Lithium iron phosphate positive electrode material precursor as well as preparation method, device and application thereof

Through a two-step oxidation method and induction reaction, combined with ferrous ion concentration monitoring and the use of nickel iron ore raw materials, the problems of raw material adaptability and low purity in the preparation of lithium iron phosphate cathode material precursors are solved, achieving high efficiency and low cost. production, improving product quality and production stability.

CN118723955AActive Publication Date: 2024-10-01YICHANG BRUNP YIHUA NEW MATERIAL CO LTD +2

Patent Information

Application Number
CN202410723137.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-10-01
Estimated Expiration
2044-06-05

AI Technical Summary

Technical Problem

The existing lithium iron phosphate cathode material precursor preparation process has the problems of single raw material adaptability, high cost, low product purity and many impurities. It is difficult to meet the synthesis and production needs of multiple types of raw materials, and the monitoring indicators are not sensitive enough, affecting production stability.

Method used

Using a two-step oxidation method combined with induction and aging steps, through primary oxidation, induction reaction and secondary oxidation, the concentration of ferrous ions is monitored for dosing control, and nickel-iron ore raw materials are used to achieve a wide range of raw material sources, sufficient reactions, and product purity. Preparation of high-quality lithium iron phosphate cathode material precursor.

Benefits of technology

It effectively reduces the impurity content in the lithium iron phosphate cathode material precursor, improves the purity and specific surface area of ​​the product, enables lower-cost production, and enhances the controllability and production stability of the preparation method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118723955A_ABST
    Figure CN118723955A_ABST
Patent Text Reader

Abstract

The invention discloses a lithium iron phosphate positive electrode material precursor as well as a preparation method, a device and application thereof, and the preparation method, the device and the application thereof have the advantages that the removal of impurities in the lithium iron phosphate positive electrode material precursor is facilitated through two-step oxidation heat preservation and monitoring of the end point of two-step oxidation through ferrous concentration, and raw materials from ferronickel ore can be utilized; the method has the advantages of wide raw material source, sufficient reaction and high product purity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery positive electrode materials, and in particular to a lithium iron phosphate positive electrode material precursor and a preparation method, device and application thereof. Background Art

[0002] As the research and development and industrialization of new energy vehicles have attracted much attention, lithium iron phosphate has become one of the mainstream positive electrode materials for new energy vehicle batteries.

[0003] There are three main methods for preparing lithium iron phosphate: ① Ferrous oxalate method and ferrous acetate method: This method was the first to be proposed for preparing lithium iron phosphate and is also the main process used in industrial-scale production. However, it is difficult, the compacted density of the product is low and the cost is high, so it has been gradually eliminated. ② Iron oxide red method: This method uses Fe 2 O 3 The raw material requirements are relatively strict, and the form and amount of divalent iron oxides may vary depending on the preparation process. ③ Ferric phosphate method and ferrous phosphate method: This is the current mainstream process route, but it requires that the iron-phosphorus molar ratio and the number of crystal water in the ferrous phosphate raw material must be constant to ensure the accuracy of the ingredients. It has become the mainstream process route.

[0004] The precursor of lithium iron phosphate is iron phosphate. So far, the main methods for synthesizing iron phosphate include co-precipitation, hydrothermal, sonicochemical, sol-gel, fluorine system, surfactant template, biological template, etc. The existing preparation process and equipment of lithium iron phosphate positive electrode material precursors have the following problems: 1. The adaptable synthetic raw materials are relatively single, which cannot meet the synthetic production requirements of various raw materials such as nickel-iron system, and cannot achieve lower-cost iron phosphate production; 2. The raw materials are not fully reacted, the product has many impurities and the product purity is low; the monitoring indicators are not sensitive enough, the error is large, which affects the production stability.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The purpose of the present invention is to provide a lithium iron phosphate positive electrode material precursor and a preparation method, device and application thereof. The preparation method has high controllability and low requirements for raw materials. The prepared lithium iron phosphate positive electrode material precursor has a low content of impurities, which is conducive to obtaining a high-quality lithium iron phosphate positive electrode material precursor.

[0007] The present invention is achieved in that:

[0008] In a first aspect, the present invention provides a method for preparing a lithium iron phosphate positive electrode material precursor, comprising:

[0009] Primary oxidation, reacting the phosphorus-formulated liquid containing ferrous ions and phosphate with a first oxidant to obtain a first ferric phosphate slurry, wherein the ferrous content in the first ferric phosphate slurry is 12-14 g / L, the concentration of ferrous ions in the phosphorus-formulated liquid is greater than 30 g / L, and the iron-phosphorus molar ratio of the phosphorus-formulated liquid is 0.9-1.0;

[0010] Inducing the reaction, adding FePO to the first iron phosphate slurry 4 an inducer for crystal formation to obtain a second ferric phosphate slurry;

[0011] Secondary oxidation, adding a second oxidant to the second ferric phosphate slurry to react to obtain a third ferric phosphate slurry, wherein the concentration of ferrous ions in the third ferric phosphate slurry is 1 g / L-2 g / L;

[0012] Calcination: After aging and solid-liquid separation of the third iron phosphate slurry, calcination is performed to obtain a lithium iron phosphate positive electrode material precursor.

[0013] In an optional embodiment, the iron-phosphorus molar ratio of the phosphorus-matched liquid is 0.96-0.98, and the ferrous ion concentration in the phosphorus-matched liquid is 40 g / L-70 g / L;

[0014] Preferably, the temperature of the primary oxidation step is 45°C-55°C;

[0015] Preferably, the first oxidant is hydrogen peroxide.

[0016] In an optional embodiment, the inducing agent is hexadecyltrimethylammonium bromide;

[0017] Preferably, the amount of the inducer is 1.5wt%-2.5wt% of the first ferric phosphate slurry;

[0018] Preferably, the induction reaction temperature is 65°C-75°C, and the time is 2.5h-3.5h.

