and the mass of the photosensitive catalyst is 1.2% of the total amount of polyvinyl alcohol and furan-based copolyester.
[0051] Example 7 Based on Example 1, the difference from Example 1 is that the component A includes the following components: polyvinyl alcohol, furan-based copolyester, solvent, and photosensitive catalyst, the solvent is dimethylformamide, the photosensitive catalyst is benzophenone, the mass ratio of polyvinyl alcohol and furan-based copolyester is 1.5:1, 10 ml of solvent is used for 1 g of the total amount of polyvinyl alcohol and furan-based copolyester, and the mass of the photosensitive catalyst is 1.4% of the total amount of polyvinyl alcohol and furan-based copolyester.
[0052] Example 8 Based on Example 1, the difference from Example 1 is that the crack on the surface of the inner membrane is a trumpet-shaped structure that expands inward and contracts outward, the narrow end of the crack is close to the outer membrane, and the wide side of the crack is close to the inner side of the inner membrane, and the wide side of the crack has a slit width d1 that is 3 times the narrow end slit width d2.
[0053] Example 9 Based on Example 1, the difference from Example 1 is that the wide side opening width d1 of the crack is 3.5 times the narrow side opening width d2.
[0054] Example 10 Based on Example 1, the difference from Example 1 is that the crack is a rectangular structure with the same width inside and outside.
[0055] Embodiment 11 This embodiment is based on the embodiment 1, but is different from the embodiment 1 in that the depth of the crack on the surface of the inner film is 3 / 5 of the thickness of the inner film.
[0056] Comparative Example 1 Different from Example 1, the conductive material in this comparative example includes polyvinyl alcohol and copper powder, and the amount of copper powder added is the same as the amount of 4-(2-aminophenyl)-pyridine-3-oxacyclo-5-thiophene-2-yl. The polyvinyl alcohol mixed with copper powder is sprayed as a conductive adhesive layer between the inner film and the outer film to fill the gap. The other parts are the same as Example 1.
[0057] Comparative Example 2 Different from Example 1, the mass ratio of polyvinyl alcohol to the homemade cross-linking agent in the conductive material is 7.6:1.
[0058] Insufficient amount of cross-linking agent leads to insufficient cross-linking points and reduced overall performance.
[0059] Comparative Example 3 Different from Example 1, the mass ratio of polyvinyl alcohol to the homemade cross-linking agent in the conductive material is 7.1:1.
[0060] Excessive cross-linking will reduce tensile and compressive strength.
[0061] Comparative Example 4 The difference from Example 1 is that the outer film includes component A and component B, and the mass of component B is 0.5% of the mass of component A.
[0062] Comparative Example 5 Different from Example 1, the outer film includes component A and component B, and the mass of component B is 2.5% of the mass of component A.
[0063] Comparative Example 6 Based on Example 1, this comparative example is different from Example 1 in that: the component A includes the following components: polyvinyl alcohol, furan-based copolyester, solvent, and photosensitive catalyst, the solvent is dimethylformamide, the photosensitive catalyst is benzophenone, the mass ratio of polyvinyl alcohol and furan-based copolyester is 1.5:1, 10 ml of solvent is used for 1 g of the total amount of polyvinyl alcohol and furan-based copolyester, and the mass of the photosensitive catalyst is 1.1% of the total amount of polyvinyl alcohol and furan-based copolyester.
[0064] Comparative Example 7 Based on Example 1, this comparative example is different from Example 1 in that: the component A includes the following components: polyvinyl alcohol, furan-based copolyester, solvent, and photosensitive catalyst, the solvent is dimethylformamide, the photosensitive catalyst is benzophenone, the mass ratio of polyvinyl alcohol to furan-based copolyester is 1.5:1, 10 ml of solvent is used for 1 g of the total amount of polyvinyl alcohol and furan-based copolyester, and the mass of the photosensitive catalyst is 1.5% of the total amount of polyvinyl alcohol and furan-based copolyester.
[0065] Comparative Example 8 Based on Example 1, the difference between this comparative example and Example 1 is that the outer layer film of this comparative example adopts polyvinyl alcohol film.
[0066] Comparative Example 9 Based on Example 1, the difference between this comparative example and Example 1 is that: in this comparative example, there is no crack on the inner layer film, and a polyethylene film with a smooth and flat surface is directly prepared by the existing blow molding or extrusion molding method; the conductive material is still evenly sprayed between the inner layer film and the outer layer film, and the thickness of the conductive material after film formation is consistent with the film thickness of the conductive material in Example 1 excluding the portion with crack depth.
