Composite fireproof and heat-insulating material, preparation method and application
By using a composite fire-resistant and thermal insulation material of modified SiO2 aerogel and glass fiber felt layer in new energy vehicle batteries, the problem of insufficient thermal insulation performance in the prior art is solved, and efficient thermal management and flame retardant are achieved Performance, suitable for preventing thermal runaway between the battery cells.
Patent Information
- Application Number
- CN202411186376.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-28
AI Technical Summary
The existing silica aerogel insulation felt is insufficient in thermal insulation performance in new energy vehicle batteries, especially when the space between the battery cells is limited, it is difficult to effectively prevent thermal runaway.
Using composite fire-resistant heat insulation materials, the modified SiO2 aerogel and glass fiber felt layer are introduced into the aerogel layer, and monomethoxy hydrophobic flame retardant modifier and tris (monomethoxy) The synergistic effect of the hydrophobic flame retardant modifier is modified by the surface derivatization method to form Si-O-Si bonds, which enhances the hydrophobic and flame retardant properties of the material, and is molded by a vacuum plate pressing.
The thermal insulation performance of the material is significantly improved, with the thermal conductivity of 25℃ as low as 0.019W/(m·K), the thermal insulation temperature difference reaches above 160℃, the flame retardant level reaches V-0, and excellent performance.
Smart Images

Figure CN118721936B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of thermal insulation materials for battery cells in new energy vehicle batteries, and in particular to a composite fireproof thermal insulation material, a preparation method and an application thereof. Background Art
[0002] Aerogel is a nanoporous material with comprehensive performance. Its unique structure gives it extremely low thermal conductivity, high porosity and a series of excellent physical and chemical properties. In new energy vehicle batteries, aerogel is mainly used as a thermal insulation material for battery cells to prevent the spread of thermal runaway in battery cells.
[0003] Existing silica aerogel insulation felts are composed of aerogel nanoparticles / fiber composites. The interactions between nanoparticles and between nanoparticles and fibers are very small, which makes the prepared materials always have the problem of easy shedding of aerogel nanoparticles. Usually, an insulating film is used to encapsulate the aerogel to prevent it from falling off. However, existing aerogels still have the problem of insufficient thermal insulation performance, especially when the space between battery cells is limited and the thickness of the aerogel material is thin, its thermal insulation performance cannot meet the requirements of preventing thermal runaway. Summary of the invention
[0004] In order to solve the problem of insufficient thermal insulation performance of existing aerogels, the present invention independently developed a composite fireproof and thermal insulation material, which can achieve the technical goal of preventing thermal runaway between battery cells with limited space.
[0005] A composite fireproof and heat-insulating material, the structure of the material comprising: a heat-insulating structure, a first packaging structure and a second packaging structure, the heat-insulating structure being arranged between the first packaging structure and the second packaging structure;
[0006] The thermal insulation structure consists of an aerogel layer, a first glass fiber felt layer and a second glass fiber felt layer, and the aerogel layer is arranged between the first glass fiber felt layer and the second glass fiber felt layer;
[0007] The aerogel layer (1a) is formed by mixing and pressing the following raw materials in parts by weight: 80-85 parts of modified SiO2 aerogel powder with an average particle size of 0.5-3 μm, 3-10 parts of a stabilizer, and 5-10 parts of a binder;
[0008] The modified SiO2 aerogel is prepared by modifying wet SiO2 gel through the synergistic effect of monomethoxy hydrophobic flame retardant modifier a and tri(monomethoxy) hydrophobic flame retardant modifier b using a surface derivatization method.
[0009] Preferably, the first packaging structure consists of a first bonding layer and a first packaging layer, and the first bonding layer is in direct contact with the first glass fiber felt layer;
[0010] The second packaging structure consists of a second adhesive layer and a second packaging layer, and the second adhesive layer is in direct contact with the second glass fiber felt layer.
[0011] Preferably, the stabilizer is one of methyl cellulose, hydroxypropyl methyl cellulose and ethyl cellulose;
[0012] The binder is one of acrylic emulsion, nitrile latex, styrene-butadiene latex and white latex;
[0013] The first glass fiber felt layer and the second glass fiber felt layer are glass fiber surface felts;
[0014] The first encapsulation layer and the second encapsulation layer are one of PE film, PP film, PET film and PI film;
[0015] The first bonding layer and the second bonding layer are epoxy resin films.