[0019] In an optional embodiment, the temperature of the secondary oxidation step is 90°C-100°C, and the time is 3.5h-4.5h;

[0020] Preferably, the second oxidant is hydrogen peroxide.

[0021] In an optional embodiment, the temperature of the aging step is 70°C-95°C, and the time is 8h-10h.

[0022] In an optional embodiment, the calcination temperature is 550°C-600°C, and the calcination time is 2.5-3.5 hours.

[0023] In the second aspect, the present invention provides an apparatus for the preparation method of the lithium iron phosphate positive electrode material precursor as described in any one of the aforementioned embodiments, comprising: a post-phosphorus preparation liquid tank, a multi-stage reaction tank and an aging and insulation tank connected in series in sequence, the multi-stage reaction tank is provided with an inducer dosing tube, an oxidant dosing tube for adding a first oxidant and a second oxidant, the multi-stage reaction tank is also provided with a dosing control probe for measuring the concentration of ferrous ions, the dosing control probe is connected to a dosing controller capable of controlling the liquid flow in the oxidant dosing tube via a dosing control signal line.

[0024] In an optional embodiment, the aging and heat preservation tank is connected in series via a discharge pipe to a filter press for filtering the slurry, a drying device for drying the filter cake obtained by the filtration, and a rotary kiln for calcining the dried material.

[0025] In a third aspect, the present invention provides a lithium iron phosphate positive electrode material precursor, which is prepared by the preparation method of the lithium iron phosphate positive electrode material precursor described in any one of the aforementioned embodiments.

[0026] In a fourth aspect, the present invention provides a lithium iron phosphate positive electrode material, which is obtained by mixing the lithium iron phosphate positive electrode material precursor described in the above embodiment with a lithium source and then sintering.

[0027] In a fifth aspect, the present invention provides a lithium-ion battery comprising the lithium iron phosphate positive electrode material described in the aforementioned embodiment.

[0028] The present invention has the following beneficial effects:

[0029] The present invention is beneficial to the removal of impurities in the lithium iron phosphate positive electrode material precursor by two-step oxidation insulation and monitoring the endpoint of the two-step oxidation by ferrous concentration, and can utilize raw materials derived from nickel-iron ore, thereby achieving the advantages of wide raw material sources, sufficient reaction and high product purity. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0031] Figure 1 This is a flow chart of a method for preparing a lithium iron phosphate positive electrode material precursor in Example 1 of the present invention;

[0032] Figure 2 This is a schematic structural diagram of a device for lithium iron phosphate cathode material precursor used in Example 1 of the present invention;

[0033] Figure 3 This is a SEM image of the lithium iron phosphate cathode material precursor prepared in Example 1;

[0034] Figure 4 This is a SEM image of the lithium iron phosphate positive electrode material precursor prepared in Example 2.

[0035] In the figure: 1.1-phosphorus preparation liquid feed pipeline; 1.2-phosphorus preparation liquid tank; 1.3-phosphorus preparation liquid pump; 2.1-steam pipeline; 2.1.1-steam heating coil; 2.2-hydrogen peroxide dosing pump; 2.3-dosing controller; 2.3.1-dosing control probe; 2.3.2-dosing control signal line; 2.4-inducing agent dosing pump; 2.6-multi-stage reaction tank; 2.7-aging and insulation tank; 2.8-filter press; 2.9-flash evaporation device; 2.10-rotary kiln; 2.11-finished product. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0037] An embodiment of the present invention provides a method for preparing a lithium iron phosphate positive electrode material precursor, comprising:

[0038] Primary oxidation, reacting the phosphorus-formulated liquid containing ferrous ions and phosphate with a first oxidant to obtain a first ferric phosphate slurry, wherein the ferrous content in the first ferric phosphate slurry is 12-14 g / L, the concentration of ferrous ions in the phosphorus-formulated liquid is greater than 30 g / L, and the iron-phosphorus molar ratio of the phosphorus-formulated liquid is 0.9-1.0;

[0039] Inducing the reaction, adding FePO to the first iron phosphate slurry 4 an inducer for crystal formation to obtain a second ferric phosphate slurry;

[0040] Secondary oxidation, adding a second oxidant to the second ferric phosphate slurry to react to obtain a third ferric phosphate slurry, wherein the concentration of ferrous ions in the third ferric phosphate slurry is 1 g / L-2 g / L;

[0041] Calcination: After aging and solid-liquid separation of the third iron phosphate slurry, calcination is performed to obtain a lithium iron phosphate positive electrode material precursor.

[0042] The impurity content in the lithium iron phosphate positive electrode material precursor has a great influence on the lithium iron phosphate positive electrode material. The leachate obtained from the acid leaching of nickel iron ore contains a large amount of nickel and sulfur elements, which are easily mixed in the lithium iron phosphate positive electrode material precursor, making it difficult to obtain high-quality lithium iron phosphate positive electrode material.

[0043] In the embodiment of the present invention, the first oxidant is used in the primary oxidation to oxidize most of the ferrous ions in the reaction solution into ferric iron to obtain the first iron phosphate slurry. The first iron phosphate slurry is acidic, which is not conducive to the precipitation of iron phosphate. Therefore, an inducing agent is added to the reaction solution after the primary reaction to induce iron phosphate to precipitate under acidic conditions, and a second iron phosphate slurry with a greater concentration of iron phosphate crystals is obtained. At the same time, while the iron phosphate crystals are precipitated, since there are still a large number of unoxidized ferrous ions in the reaction system, the ferric iron in the iron phosphate crystals will undergo a replacement reaction with the free ferrous ions in the reaction system, and the movement of the iron ions makes the channels in the iron phosphate crystals larger, which is conducive to the removal of impurities such as Ni and S wrapped in the iron phosphate precipitation, so the purity of the iron phosphate crystals contained in the third iron phosphate slurry is greater than the purity of the iron phosphate crystals contained in the second iron phosphate slurry, which is conducive to reducing the impurity content in the lithium iron phosphate positive electrode material precursor product.