[0067] Comparative Example 10 Based on Example 1, the difference between this comparative example and Example 1 is that the depth of the crack on the surface of the inner film in this comparative example directly penetrates the inner film. In this comparative example, when the depth of the crack on the surface of the inner film directly penetrates the inner film, the inner wall of the inner film needs an additional leveling process to ensure that the inner wall of the inner film is smooth and flat, otherwise the inner film is prone to material jam.
[0068] Test Example 1 Element detection was performed on the packaging materials in Examples 1-11 and Comparative Examples 1-10, and the contents of cadmium (Cd), lead (Pb), and hexavalent chromium (Cr(VI)) in the packaging materials were determined according to the existing method, with the unit being mg / kg. Cadmium (Cd), lead (Pb), and hexavalent chromium (Cr(VI)) were not detected in the packaging materials in Examples 1-11 and Comparative Examples 1-10. However, for Comparative Example 1, copper powder was precipitated on the surface of the packaging material under a high temperature and high humidity detection environment (temperature greater than 100°C, humidity of about 90%).
[0069] Test Example 2 The packaging inner bags prepared from the packaging materials in Examples 1-11 and Comparative Examples 1-10 were tested for oxygen barrier, water barrier, interlayer peeling and antistatic properties. The test results are shown in Table 1.
[0070] Oxygen barrier performance test method: Use OX2 / 230 oxygen transmission rate test system to measure the oxygen transmission rate of the inner bag of the packaging, the unit is cm³ / m²·24h·0.1MPa; Water barrier performance testing method: Use a water vapor transmission rate tester to measure the water vapor barrier performance of the packaging bag. The testing method of the water vapor transmission rate tester is an existing technology and will not be explained in detail here. The smaller the water vapor transmission rate value, the better the barrier performance of the packaging bag; the water vapor transmission rate is 1g / m 2 .day.Below 1atm indicates good water barrier properties.
[0071] Interlayer peeling: Apply a peeling force of 200N to see if the layers can be peeled apart.
[0072] Antistatic performance: Test the friction voltage (in volts) of the packaging bag, fix the metal plate on the test electrode of the electrostatic voltage tester, and ensure that the metal plate is in good contact with the electrode of the test instrument; perform friction: create friction between the packaging bag and the metal plate at a friction speed of 120 times / min, and record the voltage value displayed by the electrostatic voltage tester after 2 minutes of friction. This value is the maximum friction voltage generated by the antistatic bag during the friction process. The smaller the friction voltage, the better the antistatic performance. When the friction voltage is greater than 100 volts, the electrostatic force generated can adsorb polysilicon.
[0073] Table 1 Packaging bag performance test results Test Example 3 The transverse and longitudinal breaking pressures of the films prepared from the packaging materials in Examples 1-11 and Comparative Examples 1-10 were tested. The test results are shown in Table 2.
[0074] Breaking pressure: A tensile testing machine is used to measure the tensile force (N) when the film is broken in the transverse and longitudinal directions. The detection method of the film's transverse and longitudinal breaking pressure is an existing technology and will not be elaborated on here.
[0075] Table 2 Film tensile properties test Combining the data of Table 1 and Table 2, it can be seen that Example 1 of the present invention is the best ratio. Too much or too little addition of the cross-linking agent will affect the tensile strength, barrier properties and antistatic properties of the packaging material. Therefore, the present invention limits the use ratio of the cross-linking agent and polyvinyl alcohol; the tensile strength (breaking force) of the packaging material of the present invention is up to 180N, which can fully meet the storage and transportation of electronic polysilicon; the antistatic performance of the present invention is good, it will not adsorb polysilicon, and can be used as an inner packaging bag for electronic polysilicon. Combining Examples 1, 8, 9, and 10, it can be seen that the structure of the gap of the present invention has a significant impact on the anti-electrical performance of the packaging material. The greater the width difference between the narrow end and the wide surface of the gap, the better the anti-electrical performance. However, since the overall width of the gap itself is relatively small, the greater the width difference between the narrow end and the wide surface of the gap, the greater the difficulty of processing the gap. Therefore, the present invention preferably selects the optimal width difference.
