Packaging comprising a sealed contact region with a nonwoven having an adhesive surface with an
By pre-bonding the embossed pattern on the fiber nonwoven sheet and combining it with the polymer connection layer to form a sealed contact area, the problem of cracking of the fiber nonwoven sheet when peeled off after sterilization is solved and clean peeling is achieved. and high sealing properties, suitable for sterile packaging.
Patent Information
- Application Number
- CN202410985247.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2016-10-11
- Filing Date
- 2017-09-13
- Publication Date
- 2024-10-01
AI Technical Summary
Existing fibrous nonwoven sheets easily cause surface cracks when peeled off after sterilization, which may contaminate enclosed environments, especially in health-related environments, which is challenging to prevent contamination.
Constructed from a breathable fibrous nonwoven sheet with a pre-bonded embossed embossing pattern and combined with a polymeric tie layer to create a sealed contact area to improve sealing and peel performance and reduce fiber tearing.
Achieving excellent peeling performance in a sterile environment, significantly reducing fiber tearing, providing clean peeling capabilities, and improving seal strength and durability, avoiding the risk of contamination.
Smart Images

Figure CN118723325A_ABST
Abstract
Description
[0001] This application is a divisional application of an invention patent application, the application date of the parent case is September 13, 2017, the application number is 201780063000.8 (PCT / US2017 / 051323), and the invention name is "Packaging including a sealed contact area with a non-woven fabric having an adhesive surface with an embossed pattern". Background Art
[0002] FIELD OF THE INVENTION The present invention relates to improved packaging for providing a closed internal environment capable of sterilization, and air-permeable fibrous nonwoven sheet structures suitable for use therein.
[0003] Description of the Related Art. U.S. Patent No. 6,034,008 to Lim et al. discloses a sheet material suitable for use in filtration and sterile packaging having a thickness at least equivalent to that which has been conventionally used for such applications. Spunbond olefin nonwoven sheet materials have the strength, weight, and barrier properties of those of conventional olefin nonwoven sheet materials, but also have significantly improved air and liquid permeability.
[0004] Specifically, Lim et al. disclose a full-surface bonded "hard structure" product having the feel of glossy paper (commonly used in a variety of applications, including aseptic packaging); and a point-bonded and softened "soft structure" product for apparel applications with a more fabric-like feel.
[0005] As disclosed by Lim et al., it is believed that the full surface bonding of the "hard structure" flash spun sheet products causes the high surface area plexifilamentary fibers of the sheet to shrink, which in turn causes the pores between the fibers to open. As a result, the "hard structure" sheet products generally have higher moisture vapor transmission rates and higher hydrostraic head values than the "soft structure" sheet products. It has been found that such more permeable materials have great utility in aseptic packaging materials, where the increased permeability allows the material to perform its function in a more effective manner.
[0006] Fibrous nonwoven sheets are useful in sterilizable packages because they allow manufacturers to first package items and then sterilize the items in the package using gases such as steam, ethylene oxide, or some combination thereof. Sterilizing gases can penetrate the fibrous nonwoven sheets of the package to sterilize the enclosed interior of the package. Suitable fibrous nonwoven sheets also provide shielding against contaminants to prevent the sterilized packaged items from being contaminated before opening the package.
[0007] It is not uncommon for sterilized packages to be opened in a sterilized environment, and a desirable feature of a fibrous nonwoven sheet is that it can be peeled from the package without excessive tearing of the nonwoven sheet surface when the sheet is removed. Some believe that surface disruption (fiber tearing) of the nonwoven sheet during peeling may contaminate the sterilized environment in which the package is opened.
[0008] Since most sterilized packaging is used in health-related settings (like operating rooms), any improvement that helps prevent or reduce any possible contamination is desirable. In packaging, any improvement in the peeling properties of fibrous nonwoven structures, in particular, is highly desirable. Summary of the invention
[0009] The present invention relates to a packaging material for providing a closed internal environment capable of being sterilized, the packaging material comprising a breathable fibrous nonwoven sheet structure, a polymer connecting layer, and a packaging material substrate; the nonwoven sheet structure has a first surface and a second surface; the closed internal environment is formed by sealing the contact area between the first surface of the nonwoven sheet structure and the packaging material structure, the sealed contact area being formed by the polymer connecting layer; wherein the first surface of the nonwoven sheet structure is pre-bonded with an embossed pattern at least in the sealed contact area.
[0010] The present invention also relates to a fibrous nonwoven sheet structure suitable for use in aseptic packaging, the sheet structure being breathable and having a first surface and a second surface; the first surface being bonded with an embossed pattern and the second surface being capable of receiving printing; the sheet structure having a particle barrier penetration of less than 10%, a Gurley Hill porosity of 40 seconds or less, and a porosity of 3500 g / m 2 / day or greater moisture vapor transmission rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 and Figure 2 Here are some illustrations of embossing patterns.
[0012] Figure 3 and Figure 4 are illustrations of some packaging substrates showing the sealing areas.
[0013] Figure 5 is a diagram illustrating the location of four samples used to determine the seal strength of a package. DETAILED DESCRIPTION
[0014] The present invention relates to a packaging material for providing a closed internal environment capable of sterilization and a breathable fibrous nonwoven sheet structure useful in such a structure, wherein the nonwoven sheet structure has at least one surface pre-bonded with an embossed embossed pattern and has a particle barrier penetration rate of less than 10%, a Glihill porosity of 40 seconds or less, and a 3500 g / m 2 / day or greater moisture vapor transmission rate.