[0044] In addition, secondary oxidation is carried out after the induction reaction to oxidize the remaining divalent iron ions in the second ferric phosphate slurry. It should be noted that, during the secondary oxidation, not all ferrous ions are oxidized, and some ferrous ions also remain, so that the concentration of ferrous ions in the third ferric phosphate slurry is 1g / L-2g / L, so that in the subsequent aging step, ferrous ions and ferric ions undergo a replacement reaction to promote the removal of impurities.

[0045] It should be noted that, since the pH of the liquid after phosphorus matching is about 0.5, acidity is high, pH fluctuation is small as the reaction proceeds, and the accuracy of monitoring is low. In the present application, the reaction process is monitored by monitoring the content of ferrous ions, which is more accurate than detecting pH. In addition, the utilization rate of the oxidant in the initial reaction step is relatively higher, therefore, while ensuring that impurities are removed to meet the requirements, the ferrous content in the first ferrous phosphate slurry should be as low as possible; The ferrous ion concentration in the third ferrous phosphate slurry is improved within a certain range, which is conducive to the removal of impurities, but the excessive concentration is not conducive to the improvement of ferrous ion conversion rate.

[0046] After aging, the slurry is separated into solid and liquid, mainly to remove the free water contained in the iron phosphate. However, since the iron phosphate crystals also contain bound water, the iron phosphate crystals need to be calcined to remove the bound water to obtain the lithium iron phosphate positive electrode material precursor. In addition, during the calcination process, impurities such as sulfur will also escape, and a large number of channels will be generated when the impurities and bound water escape, which is conducive to increasing the specific surface area of ​​the lithium iron phosphate positive electrode material precursor.

[0047] In some embodiments, the iron-phosphorus molar ratio of the phosphorus-formulated solution is 0.96-0.98;

[0048] Normally, the iron-phosphorus molar ratio in the phosphorus-containing solution used in preparing the lithium iron phosphate positive electrode material precursor is about 0.9. In the embodiment of the present invention, the iron-phosphorus molar ratio in the phosphorus-containing solution can be increased to 0.96-0.98, which is beneficial to improve the utilization rate of phosphorus.

[0049] In some embodiments, the concentration of ferrous ions in the phosphate-matched solution is 40 g / L-70 g / L.

[0050] Normally, the concentration of ferrous ions in the post-phosphorus solution used in the preparation of lithium iron phosphate positive electrode material precursor is 40g / L-50g / L. If the post-phosphorus solution is concentrated to increase the concentration of ferrous ions in the post-phosphorus solution, the concentration of impurities in the post-phosphorus solution will also increase in proportion, thereby increasing the content of impurities mixed in the iron phosphate crystals, resulting in a decrease in the quality of the lithium iron phosphate positive electrode material precursor finally prepared. In the present application, the impurities mixed in the iron phosphate crystals are significantly reduced by combining two-stage oxidation with induction and aging steps, so that the preparation method in the present application can obtain a higher quality lithium iron phosphate positive electrode material precursor even if a concentrated post-phosphorus solution with a higher ferrous ion concentration is used. In the present invention, increasing the concentration of ferrous ions in the post-phosphorus solution is conducive to increasing production capacity and reducing energy consumption.

[0051] In some embodiments, the temperature of the primary oxidation step is 45° C.-55° C., which is conducive to the oxidation reaction and improves the utilization rate of the first oxidant.

[0052] In some embodiments, the first oxidant is hydrogen peroxide, which can oxidize ferrous ions into ferric ions without introducing impurities.

[0053] In some embodiments, the inducer is hexadecyltrimethylammonium bromide, which can effectively induce the precipitation of ferric phosphate under acidic conditions.

[0054] In some embodiments, the amount of the inducer is 1.5wt%-2.5wt% of the first ferric phosphate slurry. Controlling the amount of the inducer is beneficial to promoting the precipitation of ferric phosphate while avoiding the influence of the inducer residue on the final product.

[0055] In some embodiments, the induction reaction temperature is 65°C-75°C, and the time is 2.5h-3.5h. In the embodiment of the present application, the primary oxidation reaction releases heat, which increases the temperature of the reaction system; at the same time, in order to control the precipitation speed of iron phosphate crystals not too fast to avoid a large amount of impurities, the induction reaction temperature should not be too high.

[0056] In some embodiments, the temperature of the secondary oxidation step is 90°C-100°C, and the time is 3.5h-4.5h. In the embodiment of the present application, the secondary oxidation step releases heat, causing the temperature of the reaction liquid to rise, so the temperature of the secondary oxidation step is higher than the temperature of the induction reaction, and at the same time, keeping warm at this temperature for 3.5h-4.5h is conducive to the conversion of the amorphous iron phosphate crystals into fixed crystals.

[0057] In some embodiments, the second oxidant is hydrogen peroxide, which can oxidize ferrous ions into ferric ions without introducing impurities.

[0058] In some embodiments, the temperature of the aging step is 70° C.-95° C. and the time is 8 h-10 h. This temperature is conducive to the further growth and perfection of the iron phosphate crystals.

[0059] In some embodiments, the calcination temperature is 550° C.-600° C. and the time is 2.5-3.5 hours. This temperature is conducive to the removal of bound water and impurities, and at the same time, the lithium iron phosphate cathode material precursor has a suitable specific surface area.

[0060] The present invention also provides an embodiment of a device for the preparation method of the lithium iron phosphate positive electrode material precursor applied to any one of the aforementioned embodiments, comprising: a post-phosphorus preparation liquid tank 1.2, a multi-stage reaction tank 2.6 and an aging and insulation tank 2.7 connected in series in sequence, the multi-stage reaction tank 2.6 is provided with an inducer dosing tube, an oxidant dosing tube for adding a first oxidant and a second oxidant, the multi-stage reaction tank 2.6 is also provided with a dosing control probe 2.3.1 for measuring the concentration of ferrous ions, the dosing control probe 2.3.1 is connected to a dosing controller 2.3 capable of controlling the liquid flow in the oxidant dosing tube via a dosing control signal line 2.3.2.