[0016] Preferably, the synthesis method of the monomethoxy hydrophobic flame retardant modifier a is:
[0017] Potassium carbonate and potassium iodide are used to catalyze the substitution reaction between the amino group of n-pentylamine and the chlorine functional group of chloro(dimethyl)methoxysilane to obtain a monomethoxy secondary amine monomer;
[0018] A monomethoxy hydrophobic flame retardant modifier a is obtained by a Kabachnik-Fields reaction of a monomethoxy secondary amine monomer, polyformaldehyde and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and the molar ratio of the monomethoxy secondary amine monomer, polyformaldehyde and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to be reacted is controlled to be 1:(1-1.08):1.
[0019] Preferably, the synthesis method of the tri(monomethoxy) hydrophobic flame retardant modifier b is: a monomethoxy secondary amine monomer, 2,4,6-tri(4-formylphenyl)-1,3,5-triazine and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide undergo a Kabachnik-Fields reaction, and the molar ratio of the monomethoxy secondary amine monomer, 2,4,6-tri(4-formylphenyl)-1,3,5-triazine and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to be reacted is controlled to be (3.05-3.2):1:(3.05-3.2), thereby synthesizing the tri(monomethoxy) hydrophobic flame retardant modifier b.
[0020] Preferably, the mass ratio of the monomethoxy hydrophobic flame retardant modifier a to the tri(monomethoxy) hydrophobic flame retardant modifier b is (7-9):(1-3).
[0021] A method for preparing a composite fireproof and heat-insulating material comprises the following steps:
[0022] Laying melamine foam on the bottom of the mold cavity of a vacuum flat-plate rapid pressing machine, laying a first packaging layer of a first packaging structure on the melamine foam, and laying a first adhesive layer on the first packaging layer;
[0023] Laying a first fiberglass felt layer on the first bonding layer;
[0024] The raw materials of the aerogel layer are mixed and stirred evenly and then laid on the first glass fiber felt layer, and the thickness of the aerogel layer is set according to the compression ratio;
[0025] Laying a second glass fiber felt layer on the aerogel layer, laying a second adhesive layer of a second packaging structure on the second glass fiber felt layer, and laying a second packaging layer on the second adhesive layer;
[0026] The composite fireproof and heat-insulating material is formed by flat-plate pressing for 5-20s under the conditions of vacuum degree 10-90kPa, pressure 1-5MPa and temperature 105-130°C to obtain a composite fireproof and heat-insulating material.
[0027] The composite fireproof and heat-insulating material is installed between cells with limited space in new energy vehicle batteries to prevent thermal runaway.
[0028] Compared with the prior art, the present invention has the following beneficial technical effects:
[0029] The invention independently synthesizes a monomethoxy hydrophobic flame retardant modifier a and a tri(monomethoxy) hydrophobic flame retardant modifier b by molecular structure design and Kabachnik-Fields reaction, and performs modification treatment on wet SiO2 gel by synergistic effect of the monomethoxy hydrophobic flame retardant modifier a and the tri(monomethoxy) hydrophobic flame retardant modifier b, and the specific process is as follows: using a surface derivatization method, hydrolyzing the hydrolyzed functional group of the monomethoxy hydrophobic flame retardant modifier a to obtain a silanol functional group, the silanol functional group condenses with the silanol functional group on the surface of the wet gel to generate a Si-O-Si bond, and simultaneously hydrolyzing the hydrolyzed functional group of the tri(monomethoxy) hydrophobic flame retardant modifier b to obtain a silanol functional group, the silanol functional group condenses with the silanol functional group on the surface of the wet gel to generate a Si-O-Si bond, thereby obtaining a modified SiO2 aerogel;
[0030] The modified SiO2 aerogel powder is used as the raw material of the aerogel layer in the thermal insulation structure, which overcomes the shortcomings of ordinary aerogel powder that it is very easy to absorb moisture and cause structural collapse, and the thermal insulation performance is unstable. A composite fireproof thermal insulation material is prepared based on this. Experimental results show that: the thermal conductivity of the composite fireproof thermal insulation material at 25°C is as low as 0.019W / (m·K), the insulation temperature difference can reach more than 160°C, and the flame retardant grade reaches V-0. It is a new composite fireproof thermal insulation material with excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a schematic diagram of the product structure of the composite fireproof and heat-insulating material;
[0032] Among them, 1-insulating structure, 1a-aerogel layer, 1b-first glass fiber felt layer, 1c-second glass fiber felt layer, 2-first packaging structure, 2a-first bonding layer, 2b-first packaging layer, 3-second packaging structure, 3a-second bonding layer, 3b-second packaging layer. DETAILED DESCRIPTION Embodiment 1:
[0033] A composite fireproof and heat-insulating material, such as Figure 1 As shown, the product structure includes: a heat insulation structure 1, a first packaging structure 2 and a second packaging structure 3, wherein the heat insulation structure 1 is arranged between the first packaging structure 2 and the second packaging structure 3;