[0076] In summary, the packaging material prepared by the present invention has good antistatic properties, high barrier properties, strong tensile strength, and no metal content. It will not have any metal precipitation in high temperature, high humidity and other environments, and has good protection for polycrystalline silicon.
[0077] The above description is only a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions and improvements made by any technician familiar with the field within the spirit and principle of the present invention should be included in the scope of protection of the present invention.
Claims
1. A multi-purpose functional inner packaging material for electronic polysilicon, characterized in that: it comprises an inner film and an outer film which are laminated together, the conductivity of the outer film is better than that of the inner film; the inner film is a polyethylene film, the inner film is prepared based on a crack template method, cracks are evenly distributed on the outer surface of the inner film, a conductive material is filled between the inner film and the outer film, the conductive material is evenly distributed between the inner film and the outer film, and the conductive material is filled in the cracks on the surface of the inner film; The conductive material is a conductive adhesive layer obtained by cross-linking polyvinyl alcohol under the action of a self-made cross-linking agent, and the self-made cross-linking agent is 4-(2-aminophenyl)-pyridine-3-oxacyclo-5-thiophene-2-acyl; Preparation method of the homemade cross-linking agent The following steps are involved: A. Under alkaline conditions, hydroquinone and benzaldehyde are subjected to Aldour condensation reaction to obtain dihydroxydiphenylmethane, and then, the dihydroxydiphenylmethane is converted into a benzene derivative by Bergmann cyclization reaction at 200°C; B. Using dimethyl sulfoxide as solvent, the prepared benzene derivative is subjected to condensation and cyclization reaction with 4-chloro-3-nitropyridine and 3-oxacyclo-5-thiophene-2-carboxaldehyde to obtain 4-(2-aminophenyl)-pyridine-3-oxacyclo-5-thiophene-2-acyl.
2. The multi-purpose functional inner packaging material for electronic polycrystalline silicon according to claim 1, Features: The mass ratio of polyvinyl alcohol to the self-made cross-linking agent in the conductive material is 7.2-7.5:
1.
3. The multi-purpose functional inner packaging material for electronic polycrystalline silicon according to claim 2, Features: The mass ratio of polyvinyl alcohol to the homemade cross-linking agent in the conductive material is 7.4:
1.
4. The multi-purpose functional inner packaging material for electronic polycrystalline silicon according to claim 1, Features: The outer film comprises component A and component B, wherein the mass of component B is 1-2% of the mass of component A; The component A comprises the following components: polyvinyl alcohol, furan-based copolyester, solvent, and photosensitive catalyst, wherein the solvent is dimethylformamide, the photosensitive catalyst is benzophenone, the mass ratio of polyvinyl alcohol to furan-based copolyester is 1.5:1, 10 ml of solvent is used for 1 g of the total amount of polyvinyl alcohol and furan-based copolyester, and the mass of the photosensitive catalyst is 1.2-1.4% of the total amount of polyvinyl alcohol and furan-based copolyester; The component B consists of the following components: 100 wt% of nano-layered silicate-modified PVA; The component A is used to prepare the base film of the outer film, and the component B is used to prepare the coating layer of the outer layer of the base film.
5. The multi-purpose functional inner packaging material for electronic polycrystalline silicon according to claim 4, Features: The mass of component B is 1.5% of the mass of component A; The mass of the photosensitive catalyst in the component A is 1.3% of the total amount of polyvinyl alcohol and furan-based copolyester.
6. The multi-purpose functional inner packaging material for electronic polycrystalline silicon according to claim 5, Features: The outer layer membrane is prepared by the following method: a. Prepare a base film with component A: use dimethylformamide as solvent, dissolve polyvinyl alcohol and furan-based copolyester in dimethylformamide, stir evenly, add benzophenone, continue stirring and heat to 40°C, and then irradiate the reactants with ultraviolet light. Under the irradiation of ultraviolet light, benzophenone induces an etherification reaction between polyvinyl alcohol and furan-based copolyester, combines the hydroxyl group in PVA with the hydroxyl group in furan-based copolyester to form an ether bond, and obtains a new copolymer containing an ether bond. The new copolymer is formed and cooled to obtain a base film; b. Coating: A coating machine is used to coat the nano-layered silicate-modified PVA on the outer surface of the base film to obtain an outer film, and the inner surface of the outer film is bonded to the inner film through a conductive material.