[0061] In the embodiment of the present application, the concentration of ferrous ions in the reaction solution is measured by the dosing control probe 2.3.1, and the concentration of ferrous ions is fed back to the dosing control instrument 2.3 in real time, so that the dosing control instrument 2.3 controls the amount of the first oxidant or the second oxidant added. The amount of the oxidant added is determined by detecting the concentration of ferrous ions. The device has a high degree of automation, a high accuracy of the detection result, and a low manual error, which is conducive to improving production efficiency and improving product stability.

[0062] In some embodiments, the aging and heat preservation tank is connected in series via a discharge pipe to a filter press 2.8 for filtering the slurry, a drying device for drying the filter cake obtained by the filtering, and a rotary kiln 2.10 for calcining the dried material.

[0063] Specifically, the working process of the production device of the lithium iron phosphate positive electrode material precursor in the embodiment of the present invention is divided into:

[0064] A. Primary reaction: the phosphorus-formulated liquid enters the phosphorus-formulated liquid tank 1.2 through the phosphorus-formulated liquid feeding pipeline 1.1, and enters the multi-stage reaction tank 2.6 through the phosphorus-formulated liquid pump 1.3. The steam enters the steam heating coil 2.1.1 through the steam pipeline 2.1 to heat the phosphorus-formulated liquid in the multi-stage reaction tank 2.6. The stirring is started. When the dosing controller 2.3 detects that the liquid temperature has reached the specified temperature, it preliminarily calculates the amount of hydrogen peroxide added for the first time according to the monitored ferrous content, starts the hydrogen peroxide dosing pump 2.2, and adds hydrogen peroxide into the multi-stage reaction tank 2.6 for oxidation reaction until the ferrous content in the first ferric phosphate slurry is 12-14 g / L. If the amount of hydrogen peroxide added is insufficient, the dosing controller 2.3 can control the hydrogen peroxide dosing pump 2.2 to add hydrogen peroxide. In order to avoid a large temperature fluctuation in the multi-stage reaction tank 2.6 caused by the addition of hydrogen peroxide, a steam pipeline 2.1 can be provided on the outer layer of the oxidant dosing pipe to preheat the oxidant.

[0065] B. Induced reaction: by increasing the steam volume of the steam heating coil 2.1.1, the temperature of the liquid after the first oxidation is raised to the specified temperature of the induced reaction, and then the inducer dosing pump 2.4 is started through the dosing controller 2.3, and the inducer is quantitatively added and kept warm for a preset time to achieve the precipitation of iron phosphate, and promote the removal of Ni and S impurities, thereby improving the purity of iron phosphate in the slurry;

[0066] C. Secondary oxidation reaction: After the induction reaction is completed, the concentration of ferrous iron is detected by the dosing controller 2.3, and the amount of the hydrogen peroxide dosing pump 2.2 added is calculated and adjusted according to the feedback signal of the ferrous iron concentration. The steam volume of the steam heating coil 2.1.1 is increased, the temperature is raised to the secondary oxidation temperature and then kept warm. In this process, hydrogen peroxide is quantitatively added for the second time to achieve the formation of ferric phosphate precipitate by ferrous iron and phosphoric acid under the oxidation action of hydrogen peroxide, thereby improving the utilization rate of ferrous iron and the purity of ferric phosphate precipitate.

[0067] D. The iron phosphate slurry produced after the reaction in the multi-stage reaction tank 2.6 is transported to the aging and heat preservation tank 2.7 by a pump, in which the aging reaction is completed to further promote the crystallization and molding of the iron phosphate. The molded iron phosphate slurry enters the filter press 2.8 by a pump for filtration and washing. After the impurities are removed, they are washed and removed. After the impurities are removed, the iron phosphate filter cake is conveyed to the flash evaporator 2.9 by a belt to be crushed and dried to become iron phosphate powder. Subsequently, the iron phosphate powder enters the rotary kiln 2.10 for calcination, dehydration and desulfurization to produce qualified iron phosphate products.

[0068] In the device of the present invention, the input end of the feeding controller 2.3 is connected to the feeding control probe 2.3.1 through the feeding control signal line 2.3.2, and the output end is connected to the hydrogen peroxide feeding pump 2.2 and the inducer feeding pump 2.4 through the feeding control signal line 2.3.2. The temperature and ferrous iron concentration are detected by the feeding control probe 2.3.1, and after the temperature reaches the standard, the hydrogen peroxide feeding amount is calculated by the feedback ferrous iron concentration signal using the built-in feeding calculation program of the feeding controller 2.3, and the flow regulating knob of the hydrogen peroxide feeding pump 2.2 is adjusted according to the calculated value of the feeding amount to realize automatic feeding control; the inducer feeding amount is calculated by the feedback total iron concentration signal using the built-in feeding calculation program of the feeding controller 2.3, and the flow regulating knob of the inducer feeding pump 2.4 is adjusted according to the calculated value of the feeding amount to realize automatic feeding control.

[0069] Another embodiment of the present invention provides a lithium iron phosphate positive electrode material precursor, which is prepared by the preparation method of the lithium iron phosphate positive electrode material precursor described in any one of the aforementioned embodiments.

[0070] Another embodiment of the present invention provides a lithium iron phosphate positive electrode material, which is obtained by mixing the lithium iron phosphate positive electrode material precursor described in the above embodiment with a lithium source and then sintering.

[0071] The present invention provides a positive electrode plate, comprising the positive electrode material described in the above embodiment.

[0072] In the positive electrode sheet of the present invention, the positive electrode film layer generally comprises the positive electrode material and optionally a binder and optionally a conductive agent, and is generally formed by coating the positive electrode slurry, drying, and cold pressing. The positive electrode slurry is generally formed by dispersing the positive electrode material and optionally a conductive agent and optionally a binder in a solvent and stirring them uniformly. The solvent may be N-methylpyrrolidone (NMP).