[0034] The heat insulation structure 1 is composed of an aerogel layer 1a, a first glass fiber felt layer 1b and a second glass fiber felt layer 1c, and the aerogel layer 1a is arranged between the first glass fiber felt layer 1b and the second glass fiber felt layer 1c;
[0035] The thickness of the first glass fiber felt layer 1b and the second glass fiber felt layer 1c is set to 200 μm;
[0036] The glass fiber felt is a glass fiber surface felt purchased from Dezhou Hongtai Geotechnical Materials Co., Ltd.;
[0037] The first packaging structure 2 is composed of a first bonding layer 2a and a first packaging layer 2b, and the first bonding layer 2a is in direct contact with the first glass fiber felt layer 1b;
[0038] The second encapsulation structure 3 is composed of a second adhesive layer 3a and a second encapsulation layer 3b, and the second adhesive layer 3a is in direct contact with the second glass fiber felt layer 1c;
[0039] The thickness of the first encapsulation layer 2b and the second encapsulation layer 3b is set to 40 μm. The first encapsulation layer 2b and the second encapsulation layer 3b can be made of one of PE film, PP film, PET film and PI film. In this embodiment, PET film is selected and purchased from Shanghai Jiri Electronics Co., Ltd.;
[0040] The thickness of the first adhesive layer 2a and the second adhesive layer 3a is set to 10 μm, and the first adhesive layer 2a and the second adhesive layer 3a are epoxy resin films purchased from Huizhou Hongtian Electronic Materials Co., Ltd.;
[0041] The thickness of the aerogel layer 1a is set to 1.2 mm, and the aerogel layer 1a is formed by mixing and pressing the following raw materials in parts by weight: 80 parts of modified SiO2 aerogel powder with an average particle size of 2 μm, 5 parts of stabilizer, and 7 parts of binder; wherein the preparation method of the modified SiO2 aerogel powder is shown in the following experimental example;
[0042] The stabilizer can be selected from methylcellulose, hydroxypropyl methylcellulose, and ethyl cellulose. The stabilizer used in this embodiment is hydroxypropyl methylcellulose purchased from Shanghai MacLean Biochemical Technology Co., Ltd.
[0043] The binder can be selected from one of acrylic emulsion, nitrile latex, styrene butadiene latex, and white latex. In this embodiment, acrylic emulsion is selected. The product number of acrylic emulsion is B332HT, which is purchased from Shenzhen Wenuohua Chemical Materials Co., Ltd. Embodiment 2:
[0044] The method for preparing the composite fireproof and heat-insulating material in Example 1 comprises the following steps:
[0045] Step S1: set the density to 0.09 g / cm 3 The melamine foam is laid on the bottom of the mold cavity of the vacuum flat-plate rapid pressing machine, the first packaging layer 2b is laid on the melamine foam, and the first bonding layer 2a is laid on the first packaging layer 2b;
[0046] Step S2, laying a first glass fiber felt layer 1b on the first adhesive layer 2a;
[0047] The raw materials of the aerogel layer 1a are mixed and stirred evenly and then laid on the first glass fiber felt layer 1b. According to the compression ratio of 40%, the thickness of the aerogel layer 1a is set to 2 mm;
[0048] Laying a second glass fiber felt layer 1c on the aerogel layer 1a, laying a second adhesive layer 3a on the second glass fiber felt layer 1c, and laying a second packaging layer 3b on the second adhesive layer 3a;
[0049] Step S3, under the conditions of vacuum degree 50 kPa, pressure 3 MPa, and temperature 120° C., pressing on a flat plate in a vacuum flat plate rapid pressing machine for 10 seconds to obtain a composite fireproof and heat-insulating material. Embodiment 3:
[0050] The performance test of the composite fireproof and heat-insulating material prepared in Example 2 was carried out, and the test method was as follows:
[0051] (1) Thermal conductivity test at 25°C: According to GB / T10295-2008 standard, the sample size is 200mm×200mm×6mm, the hot surface temperature is 35°C, the cold surface temperature is 15°C, and the test pressure is 80N;
[0052] (2) Thermal insulation temperature difference test: Set the temperature of the heating table of the back temperature tester to 470°C, place the sample on the heating table, set the pressure to 0.7 MPa, turn off the heating switch and stop pressurizing after heating for 2 minutes, keep the sample in a compressed state and cool it naturally, record the temperature difference between the hot and cold surfaces when the cold surface is at the peak temperature, and repeat the test ten times;
[0053] (3) Flame retardant test: According to UL94 V-0 standard, the sample size is 125 mm × 13 mm. Clamp the upper end of the sample, perpendicular to the ground, move the adjusted flame to the center of the lower end of the sample, and continuously apply the flame for (10 ± 0.5) s. The equipment automatically counts the time. After 10 s, the flame is removed and the first afterflame t1 is counted at the same time. After the afterflame completely disappears, quickly apply the second flame to the sample. After 10 s, the flame is removed and the second afterflame t2 and the second afterburn t3 are counted at the same time. Five sets of parallel samples are made.
