Method for preparing sodium ferric phosphate sulfate composite positive electrode material by utilizing industrial waste residue ferric sulfate and application of sodium ferric phosphate sulfate composite positive electrode material

By using industrial waste iron sulfate to prepare sodium iron phosphate sulfate composite cathode material with a NASICON structure, the problem of low energy density and high cost of sodium-ion battery materials has been solved, high-capacity and low-cost battery performance improvements have been achieved, and industrial applications have been achieved. High-value reuse of waste materials.

CN118723964APending Publication Date: 2024-10-01KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410969305.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing cathode materials for sodium-ion batteries face problems such as low energy density, high raw material costs, and low electronic conductivity. Lithium-ion batteries have limited lithium resources, which hinders their application in large-scale energy storage systems.

Method used

Industrial waste iron sulfate was used to prepare sodium iron phosphate sulfate composite cathode material with a NASICON structure through a solid-phase method. The electronic conductivity was improved by designing a cross-linked layered structure, and cheap carbon sources were used to reduce costs.

Benefits of technology

A high-capacity, low-cost, simple-to-operate sodium-ion battery cathode material has been achieved, which improves electronic conductivity, enables high-value reuse of industrial waste, and reduces energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118723964A_ABST
    Figure CN118723964A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing a sodium ferric phosphate sulfate composite positive electrode material by utilizing industrial waste residue ferric sulfate and application, and the preparation method comprises the following specific steps: step 1, weighing a certain amount of industrial waste residue ferric sulfate, adding deionized water to fully dissolve, filtering to remove impurities, adding a strong oxidant, and uniformly stirring; after reacting for a certain time, evaporating, concentrating, cooling and crystallizing to obtain impurity-removed ferric sulfate Fe2 (SO4) 3; and 2, weighing sodium dihydrogen phosphate NaH2 (PO4) and the impurity-removed ferric sulfate Fe2 (SO4) 3 according to a molar ratio of 1: 1, dissolving in deionized water, adding a carbon source, stirring by using a magnetic stirrer to form a viscous gel, drying, grinding, carrying out segmented calcination treatment in an inert atmosphere, and cooling to room temperature to obtain the target product sodium ferric phosphate sulfate (NaFe2PO4 (SO4) 2) composite positive electrode material. Wherein the carbon source is calculated according to the mass of the required target product sodium ferric phosphate sulfate positive electrode material. The composite positive electrode material prepared by the preparation method disclosed by the invention has a unique NASICON structure and can realize relatively high capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparing positive electrode materials for sodium ion batteries by utilizing industrial waste, and specifically relates to a method for preparing sodium iron phosphate sulfate composite positive electrode material by utilizing industrial waste slag iron sulfate and application thereof. Background Art

[0002] Environmental pollution and limited fossil energy have promoted the development of renewable clean energy. However, the development of renewable clean energy is affected by intermittent and regional characteristics, and requires large-scale energy storage systems to work together. Electrochemical energy storage technology has the advantages of high energy conversion efficiency and long cycle life, and has great application potential in large-scale energy storage systems. Lithium-ion batteries, as a typical electrochemical energy storage technology, have been commercialized. However, the limited and uneven nature of lithium resources hinders its widespread application in large-scale energy storage systems. Therefore, sodium-ion batteries, which are similar to lithium-ion batteries in working principles and production processes, are one of the most promising next-generation energy storage technologies due to their advantages such as abundant sodium resources, low cost and wide distribution, and are an effective supplement to lithium-ion batteries. Compared with lithium-ion batteries, sodium-ion batteries have certain advantages in low-temperature performance, rate performance, safety performance and cost.