[0073] In some optional embodiments, based on the total weight of the positive electrode film layer, the positive electrode film layer may contain 70wt% to 97wt% of the positive electrode material. Optionally, the weight proportion of the positive electrode material in the positive electrode film layer is 85% to 97%, 90% to 97%, or 95% to 97%. By regulating the proportion of the positive electrode material in the positive electrode film layer, the energy density and cycle life of the lithium-ion battery can be further improved.

[0074] In some embodiments, the binder of the positive electrode film layer may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and modified polymers thereof.

[0075] The conductive agent can improve the electronic conductivity of the positive electrode film layer. In some optional embodiments, based on the total weight of the positive electrode film layer, the positive electrode film layer may contain 2 wt% to 20 wt% of the conductive agent. Optionally, the weight proportion of the conductive agent in the positive electrode film layer is 2% to 10%, or 2% to 5%.

[0076] In some embodiments, the conductive agent of the positive electrode film layer may include one or more of superconducting carbon, carbon black (such as SuperP, acetylene black, Ketjen black), carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0077] It should be noted that the composition or parameters of each positive electrode film layer given in the present invention refer to the composition or parameter range of the single-sided film layer of the positive electrode current collector. When the positive electrode film layer is arranged on two opposite surfaces of the positive electrode current collector, the composition or parameters of the positive electrode film layer on any one of the surfaces meet the requirements of the present invention, which is considered to fall within the protection scope of the present invention.

[0078] The present invention provides a lithium-ion battery, comprising the positive electrode sheet described in the above embodiment, and also comprising a negative electrode sheet, an electrolyte and a separator.

[0079] [Negative electrode]

[0080] The negative electrode plate of the present invention comprises a negative electrode current collector and a negative electrode film layer arranged on at least one surface of the negative electrode current collector.

[0081] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is laminated on any one or both of the two opposite surfaces of the negative electrode current collector.

[0082] The negative electrode current collector may be made of a material with good electrical conductivity and mechanical strength to perform the functions of conducting and collecting current. In some embodiments, the negative electrode current collector may be made of copper foil.

[0083] In the negative electrode sheet of the present invention, the negative electrode film layer generally comprises a negative electrode active material and optionally a binder, optionally a conductive agent and other optional additives. It is generally formed by coating a negative electrode slurry on a negative electrode current collector, drying, and cold pressing. The negative electrode slurry is generally formed by dispersing a negative electrode positive electrode material and optionally a conductive agent, optionally a binder, and optionally a additive in a solvent and stirring uniformly. The solvent may be N-methylpyrrolidone (NMP) or deionized water.

[0084] In some embodiments, the negative electrode active material may include one or more of artificial graphite, natural graphite, silicon-based materials, and tin-based materials. Alternatively, the negative electrode active material includes one or more of artificial graphite and natural graphite. Alternatively, the negative electrode active material includes artificial graphite.

[0085] In some embodiments, the conductive agent may include one or more of superconducting carbon, carbon black (eg, SuperP, acetylene black, Ketjen black, etc.), carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0086] In some embodiments, the binder may include one or more of styrene-butadiene rubber (SBR), water-based acrylic resin, polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS).

[0087] In some embodiments, other optional auxiliary agents include, for example, a thickener (eg, sodium carboxymethyl cellulose CMC-Na), a PTC thermistor material, and the like.

[0088] [Electrolytes]

[0089] The electrolyte plays a role in conducting ions between the positive electrode and the negative electrode. The present invention has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can be selected from an electrolyte. The electrolyte includes an electrolyte salt and a solvent.

[0090] In some embodiments, the electrolyte salt may be selected from lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ), lithium perchlorate (LiClO 4 ) lithium hexafluoroarsenate (LiAsF 6 ), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate 2 (LiPO 2 F), one or more of lithium difluorooxalate phosphate (LiDFOP) and lithium tetrafluorooxalate phosphate (LiTFOP).

[0091] In some embodiments, the solvent can be selected from one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).

[0092] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high temperature performance, and additives that improve battery low temperature performance.

[0093] [Isolation film]

[0094] The separator is disposed between the positive electrode sheet and the negative electrode sheet to play a role of isolation. The lithium ion battery of the present invention has no particular restrictions on the type of separator, and any known porous structure separator for lithium ion batteries can be selected. For example, the separator can be selected from one or more of a glass fiber film, a non-woven film, a polyethylene film, a polypropylene film, a polyvinylidene fluoride film, and a multilayer composite film containing one or more of them.

[0095] The positive electrode sheet, the negative electrode sheet and the isolation film can be made into an electrode assembly through a lamination process or a winding process, so that the isolation film is placed between the positive electrode sheet and the negative electrode sheet to play an isolation role; the electrode assembly is placed in an outer package, the electrolyte is injected and sealed, and a lithium-ion battery can be obtained.

[0096] The outer packaging of the lithium-ion battery is used to encapsulate the electrode assembly and the electrolyte. In some embodiments, the outer packaging of the lithium-ion battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the lithium-ion battery can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc.

[0097] The present invention has no particular limitation on the shape of the lithium-ion battery, which may be cylindrical, square or any other shape.

[0098] In some embodiments, lithium-ion batteries may be assembled into a battery module. The battery module may contain multiple lithium-ion batteries, and the specific number may be adjusted according to the application and capacity of the battery module.

[0099] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0100] The present invention provides an electrical device, comprising the lithium-ion battery described in the aforementioned embodiment.

[0101] The present invention also provides an electrical device, which includes at least one of the lithium-ion battery, battery module, or battery pack described in the present invention. The lithium-ion battery, battery module, or battery pack can be used as a power source for the device, or as an energy storage unit for the device. The device can be, but is not limited to, a mobile device (such as a mobile phone, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc. The device can select a lithium-ion battery, a battery module, or a battery pack according to its use requirements.