[0015] Surprisingly, it has been discovered that nonwoven sheet structures having bonded surfaces with embossed patterns can be used in sealed packages having interior environments capable of being sterilized. Surprisingly, (1) the embossed nonwoven surface can provide a good seal for the package structure, and also (2) the resulting package has an excellent level of peel performance (when the package is opened), in many cases better than smooth surface bonded sheets.
[0016] It is desirable that any package utilized and opened in a sterile environment have a "clean peel" or provide "sterile peel / introduction", a term used in the medical industry, referring to the requirement that the package can be opened and the contents introduced into a sterile environment without risk of contamination. As used herein, this excellent opening performance is determined by using a "fiber tear" criterion. Surprisingly, the use of a nonwoven sheet structure having at least one surface pre-bonded with an embossed pattern (in contact with the polymer tie layer) can provide a package having a clean peel and having very low fiber tear, or in fact no fiber tear.
[0017] Even more notable is that this excellent level of release performance is achieved without any additional coating on the fibrous nonwoven sheet structure. The use of nonwoven coatings can provide improved release, but the simple use of such coatings can create other loose particles that make aseptic introduction risky.
[0018] A packaging material for providing a closed interior environment capable of sterilization includes a breathable fibrous nonwoven sheet structure, a polymeric tie layer, and a packaging substrate.
[0019] The packaging substrate can be any material forming a flexible or semi-rigid packaging, for example, in the packaging of a packet (sachet), bag, sheath or blister pack. The packaging comprising a packaging substrate is generally used to protect packaged goods, and in the case of aseptic packaging, helps to maintain the packaged goods in an uncontaminated state until ready to use. In a practical application, the article to be packaged is placed in the packaging substrate, and then a polymer tie layer and an air permeable fiber nonwoven sheet structure are used to seal it to form a closed environment. Then (if necessary) suitable sterilizing gas can be used to sterilize the packaging with closed articles. In certain embodiments, the packaging substrate comprises polyamide (especially nylon), polypropylene, polyester (especially polyethylene terephthalate) and any combination thereof.
[0020] The packaging includes a polymer tie layer for sealing the contact area between the nonwoven sheet structure and the packaging structure. The polymer tie layer is preferably any flexible or semi-rigid film that is compatible with both the packaging substrate and the nonwoven sheet structure and properly seals the nonwoven sheet structure to the packaging substrate. Compatible with means that the polymer tie layer does not react adversely with the nonwoven sheet or the packaging substrate and has a suitable shelf life to keep the packaging sealed until its intended use. In some preferred embodiments, the polymer tie layer is integral with the packaging substrate. Figure 3 and Figure 4 As shown in FIG. 1 , sealing areas 15 and 17 illustrate one embodiment of an area where the polymeric tie layer forms a sealed contact area where the wrapper substrate and the fibrous nonwoven sheet structure will contact.
[0021] The polymer tie layer is preferably in the form of a film.The composition of the polymer tie layer may comprise compositions including such things as, for example, polyethylene (including low density polyethylene), ethylene vinyl acetate, and any combination thereof.
[0022] In some preferred embodiments, the polymer tie layer and the packaging substrate are integrated. In certain embodiments, they are combined in the same film. In this case, as used herein, the packaging substrate is defined as "structural material", and this structural material is integrated in the film with the polymer used as the polymer tie layer. For example, some useful structural materials include polyamide (especially nylon), polypropylene, polyester (especially polyethylene terephthalate) and any combination thereof. The structural material / polymer tie layer combination of especially desired that can be used when the packaging substrate and the polymer tie layer are integrated includes polyamide / polyethylene, polyester / polyethylene, polypropylene / polyethylene, polypropylene / ethylene-vinyl acetate, polyamide-polypropylene / polyethylene etc.
[0023] The fiber nonwoven sheet structure is breathable, meaning that sterilizing gases such as ethylene oxide and / or steam can pass through the sheet without using excessive pressure. In particular, the fiber nonwoven sheet structure has a Gurley porosity (also referred to as Gurley Hill porosity) of 40 seconds or less. This characteristic is a measure of the time it takes for a certain volume of gas to pass through a material region where a certain pressure gradient exists; therefore, a lower number means that the material is more breathable, and a higher number means that the material is less permeable. In some embodiments, the fiber nonwoven sheet structure has a Gurley porosity of 10 seconds or less. In some embodiments, the fiber nonwoven sheet structure has a Gurley porosity of 5 seconds or less, and in some most preferred embodiments, the fiber nonwoven sheet structure has a Gurley porosity of 3 seconds or less.
[0024] Another indicator of permeability is the measurement of moisture vapor transmission, where higher values are more permeable. This is particularly important when steam is used as part of a sterilization process. The fibrous nonwoven sheet structure has a moisture vapor transmission of at least 3500 g / m 2 / day or greater moisture vapor transmission rate. In some preferred embodiments, the fiber nonwoven sheet structure has a moisture vapor transmission rate of at least 7500 g / m 2 / day or greater moisture vapor transmission rate. In some other embodiments, the fibrous nonwoven sheet structure has a moisture vapor transmission rate of at least 9000 g / m 2 / day or greater moisture vapor transmission rate. Preferably, the fibrous nonwoven sheet structure is uncoated, giving a more permeable sheet structure. The use of a coating to improve adhesion tends to seal the surface of the nonwoven sheet structure, reducing the rate at which sterilizing gas can pass through the structure.