[0054] The above experimental results are shown in Table 1 below;
[0055] Table 1 Performance test results of composite fireproof and heat-insulating materials
[0056] Product No. Performance Index Composite fireproof and heat-insulating materials Comparative Example Thermal conductivity at 25℃(W / (m·K)) 0.019 0.024 Insulation temperature difference (℃) ≥160 ≥150 Flame retardant grade V-0 V-1
[0057] Note: The difference between the comparative example and the composite fireproof and heat-insulating material is that SiO2 aerogel powder is used instead of modified SiO2 aerogel powder. The preparation method of SiO2 aerogel powder is shown in the following experimental example.
[0058] The experimental results show that the composite fireproof thermal insulation material prepared by using modified SiO2 aerogel powder as the raw material of the aerogel layer 1a in the thermal insulation structure 1 has achieved beneficial technical effects of significantly improving the flame retardant, thermal insulation and thermal conductivity properties.
[0059] Experimental example:
[0060] Due to the presence of hydrophilic hydroxyl functional groups on the surface of SiO2 aerogel, SiO2 aerogel is very easy to absorb moisture and cause structural collapse, which in turn affects the thermal insulation effect and service life. Therefore, the present invention uses molecular structure design and Kabachnik-Fields reaction to synthesize two new modifiers with both flame retardant and hydrophobic functions, which are used to improve the hydrophobic and flame retardant properties of SiO2 aerogel.
[0061] Synthesis of monomethoxy secondary amine monomer: Potassium carbonate and potassium iodide are used to synergistically catalyze the substitution reaction between the amino functional group of n-pentylamine and the chloro functional group of chloro(dimethyl)methoxysilane to obtain a monomethoxy secondary amine monomer. The specific synthesis steps are: 7.1 mL of chloro(dimethyl)methoxysilane, 6.95 mL of n-pentylamine, 20.7 g of potassium carbonate, 0.83 g of potassium iodide and 80 mL of anhydrous toluene are added to a dry round-bottom flask, nitrogen is blown and oxygen is discharged three times under ice bath conditions, nitrogen protection is used, and the reaction is carried out at 80°C for 24 hours. After the reaction is completed, the monomer is washed with deionized water, filtered, spin-dried, and dried to obtain a monomethoxy secondary amine monomer, whose chemical structure is:
[0062] ;
[0063] The characterization results of the nuclear magnetic resonance hydrogen spectrum of the monomethoxy secondary amine monomer are as follows:
[0064] 1 H NMR (400MHz, DMSO-d6, δ, ppm): 0.07 (s, 6H), 0.88-0.92 (t, 3H), 1.32-1.38 (m, 4H), 1.5 2-1.59(m, 2H), 2.01-2.03(d, 2H), 2.57-2.62(m, 2H), 3.07-3.13(m, 1H), 3.45(s, 3H);