[0102] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0103] Example 1

[0104] This embodiment provides a method for preparing a lithium iron phosphate positive electrode material precursor, and the specific steps are as follows: Figure 1 As shown, use Figure 2 The device shown in the figure comprises the following specific steps:

[0105] Primary reaction: Fe 2+ Concentration 65g / L, Ni 2+ The post-phosphorus liquid with a concentration of 62g / L and an iron-phosphorus ratio of 0.965 was pumped from the post-phosphorus liquid tank to the multi-stage reaction tank. After the temperature was raised to 50°C by the steam heating coil 2.1.1, 23.02kg of 27.5% hydrogen peroxide was added by the dosing controller. After the primary reaction was completed, the ferrous iron concentration in the reaction system was 13.2g / L.

[0106] Induction reaction: After the primary reaction is completed, the liquid in the multi-stage reaction tank is heated to 70°C by the steam heating coil 2.1.1, and the dosing controller controls the induction agent dosing pump to add CTAB induction agent to promote precipitation. The amount of CTAB added is 2wt% of the liquid in the multi-stage reaction tank. After the addition of CTAB, the reaction liquid is kept at 70°C for 3 hours. During the insulation process, the amorphous iron phosphate precipitate is converted into orthorhombic iron phosphate.

[0107] Secondary oxidation: After the reaction is induced, the dosing controller automatically monitors the concentration of ferrous iron in the reaction solution and adds 5.7 kg of 27.5% hydrogen peroxide for the second time until the concentration of ferrous iron in the reaction solution is 1.51 g / L. The liquid is heated to 95°C by the heating coil and kept warm for 4 hours.

[0108] Aging, filter pressing, flash evaporation, and rotary kiln calcination: After the liquid in the multi-stage reaction tank is kept at 95°C for 4 hours, it enters the insulation aging tank for 9 hours. After the aging and insulation are completed, it enters the filter pressing system, completes the filter pressing and washing, and obtains the filter cake. At this time, the Ni content in the filter cake is 90ppm and the S content is 2000ppm as detected by ICP. The filter cake is flash dried and calcined in a rotary kiln at 580°C for 3 hours to obtain the finished iron phosphate. The finished iron phosphate is tested by ICP for Ni: 120ppm and S: 150ppm. The finished iron phosphate SEM is as follows Figure 3 , the particles have high sphericity and concentrated particle size distribution.

[0109] Embodiment 2:

[0110] This embodiment provides a method for preparing a lithium iron phosphate positive electrode material precursor, and the specific steps are as follows: Figure 1 As shown, use Figure 2 The device shown in the figure comprises the following specific steps:

[0111] Primary reaction: Fe 2+ Concentration 65g / L, Ni 2+ 400L of the post-phosphorus liquid with a concentration of 62g / L and an iron-phosphorus ratio of 0.963 was pumped from the post-phosphorus liquid tank to the multi-stage reaction tank. After the temperature was raised to 50°C by the steam heating coil 2.1.1, 23.12kg of 27.5% hydrogen peroxide was added by the dosing controller. After the primary reaction was completed, the ferrous iron concentration in the reaction system was 12.8g / L.

[0112] Induction reaction: After the primary reaction is completed, the liquid in the multi-stage reaction tank is heated to 70°C by the steam heating coil 2.1.1, and the dosing controller controls the induction agent dosing pump to add CTAB induction agent to promote precipitation. The amount of CTAB added is 2wt% of the liquid in the multi-stage reaction tank. After the addition of CTAB, the reaction liquid is kept at 70°C for 3 hours. During the insulation process, the amorphous iron phosphate precipitate is converted into orthorhombic iron phosphate.

[0113] Secondary oxidation: After the reaction is induced, the dosing controller automatically monitors the concentration of ferrous iron in the reaction solution and adds 5 kg of 27.5% hydrogen peroxide for the second time until the concentration of ferrous iron in the reaction solution is 1.49 g / L. The liquid is heated to 95°C by the heating coil and kept warm for 4 hours.

[0114] Aging, filter pressing, flash evaporation, and rotary kiln calcination: After the liquid in the multi-stage reaction tank is kept at 95°C for 4 hours, it enters the insulation aging tank for 9 hours. After aging and insulation, it enters the filter pressing system, completes the filter pressing and washing, and obtains the filter cake. At this time, the Ni in the filter cake is 85ppm and the S is 2100ppm as detected by ICP. The filter cake is flash dried and calcined in a rotary kiln at 580°C for 3 hours to obtain the finished iron phosphate. The finished iron phosphate is tested by ICP for Ni: 115ppm and S: 160ppm. The SEM of the finished iron phosphate is Figure 4 , the particles have high sphericity and concentrated particle size distribution.

[0115] Example 3

[0116] This embodiment provides a method for preparing a lithium iron phosphate positive electrode material precursor, which is different from Example 1 only in that the amount of hydrogen peroxide used in the primary reaction and the secondary oxidation steps is adjusted so that the ferrous iron concentration in the reaction system is 12 g / L after the primary reaction is completed, and the ferrous iron concentration in the reaction system is 1.49 g / L after the secondary oxidation is completed.

[0117] Example 4

[0118] This embodiment provides a method for preparing a lithium iron phosphate positive electrode material precursor, which is different from Example 1 only in that the amount of hydrogen peroxide used in the primary reaction and the secondary oxidation steps is adjusted so that the ferrous iron concentration in the reaction system after the primary reaction is completed is 14 g / L, and the ferrous iron concentration in the reaction system after the secondary oxidation is completed is 1.49 g / L.

[0119] Example 5

[0120] This embodiment provides a method for preparing a lithium iron phosphate positive electrode material precursor, which is different from Embodiment 1 only in that the amount of hydrogen peroxide used in the secondary oxidation step is adjusted so that the ferrous iron concentration in the reaction system is 1 g / L after the secondary oxidation is completed.