[0025] The fibrous nonwoven sheet structure has a first surface and a second surface, wherein the first surface is bonded with an embossed pattern. As used herein, the phrase "bonded with an embossed pattern" means that the surface has at least two characteristics, the first of which is that the fibrous material on the surface has been "bonded", which means that the fibrous material has been substantially consolidated and stabilized by heat and pressure provided to the sheet from a heating source (such as a roller); in addition, the surface has an embossed pattern that gives the surface a visual texture. As used herein, the use of the term "pre-bonded" means that the fibrous nonwoven sheet structure is embossed before it is incorporated into any packaging.
[0026] In one embodiment, the embossed pattern in the sheet is provided by calendering the nonwoven sheet in the roll gap between a heated metal roll and an elastomeric support roll, and the metal roll is provided with a pattern of a raised area or boss extending radially outward from the surface of the roll. In some preferred embodiments, the raised area or boss extend 0.008 to 0.020 inch (0.20 to 0.50mm) from the surface of the remainder of the roll. In some other embodiments, the raised area or boss can have a width of 0.005 to 0.025 inch (0.12 to 0.64mm). In some preferred embodiments, the width of the raised area or boss can be 0.005 to 0.015 inch (0.12 to 0.38mm).
[0027] When a fibrous nonwoven web is pressed in the nip between a heated metal roll having raised areas or bosses and an elastomeric backing roll, the nonwoven web is provided with an embossed pattern having a depth substantially equivalent to the dimensions of the bosses. Figure 1 and Figure 2 Illustrations of two potentially useful and desirable embossing patterns are provided, wherein Figure 1 It is called the linen pattern, and Figure 2 It's called a dog-bone pattern.
[0028] A preferred method of embossing a nonwoven sheet is to thermally bond the sheet on a modified machine similar to that of Janis U.S. Pat. No. 5,972,147. Figure 2 In the method described in. In the preheating section of the improved machine, each of the sides of the nonwoven being bonded is contacted with a plurality of preheating rollers. In some preferred embodiments of the embossed nonwoven sheet described herein, the Janis machine is improved so that there are four heating rollers in this section, and the rollers are operated at a temperature sufficient to provide sufficient surface bonding of the sheet. The temperature will depend on the melting point of the bonded material. After the preheating roller, the sheet is preferably only passed through one of the multiple embossing machine sections shown, so that the embossing machine pattern is preferably only applied to one surface of the sheet. There is an embossing machine roller that can be pressed onto the support roller to form a roller gap on each embossing machine section. The pressure between the embossing machine and the support roller is represented by pounds / line inch (pli). The support roller is typically covered with an elastomeric cover and is cooled internally by a recirculating cooling medium. Subsequently, the nonwoven sheet is transferred to a plurality of cooling rollers where the temperature of the sheet material is reduced, and then wound into a roll.
[0029] The use of multiple preheated rollers operating at high temperatures not only helps to bond the first surface of the nonwoven to be embossed, but also provides an opposite second surface that is also bonded. The second surface is preferably capable of receiving printing. In addition, preferably, for best printing performance, the second surface has a smooth surface without any embossing. Many packaging items require very specific bar codes and other delicate and small markings, which require a very uniform and flat surface without the texture provided by embossing.
[0030] Alternatively, the sheet surface may first be bonded, wound on a roll, and then subsequently unwound and embossed on one side to provide a first surface bonded with an embossed pattern. Other embossing methods are also possible, as long as they provide a fiber nonwoven sheet having at least a first surface bonded with an embossed pattern. Preferably, the method provides a second surface capable of receiving printing. Preferably, the second surface is uniform and does not have any embossed pattern.
[0031] In some embodiments, the fiber nonwoven sheet structure has good shielding against pollutants and has sufficient durability to withstand general handling without damaging or contaminating the contents of the package. Therefore, the fiber nonwoven sheet structure with an embossed embossed pattern preferably has a particle shielding penetration rate of less than 10% as determined with a TSI 8130 device. It is believed that this particle shielding test is useful in determining the degree of shielding provided by the sheet to pollutants, and pollutants may include those that may be bacterial in nature. In addition, the fiber nonwoven sheet structure with an embossed embossed pattern preferably has a Mullen burst strength greater than 500 kPa and a measured Elmendorf tearing performance greater than 2 N / m.
[0032] The fibrous nonwoven sheet structure includes a nonwoven fabric that can provide a stable surface with an embossed pattern for contact with a polymer tie layer on the wrapper. Such nonwoven sheet structures can include flash spun nonwoven sheet structures, spunbond
[0033] Nonwovens, meltblown sheets, electroblown sheets, and any combination thereof. Fiber means that the material in the nonwoven sheet has some fiber properties. This fiber property can be provided by things such as staple fibers, continuous or semi-continuous fibers, and / or plexifilamentary fiber structures. The fiber material can contain a single material or multiple materials, as a combination of different fibers or as a combination of similar fibers each containing different materials. The term "nonwoven" means a planar sheet structure, including at least one randomly distributed web of fiber material, as opposed to a woven or knitted fabric, which is made of interlaced yarns or interlocking yarn loops. In some preferred embodiments, the fiber material in the nonwoven sheet is a synthetic polymer; in some embodiments, the synthetic polymer is a thermoplastic polymer. In some preferred embodiments, the fiber material in the nonwoven sheet structure does not contain an added binder; that is, the fiber material is combined in the sheet by melting of the fiber intersections in the sheet structure without adding additional binder compounds to the sheet.