7. The multi-purpose functional inner packaging material for electronic polycrystalline silicon according to claim 1, Features: The crack on the surface of the inner film is a trumpet-shaped structure that expands inward and contracts outward, with the narrow end of the crack close to the outer film and the wide side of the crack close to the inner side of the inner film.
8. The multi-purpose functional inner packaging material for electronic polycrystalline silicon according to claim 7, Features: The wide side opening width d1 of the crack is 3-4 times the narrow side opening width d2.
9. A method for preparing a multi-purpose functional inner packaging material for electronic polysilicon according to any one of claims 1 to 8, Features: The following steps are involved: S1. preparing an inner layer film: using molten polyethylene resin to prepare a polyethylene inner layer film having cracks distributed on the surface based on a crack template method; S2. preparing a conductive material; S2.1 Prepare homemade cross-linker: A. Under alkaline conditions, hydroquinone and benzaldehyde are subjected to Aldour condensation reaction to obtain dihydroxydiphenylmethane, and then, the dihydroxydiphenylmethane is converted into a benzene derivative by Bergmann cyclization reaction at 200°C; B. Using dimethyl sulfoxide as solvent, the prepared benzene derivative is subjected to condensation and cyclization reaction with 4-chloro-3-nitropyridine and 3-oxacyclo-5-thiophene-2-carboxaldehyde to obtain 4-(2-aminophenyl)-pyridine-3-oxacyclo-5-thiophene-2-acyl; S2.2 Cross-linking reaction: Under the protection of an inert gas (such as nitrogen), PVA and 4-(2-aminophenyl)-pyridine-3-oxacyclic-5-thiophene-2-acyl are dissolved in a solvent respectively. After dissolution, the PVA solution and the 4-(2-aminophenyl)-pyridine-3-oxacyclic-5-thiophene-2-acyl solution are mixed, and after mixing evenly, they are heated while stirring. After heating to 80° C., the reaction is carried out at a constant temperature. After reacting for 8-10 hours, the reaction is stopped, and the reaction mixture is cooled, filtered, and evaporated to remove the solvent to obtain a conductive material; S3, preparing outer membrane: The outer film comprises component A and component B; The component A comprises the following components: polyvinyl alcohol, furan-based copolyester, solvent, and photosensitive catalyst, wherein the solvent is dimethylformamide and the photosensitive catalyst is benzophenone; The component B consists of the following components: 100 wt% of nano-layered silicate-modified PVA; a. Prepare a base film with component A: use dimethylformamide as solvent, dissolve polyvinyl alcohol and furan-based copolyester in dimethylformamide, stir evenly, add benzophenone, continue stirring and heat to 40°C, and then irradiate the reactants with ultraviolet light. Under the irradiation of ultraviolet light, benzophenone induces an etherification reaction between polyvinyl alcohol and furan-based copolyester, combines the hydroxyl group in PVA with the hydroxyl group in furan-based copolyester to form an ether bond, and obtains a new copolymer containing an ether bond. The new copolymer is formed and cooled to obtain a base film; b. Coating: The nano-layered silicate-modified PVA is coated on the outer surface of the base film by a coating machine to obtain an outer film, and the inner surface of the outer film is bonded to the inner film by a conductive material; S4. Preparation of composite film: The conductive material prepared in step S2 is evenly sprayed on the outer surface of the inner film, the conductive material evenly covers the outer surface of the inner film and fills the cracks on the outer surface of the inner film with the conductive material, a conductive layer is formed after the conductive material is sprayed, and then the outer film is pressed on the conductive layer, the inner surface of the outer film is tightly fitted with the conductive layer, and then after pressing, cooling and forming, a multi-purpose functional inner packaging material for electronic polysilicon is prepared.
10. The method for preparing a multi-purpose functional inner packaging material for electronic polycrystalline silicon according to claim 9, Features: The depth of the cracks on the inner film surface is 3 / 5-2 / 3 of the inner film thickness.
Citation Information
Patent Citations
Cross-linked polymers and medical products derived from nucleophilically activated polyoxazoline
CN104271638A
Loose-structure polyvinyl alcohol (PVA) film and preparation method thereof
CN106674562A
Preparation and use method of benzoxazine type adhesive for polyethylene
CN110862793A
Heterodicyclic compound derivatives
CN1250776A
Production of 3-oxo-alpha-ionone
JP1992041455A
Cited By
Photovoltaic packaging adhesive film for BC battery and preparation method of photovoltaic packaging adhesive film