[0065] Synthesis of monomethoxy hydrophobic flame retardant modifier a: Monomethoxy hydrophobic flame retardant modifier a is synthesized by Kabachnik-Fields reaction of monomethoxy secondary amine monomer, polyformaldehyde and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO). The specific synthesis steps are as follows: 4.54 g of monomethoxy secondary amine monomer and 30 mL of chloroform are added to a three-necked flask equipped with a stirrer and a reflux condenser, nitrogen is passed and stirred for 10 minutes, 0.792 g of polyformaldehyde and 5.19 g of DOPO are added, refluxed at 60° C. for 24 hours, cooled to room temperature, poured into ice methanol, the precipitated product is washed with chloroform, and the product is vacuum dried at 60° C. for 24 hours to obtain monomethoxy hydrophobic flame retardant modifier a, whose chemical structure is:
[0066] ;
[0067] The characterization results of the nuclear magnetic resonance hydrogen spectrum of the monomethoxy hydrophobic flame retardant modifier a are as follows:
[0068] 1H NMR (400MHz, DMSO-d6, δ, ppm): 0.1 (s, 6H), 0.87-0.91 (t, 3H), 1.30-1.36 (m, 4H), 1.47-1.53 (m, 2H), 1.82 (s, 2H), 2.52-2.55 (t, 2H), 3.41 (s, 3H), 3.53-3.56 (d, 2H), 7.32-7.91 (m, 8H);
[0069] Synthesis of tri(monomethoxy) hydrophobic flame retardant modifier b: tri(monomethoxy) hydrophobic flame retardant modifier b is synthesized by Kabachnik-Fields reaction of monomethoxy secondary amine monomer, 2,4,6-tri(4-formylphenyl)-1,3,5-triazine and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO). The difference between its synthesis experimental steps and monomethoxy hydrophobic flame retardant modifier a is that 3.41 g of 2,4,6-tri(4-formylphenyl)-1,3,5-triazine is used to replace 0.792 g of polyformaldehyde;
[0070] The chemical structure of tri(monomethoxy) hydrophobic flame retardant modifier b is:
[0071] ;
[0072] The characterization results of the nuclear magnetic resonance hydrogen spectrum of tri(monomethoxy) hydrophobic flame retardant modifier b are as follows:
[0073] 1 H NMR (400MHz, DMSO-d6, δ, ppm): 0.11 (s, 18H), 0.87-0.91 (t, 9H), 1.24-1.37 (m, 12H), 1.43-1.58 (m, 6H), 1. 81-1.94(m, 6H), 2.47-2.66(m, 6H), 3.40(s, 9H), 4.84-4.87(d, 3H), 7.33-7.87(m, 30H), 8.20-8.22(d, 6H).
[0074] Preparation of modified SiO2 aerogel powder: 22.2 mL of tetraethyl orthosilicate was added to a mixed solution consisting of 9.0 mL of purified water and 46.7 mL of anhydrous ethanol, the pH value of the solution was adjusted to 4 with dilute hydrochloric acid, stirred at room temperature for 24 h, and the pH value of the solution was adjusted to 7 with aqueous ammonia, and the gel was allowed to stand to obtain gel, anhydrous ethanol was added to immerse the gel, aged at 50 ° C for 24 h, and then the gel was immersed in a 90% ethanol solution for further aging for 24 h to obtain a wet gel, and then a volume ratio of 5:5:0.8:0 was added. A mixed solution of n-hexane-toluene-monomethoxy hydrophobic flame retardant modifier a-tri(monomethoxy) hydrophobic flame retardant modifier b in 2 undergoes condensation reaction with the silanol functional groups on the surface of the wet gel at 45°C for 24 hours, and is then soaked in n-hexane for 24 hours. The mixture is dried at 60°C for 4 hours, 80°C for 4 hours, and 120°C for 2 hours under normal pressure to obtain a modified SiO2 aerogel. The modified SiO2 aerogel is ground and sieved to obtain a modified SiO2 aerogel powder with an average particle size of 2 μm.