[0034] In some embodiments, the fibrous nonwoven sheet structure has a basis weight of less than 55 grams per square meter. In some more preferred embodiments, the fibrous nonwoven sheet structure has a basis weight of less than 50 grams per square meter; and in some most preferred embodiments, the fibrous nonwoven sheet structure has a basis weight of less than 45 grams per square meter.
[0035] In the fiber nonwoven sheet structure, preferred fibrous material is plexifilamentary. As used herein, term plexifilamentary and plexifilamentary refer to a large number of arbitrary lengths and have a thin, banded three-dimensional integrated network of film-fibrils less than the average fibril thickness of about 4 microns and less than the median width of about 25 microns. In plexifilamentary structure, film-fibrils are generally aligned with the longitudinal axis of the structure coextensively and they are combined and separated intermittently at irregular intervals in the different positions of the whole length, width and thickness of the structure, to form a continuous three-dimensional network. Such structure is further described in detail in U.S. Patent number 3,081,519 and 3,227,794.
[0036] A preferred method of making a fibrous nonwoven sheet structure having plexifilamentary fiber material is by flash spinning. The resulting fibrous nonwoven sheet structure containing plexifilamentary film-fibril elements is also referred to as a flash-spun plexifilamentary sheet.
[0037] Thus, a preferred fiber nonwoven sheet suitable for further bonding and embossing can be made using a general flash spinning technique as described in U.S. Pat. No. 3,227,794 to Anderson and U.S. Pat. No. 3,860,369 to Brethauer et al. Particularly preferred fiber nonwoven sheets suitable for further bonding and embossing can be made using a spinning solution comprising high density polyethylene and a hydrocarbon spinning agent as, for example, in U.S. Pat. Nos. 6,010,970; 7,338,916; 8,048,513; and 6,034,008. Preferably, the fiber nonwoven sheet suitable for further bonding has improved permeability and barrier strength properties by flash spinning the sheet from a hydrocarbon-based spinning solution comprising between 12% and 20% polyethylene by weight and maintained at a temperature above 180°C before flashing; in some embodiments, the temperature is between 185°C and 195°C before flashing.
[0038] The fiber material in the nonwoven sheet is preferably a polyolefin. The polyolefin may include polyethylene, polypropylene, polymethylpentene, polybutylene, and combinations thereof. Preferably, the polyolefin is polyethylene.
[0039] Polyethylene includes not only homopolymers of ethylene but also copolymers in which at least 85% of the repeating units are derived from ethylene. A preferred polyethylene is a linear high density polyethylene having an upper melting range of about 130.0°C to 137.0°C, a molecular weight of 0.94 to 0.98 g / cm 3 A density in the range of 100 and a melt index between 0.1 and 100 (preferably between 0.1 and 4) (as defined by ASTM D-1238-57T, condition E). Polypropylene includes not only homopolymers of propylene but also copolymers in which at least 85% of the repeating units are derived from propylene units.
[0040] The package comprising the air-permeable fibrous nonwoven sheet structure, the polymer connecting layer, and the package substrate provides a closed internal environment capable of being sterilized. The closed environment is formed by sealing the contact area between the first surface of the nonwoven pre-bonded with the embossed pattern and the package structure with the polymer connecting layer.
[0041] In some embodiments, the package may be a type of pouch made of a film having a cavity for the material to be packaged, wherein the fibrous nonwoven sheet seals the package. In this embodiment, it is preferred that the polymer tie layer is integral with the film of the pouch, the tie layer being essentially the film exposed on the interior of the pouch so that it is in contact with the fibrous nonwoven sheet.
[0042] Alternatively, in some embodiments, the package may be a type of blister package, wherein the package substrate has a thermoformed blister cavity for the material to be packaged and the fibrous nonwoven sheet structure provides a cover for the package. Again, in a preferred embodiment, the polymer tie layer is integral, is the inner surface of the thermoformed cavity, and together with the cover of the package is in contact with the fibrous nonwoven sheet that seals the cavity.
[0043] The plan views of the two packaging substrates with cavities 16 and 18 are respectively Figure 3 and Figure 4 , the packaging substrate has sealing areas 15 and 17 around the cavity, respectively. When the cavity is sealed, the fiber nonwoven sheet structure covers both the sealing area and the cavity. The polymer connecting layer is arranged in the sealing area, between the packaging substrate including the cavity and the fiber nonwoven sheet material. The polymer connecting layer can be integral with the packaging substrate, which is preferred.
[0044] In certain embodiments, the packaging is manufactured by forming a desired packaging substrate with a polymer tie layer, filling the cavity with the material to be packaged, and then applying a nonwoven sheet structure pre-bonded with an embossed pattern (the embossed pattern is in contact with the polymer tie layer), and then sealing. In certain embodiments, the nonwoven sheet structure can be a cover component of a blister package. The packaging is then sealed by heat, pressure, or a combination of the two.