[0003] Sodium ion battery positive electrode materials are the key components of sodium ion batteries and have a vital impact on the performance of the battery. There are three main technical routes for sodium ion battery positive electrode materials, namely layered oxides, Prussian blue compounds and polyanion compounds. Among them, polyanion compounds have attracted widespread attention due to their advantages such as high cycle life, high theoretical working voltage and good structural stability. The polyanion positive electrode materials currently under research include: sodium vanadium phosphate, sodium iron pyrophosphate, sodium ferrous sulfate, etc. However, the main problems they face are low energy density, high raw material cost and low electronic conductivity. The low cost and wide availability of sodium have prompted people to explore Na with a NASICON framework structure. + Insert the cathode. In 2016, Goodenough et al. first reported a sodium iron sulfate phosphate positive electrode material with a NASICON framework structure. This unique material is simple to synthesize, low-cost, and can achieve a high capacity, which has attracted widespread attention. my country mainly produces titanium dioxide by sulfuric acid method. For every 1t of titanium dioxide produced, 3.5-4.0t of ferrous sulfate heptahydrate can be obtained as a by-product. At present, ferrous sulfate heptahydrate can be effectively used to produce polyferric sulfate. There is a large amount of ferric sulfate waste residue in its production process. Ferrous sulfate is one of the raw materials for the production of sodium iron sulfate phosphate. The use of waste ferric sulfate as a raw material for the production of sodium iron sulfate phosphate positive electrode materials will realize the organic combination of industrial solid waste and new energy. At present, there are no patents or literature on the use of waste ferric sulfate to produce sodium iron sulfate phosphate. Summary of the invention

[0004] The purpose of the present invention is to prepare sodium iron phosphate sulfate composite positive electrode material using industrial waste slag iron sulfate to achieve high-value reuse of industrial waste. A sodium ion battery positive electrode material with a unique NASICON structure is prepared by a solid phase method with simple operation, low cost and low energy consumption. A low-cost carbon source is used to design a cross-linked hierarchical structure, which effectively improves the electronic conductivity of the sodium iron phosphate sulfate positive electrode material.

[0005] The first aspect of the present invention provides a method for preparing sodium iron phosphate sulfate composite positive electrode material from industrial waste slag iron sulfate, comprising the following steps:

[0006] Step 1: Weigh a certain amount of industrial waste slag ferric sulfate, add deionized water to fully dissolve it, filter and remove impurities, add a certain amount of strong oxidant, react for a certain period of time, evaporate and concentrate, cool and crystallize, and obtain the impurity-free ferric sulfate Fe2(SO4)3; wherein the reaction time is 20min-30min, so that all the divalent iron ions are oxidized to trivalent iron ions.

[0007] Step 2: Weigh sodium dihydrogen phosphate NaH2(PO4) and the impurity-removed iron sulfate Fe2(SO4)3 in a molar ratio of 1:1 and dissolve them in deionized water, add a carbon source, use a magnetic stirrer to stir until it becomes a viscous gel, and after drying and grinding in a forced air drying oven, use a staged calcination treatment under an inert atmosphere, first calcining at a constant temperature of 200-300°C for 4h, then heating to 500°C for constant temperature calcination for 8-12h, and then cooling to room temperature to obtain the target product, sodium ferric phosphate sulfate (NaFe2PO4(SO4)2) composite positive electrode material; wherein the carbon source is calculated based on the mass of the required target product, sodium ferric phosphate sulfate positive electrode material.

[0008] In one embodiment, in step one, the iron sulfate after impurities removal also contains magnesium, titanium, manganese, and aluminum impurities, which can be doped as heterogeneous heteroatoms inside the lattice of the sodium ferric phosphate sulfate positive electrode material to further improve the electrochemical properties of the material, specifically including 95% to 98% iron sulfate, 0.6% to 1.6% magnesium, 0.7% to 1.2% titanium, 0.4% to 0.8% manganese, and 0.3% to 1.4% aluminum.

[0009] In one embodiment, in step 1, the strong oxidant is at least one of NaCIO3, H2O2, HNO3, and KClO3, and the added amount is 0.5% to 10% of the mass of the industrial waste slag ferric sulfate.

[0010] In one embodiment, in step 2, the carbon source is at least one of ascorbic acid, glucose, starch, citric acid, graphene, graphite, polyethylene glycol, and cyclodextrin, and the mass of the carbon source is 5% to 25% of the mass of the desired target product, sodium ferric phosphate sulfate positive electrode material.

[0011] In one embodiment, in step 2, the rotation speed of the magnetic stirrer is 300-500 rpm, and the temperature of the magnetic stirrer is 80-120°C.

[0012] In one embodiment, in step 2, the sintering treatment adopts a staged calcination treatment, firstly heating the temperature to 200-300°C at a heating rate of 1-5°C / min, calcining at this temperature for 4 hours, then heating the temperature to 500°C at a heating rate of 1-5°C / min and calcining at this temperature for 8-12 hours.

[0013] In one embodiment, in step 2, the inert gas is one of argon, nitrogen, and argon-hydrogen mixed gas.