[0121] Example 6

[0122] This embodiment provides a method for preparing a lithium iron phosphate positive electrode material precursor, which is different from Embodiment 1 only in that the amount of hydrogen peroxide used in the secondary oxidation step is adjusted so that the ferrous iron concentration in the reaction system is 2 g / L after the secondary oxidation is completed.

[0123] Example 7

[0124] This embodiment provides a method for preparing a lithium iron phosphate positive electrode material precursor, which is different from Example 1 only in that the ferrous ion concentration is 70 g / L, the iron-phosphorus molar ratio is 0.98, and the ferrous concentration in the reaction system after the primary reaction and the secondary oxidation are completed is equal to that in Example 1.

[0125] Example 8

[0126] This embodiment provides a method for preparing a lithium iron phosphate positive electrode material precursor, and the specific steps are as follows: Figure 1 As shown, use Figure 2 The device shown in the figure comprises the following specific steps:

[0127] Primary reaction: Fe 2+ Concentration 70g / L, Ni 2+The post-phosphate liquid with a concentration of 62g / L and an iron-phosphorus ratio of 0.96 is pumped from the post-phosphate liquid tank to the multi-stage reaction tank. After the temperature is raised to 50°C by the steam heating coil 2.1.1, 27.5% hydrogen peroxide is added by the dosing controller. After the primary reaction is completed, the ferrous iron concentration in the reaction system is 12g / L.

[0128] Induction reaction: After the primary reaction is completed, the liquid in the multi-stage reaction tank is heated to 65°C by the steam heating coil 2.1.1, and the dosing controller controls the induction agent dosing pump to add CTAB induction agent to promote precipitation. The amount of CTAB added is 1.5wt% of the liquid in the multi-stage reaction tank. After the addition of CTAB, the reaction liquid is kept at 65°C for 3.5h. During the insulation process, the amorphous iron phosphate precipitate is converted into orthorhombic iron phosphate.

[0129] Secondary oxidation: After the reaction is induced, the dosing controller automatically monitors the concentration of ferrous iron in the reaction solution and adds hydrogen peroxide with a concentration of 27.5 for the second time until the concentration of ferrous iron in the reaction solution is 2g / L. The liquid is heated to 90°C by the heating coil and kept warm for 4.5 hours.

[0130] Aging, filter pressing, flash evaporation, and rotary kiln calcination: After the liquid in the multi-stage reaction tank is kept at 90°C for 4.5 hours, it enters the insulation aging tank for 10 hours. After the aging and insulation are completed, it enters the filter pressing system, completes the filter pressing and washing, and obtains the filter cake. The filter cake is flash dried and calcined in a rotary kiln at 550°C for 3.5 hours to obtain the finished iron phosphate.

[0131] Example 9

[0132] This embodiment provides a method for preparing a lithium iron phosphate positive electrode material precursor, and the specific steps are as follows: Figure 1 As shown, use Figure 2 The device shown in the figure comprises the following specific steps:

[0133] Primary reaction: Fe 2+ Concentration 40g / L, Ni 2+ The post-phosphate liquid with a concentration of 62g / L and an iron-phosphorus ratio of 0.98 is pumped from the post-phosphate liquid tank to the multi-stage reaction tank. After the temperature is raised to 50°C by the steam heating coil 2.1.1, 27.5% hydrogen peroxide is added by the dosing controller. After the primary reaction is completed, the ferrous iron concentration in the reaction system is 14g / L.

[0134] Induction reaction: After the primary reaction is completed, the liquid in the multi-stage reaction tank is heated to 75°C by the steam heating coil 2.1.1, and the dosing controller controls the induction agent dosing pump to add CTAB induction agent to promote precipitation. The amount of CTAB added is 2.5wt% of the liquid in the multi-stage reaction tank. After the addition of CTAB, the reaction liquid is kept at 75°C for 2.5h. During the insulation process, the amorphous iron phosphate precipitate is converted into orthorhombic iron phosphate.

[0135] Secondary oxidation: After the reaction is induced, the dosing controller automatically monitors the concentration of ferrous iron in the reaction solution and adds hydrogen peroxide with a concentration of 27.5 for the second time until the concentration of ferrous iron in the reaction solution is 1g / L. The liquid is heated to 100℃ by the heating coil and kept warm for 3.5h.

[0136] Aging, filter pressing, flash evaporation, and rotary kiln calcination: After the liquid in the multi-stage reaction tank is kept at 100°C for 3.5 hours, it enters the insulation aging tank for 8 hours. After the aging and insulation are completed, it enters the filter pressing system, completes the filter pressing and washing, and obtains the filter cake. The filter cake is flash dried and calcined in a rotary kiln at 600°C for 2.5 hours to obtain the finished iron phosphate.

[0137] Comparative Example 1

[0138] This comparative example provides a method for preparing a lithium iron phosphate positive electrode material precursor, comprising the following steps:

[0139] Primary reaction: The difference from Example 1 is that after the primary reaction is completed, the ferrous iron in the reaction system is completely oxidized to ferric iron.

[0140] Induction reaction: After the primary reaction is completed, the liquid in the multi-stage reaction tank is heated to 70°C by the steam heating coil 2.1.1, and the dosing controller controls the induction agent dosing pump to add CTAB induction agent to promote precipitation. The amount of CTAB added is 2wt% of the liquid in the multi-stage reaction tank. After the addition of CTAB, the reaction liquid is kept at 70°C for 3 hours. During the insulation process, the amorphous iron phosphate precipitate is converted into orthorhombic iron phosphate.

[0141] Secondary oxidation: After induction, heat the liquid to 95°C via a heating coil and keep it there for 4 h.

[0142] Aging, filter pressing, flash evaporation, and rotary kiln calcination: After the liquid in the multi-stage reaction tank is kept at 95°C for 4 hours, it enters the insulation aging tank for 9 hours. After the aging and insulation are completed, it enters the filter pressing system, completes the filter pressing and washing, and obtains the filter cake. The filter cake is flash dried and calcined in a rotary kiln at 580°C for 3 hours to obtain the finished iron phosphate.