[0045] In some embodiments, a heated platen heat sealing component is typically used. Although the cavity containing the item to be packaged is completely sealed, some other areas on the package do not need to be completely sealed if necessary to provide a starting point for peeling off the fibrous nonwoven sheet structure before removing the product. If the fibrous nonwoven sheet structure is not pre-printed before sealing, the nonwoven sheet structure can be printed just before or after heat sealing.
[0046] While the preferred package embodiment is a pouch or blister type package, it should be understood that any flexible or semi-rigid package including such packages in the form of packets, bags or sleeves may use the fibrous nonwoven sheet structure pre-bonded with an embossed pattern as a breathable feature.
[0047] The formed package has a closed internal environment for the item to be packaged, the closed internal environment is formed by sealing the contact area between the first surface of the nonwoven sheet structure and the package substrate, wherein the sealed contact area is a polymer connecting layer, and the first surface of the nonwoven sheet structure is pre-bonded with an embossed imprint pattern at least in the sealed contact area. In some embodiments, the formed package has a closed internal environment including the item packaged by the closed environment, the closed environment is formed by sealing the contact area between the first surface of the nonwoven sheet structure and the package substrate, wherein the sealed contact area is a polymer connecting layer, and the first surface of the nonwoven sheet structure is pre-bonded with an embossed imprint pattern at least in the sealed contact area.
[0048] In certain embodiments, the package formed is a peelable package of heat seal.As defined herein, phrase " peelable package " means that sheet structure is sealed on the package with " peelable seal ".As defined herein, phrase " peelable seal " means that the sheet structure sealed on the package has the average peak load seal strength of at least 0.5 lbf / inch until 4 lbf / inch or less maximum value.This means that can manually, by applying at least 0.5 lbf / inch seal and 4 lbf / inch seal at the most, remove sheet structure from the package sealed.In some preferred embodiments, maximum average peak load seal strength is 3 lbf / inch or less.In addition, because the fiber nonwoven sheet structure has at least one surface bonded with embossing embossing pattern, it makes the surface bonding embossing embossing pattern can form " peelable seal " with the package.
[0049] One measure of seal integrity is characterized by a dye penetration test as described in ASTM F1929-12. Surprisingly, it was found that packaging made with a nonwoven sheet structure pre-bonded with an embossed printed pattern and attached to a polymer tie layer in the seal area via the embossed surface had no negative impact on the dye penetration test.
[0050] The resulting wrapper has excellent sealing and peeling properties. Surprisingly, the use of a fibrous nonwoven sheet structure having at least one surface (in contact with the polymeric tie layer) pre-bonded with an embossed pattern can provide a wrapper having a clean peel and very low fiber tearing, or virtually no fiber tearing. Surprisingly, when the surface of the nonwoven sheet having the embossed pattern is sealed to a film, the peeling characteristics are improved.
[0051] Improved release characteristics are shown by showing both a reduction in the percentage of wrappers with fiber tear and / or a reduction in the severity of fiber tear. Specifically, it has been found that fibrous nonwoven sheet structures having at least one surface with an embossed imprint pattern have a significant reduction in wrappers that do not provide a clean release when compared to non-embossed materials. In particular, it has been found that the use of embossed sheet structures can provide a reduction of at least 25 percent in wrappers with visual fiber tear, preferably at least 30 percent, or even higher, when compared to non-embossed structures.
[0052] In addition, it has been found that the seal strength as measured by both the average mean load and the average peak load is improved compared to using a non-embossed fibrous nonwoven sheet structure. In other words, by using an embossed surface on the side of the fibrous nonwoven sheet structure that is in contact with the polymeric tie layer, both the seal strength and the peel quality are improved simultaneously.
[0053] Test Method
[0054] Basis Weight. Basis weight is measured according to ASTM D3776 (2009).
[0055] Glihill porosity (or just "Gurley porosity"; phrases used interchangeably herein) is a measure of the permeability of a sheet material to gaseous materials. Specifically, it is a measure of the time it takes a volume of gas to pass through an area of a material where a certain pressure gradient exists. Glihill porosity is measured according to TAPPI T-460OM-88 using a Lorentzen & Wettre model SE 166 or 516 from Lorentzen & Wettre, Kista, Sweden. This test measures the time required to push 100 cubic centimeters of air through a 28.7 mm diameter sample (having an area of 1 square inch) under a water pressure of approximately 1.21 kPa (4.9 inches). The results are expressed in seconds, which are commonly referred to as Gurley Seconds. The reported values represent the average of at least 12 separate measurements.
[0056] Moisture Vapor Transmission Rate. The moisture vapor transmission rate (MVTR) is measured according to EN ISO 12572, Hygrothermal performance of building materials and products, Climate C, 2001. The measurements are carried out using the multilayer method with a relative humidity in the cup of 100% and an air flow rate over the sample of 2.5 m / s and a measuring interval of 30 minutes. The resulting MVTR is measured based on the weight loss of water in the sample. The reported value represents the average of at least 1 measurement. The measurements are carried out on a Gintronic Gravitest 6400 with an ES 420A balance from MRS Seitter, Lenning-Brück, Germany.