Claims
1. A composite fireproof and heat-insulating material, characterized in that: The material structure comprises: a heat insulation structure (1), a first packaging structure (2) and a second packaging structure (3), wherein the heat insulation structure (1) is arranged between the first packaging structure (2) and the second packaging structure (3); The thermal insulation structure (1) is composed of an aerogel layer (1a), a first glass fiber felt layer (1b) and a second glass fiber felt layer (1c), wherein the aerogel layer (1a) is arranged between the first glass fiber felt layer (1b) and the second glass fiber felt layer (1c); The aerogel layer (1a) is formed by mixing and pressing the following raw materials in parts by weight: 80-85 parts of modified SiO2 aerogel powder with an average particle size of 0.5-3 μm, 3-10 parts of a stabilizer, and 5-10 parts of a binder; The modified SiO2 aerogel is prepared by modifying the wet SiO2 gel through the synergistic effect of a monomethoxy hydrophobic flame retardant modifier a and a tri(monomethoxy) hydrophobic flame retardant modifier b using a surface derivatization method. The chemical structural formula of the monomethoxy hydrophobic flame retardant modifier a is: ; The synthesis method of the monomethoxy hydrophobic flame retardant modifier a is: Potassium carbonate and potassium iodide are used to synergistically catalyze the substitution reaction between the amino group of n-pentylamine and the chlorine functional group of chloro(dimethyl)methoxysilane to obtain a monomethoxy secondary amine monomer; A monomethoxy hydrophobic flame retardant modifier a is obtained by reacting a monomethoxy secondary amine monomer, polyformaldehyde and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide in a Kabachnik-Fields reaction, and controlling the molar ratio of the monomethoxy secondary amine monomer, polyformaldehyde and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to be 1:(1-1.08):
1. The chemical structural formula of the tri(monomethoxy) hydrophobic flame retardant modifier b is: ; The synthesis method of the tri(monomethoxy) hydrophobic flame retardant modifier b is as follows: a monomethoxy secondary amine monomer, 2,4,6-tris(4-formylphenyl)-1,3,5-triazine and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide undergo a Kabachnik-Fields reaction, and the molar ratio of the monomethoxy secondary amine monomer, 2,4,6-tris(4-formylphenyl)-1,3,5-triazine and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to be reacted is controlled to be (3.05-3.2):1:(3.05-3.2), thereby synthesizing the tri(monomethoxy) hydrophobic flame retardant modifier b.
2. A composite fireproof and heat-insulating material according to claim 1, characterized in that: The first packaging structure (2) is composed of a first adhesive layer (2a) and a first packaging layer (2b), and the first adhesive layer (2a) is in direct contact with the first glass fiber felt layer (1b); The second encapsulation structure (3) is composed of a second adhesive layer (3a) and a second encapsulation layer (3b), and the second adhesive layer (3a) is in direct contact with the second glass fiber felt layer (1c).
3. A composite fireproof and heat-insulating material according to claim 2, characterized in that: The stabilizer is one of methyl cellulose, hydroxypropyl methyl cellulose and ethyl cellulose; The binder is one of acrylic emulsion, nitrile latex, styrene-butadiene latex and white latex; The first glass fiber felt layer (1b) and the second glass fiber felt layer (1c) are glass fiber surface felts; The first encapsulation layer (2b) and the second encapsulation layer (3b) are one of a PE film, a PP film, a PET film, and a PI film; The first adhesive layer (2a) and the second adhesive layer (3a) are epoxy resin films.
4. A composite fireproof and heat-insulating material according to claim 1, characterized in that: The mass ratio of the monomethoxy hydrophobic flame retardant modifier a to the tri(monomethoxy) hydrophobic flame retardant modifier b is (7-9):(1-3).
5. The method for preparing a composite fireproof and heat-insulating material according to claim 2, characterized in that: The following steps are involved: Laying melamine foam on the bottom of the mold cavity of a vacuum flat-plate rapid laminating machine, laying a first encapsulation layer (2b) of a first encapsulation structure (2) on the melamine foam, and laying a first adhesive layer (2a) on the first encapsulation layer (2b); Laying a first glass fiber felt layer (1b) on the first adhesive layer (2a); The raw materials of the aerogel layer (1a) are mixed and stirred evenly, and then laid on the first glass fiber felt layer (1b), and the thickness of the aerogel layer (1a) is set according to the compression ratio; Laying a second glass fiber felt layer (1c) on the aerogel layer (1a), laying a second adhesive layer (3a) of a second packaging structure (3) on the second glass fiber felt layer (1c), and laying a second packaging layer (3b) on the second adhesive layer (3a); The composite fireproof and heat-insulating material is formed by flat-plate pressing for 5-20s under the conditions of vacuum degree 10-90kPa, pressure 1-5MPa and temperature 105-130°C to obtain a composite fireproof and heat-insulating material.
6. The use of a composite fireproof and heat-insulating material according to any one of claims 1 to 4, characterized in that: The composite fireproof and heat-insulating material is installed between cells with limited space in new energy vehicle batteries to prevent thermal runaway.