[0143] Comparative Example 2

[0144] This comparative example provides a method for preparing a lithium iron phosphate positive electrode material precursor, which is different from comparative example 1 only in that the concentration of ferrous iron in the reaction system after the primary reaction is completed is 1.5 g / L.

[0145] Comparative Example 3

[0146] This comparative example provides a method for preparing a lithium iron phosphate positive electrode material precursor, which is different from Example 1 only in that the amount of hydrogen peroxide used in the secondary oxidation step is adjusted so that the ferrous ions in the reaction system are completely converted into trivalent ferrous ions after the secondary oxidation is completed.

[0147] Comparative Example 4

[0148] This comparative example provides a method for preparing a lithium iron phosphate positive electrode material precursor, which is different from Example 1 only in that pH is used to replace the ferrous ion concentration to monitor the reaction system. After the primary reaction is completed, the pH of the reaction system is 0.6, and after the secondary oxidation is completed, the pH of the reaction system is 0.52.

[0149] Comparative Example 5

[0150] This comparative example provides a method for preparing a lithium iron phosphate positive electrode material precursor, which is different from Example 1 only in that the reaction solution after adding CTAB is kept warm at 70° C. for 1 hour.

[0151] The impurity content in the filter cakes obtained in the above embodiments and comparative examples and the lithium iron phosphate positive electrode material precursor was tested, and the results are shown in Table 1.

[0152]

[0153] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a lithium iron phosphate positive electrode material precursor, characterized in that: include: Primary oxidation, reacting the phosphorus-formulated liquid containing ferrous ions and phosphate with a first oxidant to obtain a first ferric phosphate slurry, wherein the ferrous content in the first ferric phosphate slurry is 12-14 g / L, the concentration of ferrous ions in the phosphorus-formulated liquid is greater than 30 g / L, and the iron-phosphorus molar ratio of the phosphorus-formulated liquid is 0.9-1.0; Inducing a reaction, adding an inducer that promotes the formation of FePO4 crystals to the first ferric phosphate slurry to obtain a second ferric phosphate slurry; Secondary oxidation, adding a second oxidant to the second ferric phosphate slurry to react to obtain a third ferric phosphate slurry, wherein the concentration of ferrous ions in the third ferric phosphate slurry is 1 g / L-2 g / L; Calcination: After aging and solid-liquid separation of the third iron phosphate slurry, calcination is performed to obtain a lithium iron phosphate positive electrode material precursor.

2. The method for preparing a lithium iron phosphate cathode material precursor according to claim 1, characterized in that: The iron-phosphorus molar ratio of the phosphorus-matched liquid is 0.96-0.98; Preferably, the concentration of ferrous ions in the phosphorus-matched solution is 40 g / L-70 g / L; Preferably, the temperature of the primary oxidation step is 45°C-55°C; Preferably, the first oxidant is hydrogen peroxide.

3. The method for preparing a lithium iron phosphate cathode material precursor according to claim 1, characterized in that: The inducing agent is hexadecyltrimethylammonium bromide; Preferably, the amount of the inducer is 1.5wt%-2.5wt% of the first ferric phosphate slurry; Preferably, the induction reaction temperature is 65°C-75°C, and the time is 2.5h-3.5h.

4. The method for preparing a lithium iron phosphate positive electrode material precursor according to claim 1, characterized in that: The temperature of the secondary oxidation step is 90°C-100°C and the time is 3.5h-4.5h; Preferably, the second oxidant is hydrogen peroxide.

5. The method for preparing a lithium iron phosphate positive electrode material precursor according to claim 1, characterized in that: The temperature of the aging step is 70°C-95°C and the time is 8h-10h; And / or, the calcination temperature is 550°C-600°C, and the calcination time is 2.5-3.5h.

6. A device applied to the method for preparing a lithium iron phosphate positive electrode material precursor according to any one of claims 1 to 5, characterized in that: include: A post-phosphorus preparation liquid tank (1.2), a multi-stage reaction tank (2.6) and an aging and heat preservation tank (2.7) are sequentially connected in series; the multi-stage reaction tank (2.6) is provided with an inducer dosing pipe and an oxidant dosing pipe for adding a first oxidant and a second oxidant; a dosing control probe (2.3.1) for measuring the concentration of ferrous ions is also provided in the multi-stage reaction tank (2.6); the dosing control probe (2.3.1) is connected to a dosing controller (2.3) capable of controlling the flow rate of liquid in the oxidant dosing pipe via a dosing control signal line (2.3.2).

7. The device according to claim 6, characterized in that include: The aging and heat preservation tank is connected in series via a discharge pipe with a filter press (2.8) for filtering the slurry, a drying device for drying the filter cake obtained by the filtering, and a rotary kiln (2.10) for calcining the dried material.

8. A lithium iron phosphate positive electrode material precursor, characterized in that: The lithium iron phosphate positive electrode material is prepared by the preparation method of the lithium iron phosphate positive electrode material precursor according to any one of claims 1 to 5.

9. A lithium iron phosphate positive electrode material, characterized in that: The lithium iron phosphate positive electrode material precursor according to claim 8 is mixed with a lithium source and then sintered.

10. A lithium ion battery, characterized in that: Including the lithium iron phosphate positive electrode material as described in claim 9.

Citation Information

Patent Citations

  • Production technology for iron phosphate and production device thereof

    CN109761209A

  • Nanometer iron phosphate and preparation method thereof, nanometer lithium iron phosphate positive electrode material and preparation method and application of nanometer lithium iron phosphate positive electrode material

    CN117602603A

  • The preparing method of lithium iron phosphate cathode active materials, the lithium iron phosphate cathod acive materials thereby and the secondary battery using the same

    KR1020150059438A

  • Method for preparing iron phosphate by using phosphorite and ferrous sulfate

    WO2024055467A1

Cited By

  • Method for preparing iron phosphate for battery and application of iron phosphate

    CN119612467A