[0057] Particle penetration. Particle penetration was measured on a TSI 8130 device from TSI, Ramsey County, Minnesota, USA. TSI 8310 is a device for measuring according to NIOSH procedure number RCT-APR-STP-57,58,59. For analysis, a TSI 8130 device was used, with a flow rate of 2.3 liters / minute produced by sodium chloride particles. In order to achieve a flow rate of 2.3 liters / minute, the control valve was closed, and the air flow was only generated by the air passing through the downstream photometer. The sodium chloride particle distribution has a count median diameter of 0.075 μm, a mass mean diameter of 0.3 μm, and a geometric standard deviation of 1.8. The measurement was performed with a rise time of 25 seconds and a measurement time of 4 seconds. The penetration is measured based on the difference in light intensity between the upstream and downstream photometers. The reported penetration is the average of at least 6 measurements. Alternatively, the particle penetration can be expressed as a logarithmic reduction value based on the following formula:
[0058] LRV-TSI 8130 = -log10 (penetration [%] / 100)
[0059] Elmendorf Tear. Elmendorf Tear is measured according to ISO 1974: 1990; Paper - Determination of tearing resistance (Elmendorf method). The Elmendorf is measured on a 09ED tear tester from Lorentzen & Wettre, Kista, Sweden. Elmendorf Tear is measured in both the machine direction (MD) and the cross direction (XD).
[0060] Mullen Burst Strength. Mullen Burst Strength was measured according to ISO 2758:2001, Paper-Determination of bursting strength. Mullen Burst was measured using a Lorenzen & Wettre model 519L from Lorentzen & Wettre, Kista, Sweden, integrated into an Autoline 400 from Lorentzen & Wettre, Kista, Sweden.
[0061] Seal Strength. Seal strength is measured according to ASTM F88 / F88M Appendix C using the "free tail" mode. Figure 5 As shown, 4 strips of each test package 25 are cut at a defined position with a width of 1 inch to test the seal 20. The strip edge is clearly defined and perpendicular to the direction of the seal. The most rigid part of the seal is placed on the upper fixture. The nonwoven sheet produced is the most rigid part in the seal, and is therefore placed on the upper fixture. The seal is tested at a grip separation rate of 300mm / min. The number of measurements for each test article is at least equal to 24. The seal strength is reported as the average value of the average load seal strength and the average value of the peak load seal strength, in pounds force / inch (lbf / in).
[0062] Dye penetration. Dye penetration is performed according to ASTM F1929-12 "Standard Test method for Detecting Seal Leaks in Porous Medical packaging by Dye Penetration". ASTM F1929-12 defines a procedure that will detect and locate leaks equal to or greater than the channel formed by a 50 μm (0.002 inch) line in the edge seal of the package formed between the transparent material and the porous sheet material. A dye penetrant solution is topically applied to the seal edge to test for leaks. After a specified time of contact with the dye penetrant of 5 seconds, the package is visually inspected for dye penetration. If no channel is visually seen, the package "passes" the dye penetration test.
[0063] Printing. The nonwoven sheets were printed with either a linear barcode or a 2D data matrix. Testing of linear barcodes was performed according to ISO 15416 and testing of 2-dimensional data matrices was performed as described in ISO 15415.
[0064] Fiber tearing. Fiber tearing is performed by visually inspecting the opened packages. The packages are opened manually in the following manner. The nonwoven sheet is grasped with one hand and the film is grasped with the other hand. The time to open one package is about one second. The package is not opened before reaching the lower edge seal. In other words, the package is not completely opened, but only opened on the top seal and two seals on the side. After opening each package, the surface of the nonwoven sheet sealed to the film is checked. The surface should be uniform and continuous, without peeling and tearing of the nonwoven sheet. If there is peeling or tearing of the nonwoven sheet, the package has fiber tearing. The above procedure is performed on at least 50 packages. The percentage of packages showing fiber tearing is determined by the number of packages showing fiber tearing divided by the total number of packages opened. Alternatively, fiber tearing can be performed according to EN 868-5 (2009), Annex E. However, this standard does not count some visual fibers of smaller lengths. As illustrated in the Examples and defined herein, a "package exhibiting fiber tear" is a package that has fibers of any length attached (visible to the naked eye) after opening.
[0065] Examples 1 and 2
[0066] An unfinished fiber nonwoven sheet for further bonding and embossing was made from a spinning solution containing high density polyethylene and n-pentane spinning agent using a general flash spinning process as described in Examples 9-15 of U.S. Pat. No. 6,034,008 to Lim et al. (except that the polymer concentration in the spinning solution was 17% by weight and the spinning temperature was 195° C.). The polyethylene had a melt flow index at 2.16 kg / 190° C. of about 0.75 g / 10 min (as measured by ASTM D1238-13). Two nonwoven sheets of different basis weights were made.
[0067] Then, by modifying the method described in U.S. Pat. No. 5,972,147 to Janis, in particular, Figure 2 The unfinished fiber nonwoven sheet is bonded with an embossed pattern by a modification of the apparatus shown in FIG. In the method shown in the figure, the sheet is alternately wrapped and preheated by a single set of two preheating rollers, and then the sheet is bonded in the nip of two sets of two calendering rollers, wherein the first set of rollers bonds one side of the sheet and the second set of rollers bonds the other side of the sheet; the sheet is then cooled by a single set of two cooling rollers.
[0068] Specifically, the Janis process is modified so that an additional set of preheat rolls is used, so that the sheet is alternately wrapped around four (as opposed to two) preheat rolls without any nip between the rolls. In addition, only the second set of calender rolls clamps the sheet, operating at a nip pressure of about 200 pounds per linear inch. The first set of calender rolls is left open and not clamping the sheet. This is followed by cooling the sheet with two sets of two cooling rolls (as opposed to a single set of two).
[0069] The specific equipment arrangement includes the bottom of the sheet wrapping around the first preheating roller (PH1), the top of the sheet wrapping around the second preheating roller (PH2), then the bottom of the sheet wrapping around the third preheating roller (PH3), and then the top of the sheet wrapping around the second preheating roller (PH4). Because the first set of calendering rollers do not clamp the sheet, the top surface of the sheet is not embossed. The second set of calendering rollers adheres to the bottom surface of the sheet and embosses a linen-like embossed pattern (such as a flax-like embossed pattern) into the surface of the sheet. Figure 1 shown).
[0070] The sheet was subsequently transferred to a cooling section and then wound into a roll. The temperatures of the preheat roll and embossing machine are shown in Table 1 and the resulting sheet properties are summarized in Table 2.
[0071] Table 1
[0072]
[0073]
[0074] Table 2
[0075]
[0076] Comparative Example A
[0077] An unfinished fiber nonwoven sheet for further bonding and embossing was made from a spinning solution comprising high density polyethylene and n-pentane spinning agent using the general flash spinning process described in Examples 9-15 of U.S. Patent No. 6,034,008 to Lim et al. (except that the polymer concentration in the spinning solution was 17% by weight and the spinning temperature was 185° C.). The polyethylene had a melt flow index at 2.16 kg / 190° C. of about 0.7 g / 10 min (as measured by ASTM D1238-13).
[0078] Then the unfinished fiber nonwoven sheet is generally bonded by the method described in the U.S. Patent No. 3,532,589 of David using a steam pressure of 66.7psia. This is the method for producing a "hard structure" nonwoven sheet described in the U.S. Patent No. 6,034,008 of Lim et al. In this method, the nonwoven sheet is subsequently passed through a heated drum, followed by a cooling drum, and then another heating drum and a cooling drum, with both sides of the thermal bonding material. The heating drum is maintained at a certain temperature, which will cause the nonwoven part to melt to cause the bonding of the sheet. The resulting sheet properties are summarized in Table 3.
[0079] Table 3
[0080]
[0081]
[0082] Example 3
[0083] The resulting nonwoven sheets from Example 1 and Comparative Example A (each having a 44 g / m 2 The Multivac R535 equipment produces 4 packages on one substrate, each package having a machine direction length of 200 mm, a transverse length of about 95 mm, and a sealing width of about 7.5 mm, such as Figure 3 5. The nonwoven sheet is attached to the packaging substrate in the sealing contact area using 2 different connecting film materials. Film 1 is Multifol GA 100 μm polyamide / polyethylene peelable film from Südpack Verpackungen GmbH & Co. KG, Ochsenhausen, Germany. Film 2 is ML E135TF PEEL, polyethylene / polyamide / polyethylene film from Wipak, Nastola, Finland.
[0084] In all cases, the bonding and embossing of the nonwoven surface of the nonwoven sheet of Example 1 with a linen pattern was sealed to the film. All packages were made with a sealing pressure of 6.5 bar and a dwell time of 1.2 seconds. The sealing temperature of each film was set to at least two levels - resulting in different sealing strengths. The package was then opened by peeling the nonwoven from the connecting film.
[0085] The sealing temperatures and the resulting seal strength values are given in Table 4. As the sealing temperature increases, the average peak seal strength and average average seal strength of the individual films increase. In addition, at higher seal strengths, the percentage of packages showing fiber tearing increases. However, in each case, the nonwoven sheet with the embossed pattern has improved both fiber tearing (peeling) and sealing properties, with the percentage reduction in fiber tearing ranging from 32% to 73%.
[0086] Table 4
[0087]
[0088]
[0089] Example 4 and Comparative Example B
[0090] Use 47g / m 2 The basis weight nonwoven sheet was repeated as in Example 2 with the same embossed linen pattern; however, the unfinished sheet was bonded using the embossing conditions shown in Table 5. The resulting bonded nonwoven sheet had a Gurley Porosity of 3.6 seconds.
[0091] For Comparative Example B, the process was repeated with the same basis weight sheet and temperature conditions as shown in Table 5, but without embossing the bottom of the sheet. (The sheet was not sandwiched between calender rolls.) The resulting nonwoven sheet was bonded without any embossing and had a Gurley Porosity of 2 seconds.
[0092] Table 5
[0093] Examples 3 B Temperature PH1(°F) 240 240 Temperature PH2 (°F) 272 272 Temperature PH3 (°F) 280 280 Temperature PH4 (°F) 286 286 Embossing machine 2 temperature (°F) 296 -
[0094] The resulting nonwoven sheet with a surface bonded and embossed with a linen pattern and a bonded nonwoven sheet without any embossing were then used to produce medical packaging using an Autovak M320 machine (Hong Kong, China). The Autovak machine simultaneously produces a nonwoven sheet with a machine direction length of about 190 mm and a cross direction length of 127 mm, and a seal width of 10 mm (eg Figure 4The nonwoven sheet was attached to the packaging substrate in the sealing contact area using a 135 μm thick polyamide / polyethylene peelable connecting film (with code UGBLGV340C, from 180 Zhongshan 5th Rd, Guangdong, China, Xiangfu (Zhongshan) Film Packaging Co., LTD, 180, Zhongshan 5th Rd, Guangdong, China). The film was preheated in the forming zone. The temperature in the forming zone was 105°C, and the dwell time was set to 1.0 second. The sealing temperature of all packagings was set to 120°C. The dwell time was adapted to change the resulting packaging seal strength. The sealing time and seal strength are shown in Table 6. The packaging was then opened by peeling the nonwoven from the connecting film. As shown in Table 6, the wrapper utilizing the nonwoven sheet that was only bonded but not embossed had higher seal strength properties but showed completely unacceptable fiber tear performance, while the wrapper utilizing the embossed nonwoven had acceptable seal strength properties and excellent fiber tear (peel) performance.
[0095] Table 6
[0096]
[0097]
[0098] Examples 5, 6, and 7
[0099] These examples show that embossing can be applied to the nonwoven sheet as a separate step after bonding the nonwoven sheet. Comparative Example B was repeated using two different nonwoven sheet basis weights, where the nonwoven sheet was bonded but not embossed. The bonded sheet was wound on a roll. The bonded nonwoven sheet roll was then subsequently unwound and embossed on one surface by clamping the sheet with a set of heated calender rolls, this time providing one surface of the sheet with a embossed pattern. Figure 2 The embossing pattern is shown as a dog-bone pattern instead of a linen pattern. The conditions for bonding and subsequent embossing are shown in Table 7. As in Example 4, the packaging is made with the same connecting film, wherein the embossed surface is in contact with the connecting film. The results are shown in Table 8.
[0100] Table 7
[0101] Examples 5 6 7 <![CDATA[Grammage (g / m 2 )]]> 41 47 47 Temperature PH1(°F) 240 240 240 Temperature PH2 (°F) 272 272 272 Temperature PH3 (°F) 280 280 280 Temperature PH4 (°F) 286 286 286 Embossing machine temperature (°F) 296 292 296 Gurley air porosity 2.6 4.8 3.2 Penetration-TSI 8130(%) 5.2 * 6.6 LRV-TSI 8130 1.3 * 1.2
[0102] (*- not measured)
[0103] Table 8
[0104]
[0105]
[0106] The package is then opened by peeling the nonwoven from the connecting film.As shown in Table 8, the package utilizing the embossed nonwoven has excellent peel properties.
[0107] Example 8
[0108] The nonwoven sheet structures with embossed imprint patterns used in Examples 1 to 7 were tested for shielding and mechanical properties. All of these inventive sheet structures had an Elmendorf tear above 2.0 N, a Mullen burst strength above 500 kPa. Using a TSI 8130 device operating at a flow rate of 2.3 L / min, all of the inventive sheet structures had a particle shield penetration of less than 10%. The non-embossed side of each nonwoven structure received printing in the form of a linear barcode and a 2D data matrix with good visual results.
Claims
1. A wound roll of a fibrous nonwoven sheet structure comprising a fibrous material, The sheet structure is air permeable and has a first surface and a second surface; The fibrous material on the first surface is surface bonded, and the second surface is capable of receiving printing, wherein the second surface has a smooth surface without any embossing; The sheet structure has a particle shield penetration of less than 10%, a Glihill porosity of 40 seconds or less, and a 3500 g / m 2 / day or greater moisture vapor transmission rate.
2. The wound roll of the fibrous nonwoven sheet structure of claim 1, wherein the fibrous nonwoven sheet structure has a Glihill porosity of 10 seconds or less.
3. A wound roll of a fibrous nonwoven sheet structure as claimed in any one of claims 1 or 2, wherein the fibrous nonwoven sheet structure has a density of 7500 g / m 2 / day or greater moisture vapor transmission rate.
4. A wound roll of a fibrous nonwoven sheet structure as claimed in any one of claims 1 or 2, wherein the sheet structure is plexifilamentary.
5. The wound roll of the fibrous nonwoven sheet structure of claim 1, wherein the fibrous nonwoven sheet structure comprises a flash spun nonwoven sheet structure.
6. The wound roll of the fibrous nonwoven sheet structure of claim 1, wherein the fibrous material is a thermoplastic polymer.
7. The wound roll of the fibrous nonwoven sheet structure of claim 1, wherein the fibrous material is free of added binder.
8. The wound roll of fibrous nonwoven sheet structure of claim 1, wherein the fibrous material is polyethylene, polypropylene, polymethylpentene, polybutylene, and combinations thereof.
9. The wound roll of a fibrous nonwoven sheet structure of claim 8, wherein the fibrous material is polyethylene.
10. The wound roll of the fibrous nonwoven sheet structure of claim 8, wherein the fibrous material is a high density polyethylene having an upper melting range of 130.0°C to 137.0°C, 0.94 to 0.98 g / cm 3 A density within a range and a melt index between 0.1 and 100 or between 0.1 and 4.
Citation Information
Patent Citations
Nonwoven medical fabric
CN101389286A
Pattern-unbonded nonwoven web and process for making same
CN1209177A
Full-surface bonded multiple component melt-spun nonwoven web
CN1890419A
Sheet materials
GB1436696A
Packaging product
US20020004351A1