[0014] In a second aspect, the present invention further provides a method for manufacturing a sodium iron phosphate sulfate composite electrode sheet, comprising:

[0015] Step 1: Mix the positive electrode active material, conductive carbon black and polyvinylidene fluoride in a mass ratio of 8:1:1, dissolve in a dispersant N-methylpyrrolidone after mixing, and grind for 20 to 30 minutes to obtain a slurry; wherein the positive electrode active material is an iron phosphate sulfate composite positive electrode material obtained by the preparation method of the sodium iron phosphate sulfate composite positive electrode material as described above;

[0016] Step 2: uniformly coating the slurry on the positive electrode current collector by a coating machine, wherein the positive electrode current collector is aluminum foil, and the coating thickness of the slurry is 50 to 200 μm; placing the aluminum foil carrying the slurry in a vacuum drying oven and drying it at 50 to 120° C. for 6 to 24 hours to obtain a sodium iron phosphate sulfate composite electrode sheet.

[0017] In a third aspect, the present invention also provides a composite sodium ion battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode and the negative electrode are located on both sides of the separator, and the electrolyte is located between the positive electrode and the negative electrode. The positive electrode is a sodium iron phosphate sulfate composite electrode sheet prepared by the manufacturing method of the sodium iron phosphate sulfate composite electrode sheet described above, and the sodium iron phosphate sulfate composite electrode sheet is a round sheet with a diameter of 14 mm; the negative electrode is a sodium metal sheet, wherein the diameter of the sodium metal sheet is 16 mm and the thickness is 0.2 to 0.4 mm; the electrolyte is 0.1 mL of a sodium perchlorate / ethylene carbonate / propylene carbonate / fluoroethylene carbonate solution with a concentration of 1 mol / L; and the separator is glass wool with a diameter of 19 mm.

[0018] Beneficial effects of the present invention:

[0019] (1) A sodium iron phosphate sulfate composite cathode material with a unique NASICON structure was synthesized by a solid-phase method, providing a process-controllable method with a short synthesis cycle and simple operation.

[0020] (2) The present invention uses carbon materials and positive electrode materials to realize the design of cross-linked layered structure in situ. The added carbon source provides a beneficial conductive network, which can effectively improve the electronic conductivity of the material, thereby improving the capacity of the material.

[0021] (3) The method for preparing sodium iron phosphate sulfate composite positive electrode material from industrial waste slag iron sulfate proposed in the present invention is simple to operate and has mild conditions. The raw materials used are cheap sodium source and carbon source, and the iron source is industrial waste slag, which reduces costs and realizes high-value reuse of industrial waste.

[0022] (4) The sodium iron phosphate sulfate NaFe2PO4(SO4)2 / C composite positive electrode material provided by the technical solution of the present invention achieves an operating voltage of more than 3V and has a relatively high capacity. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 It is a schematic flow chart of a method for preparing a composite positive electrode material for a sodium ion battery from industrial waste ferric sulfate provided in an embodiment of the present invention.

[0025] Figure 2 It is a schematic diagram of the manufacturing process of sodium iron phosphate sulfate composite electrode sheet.

[0026] Figure 3 This is the X-ray diffraction (XRD) pattern of the sodium iron phosphate sulfate NaFe2PO4(SO4)2 material prepared in Comparative Example 1.

[0027] Figure 4 This is a cycle performance diagram of the sodium ion battery prepared in Comparative Example 1 at a C / 5 rate.

[0028] Figure 5 This is a scanning electron microscope (SEM) image of the sodium iron phosphate sulfate NaFe2PO4(SO4)2 material prepared in Comparative Example 1.

[0029] Figure 6 This is a rate performance diagram of the composite sodium ion battery prepared in Example 1.

[0030] Figure 7 This is a cycle performance diagram of the composite sodium ion battery prepared in Example 2 at a C / 2 rate.

[0031] Figure 8 This is a cycle performance diagram of the composite sodium ion battery prepared in Example 3 at a C / 5 rate.

[0032] Fig. 9 This is a cycle performance diagram of the composite sodium ion battery prepared in Example 4 at a C / 5 rate.

[0033] Fig.10 This is a cycle performance diagram of the composite sodium ion battery prepared in Example 5 at a C / 5 rate. DETAILED DESCRIPTION

[0034] Hereinafter, the method for preparing sodium ferric phosphate sulfate composite positive electrode material from industrial waste slag ferric sulfate and its application will be described in detail in conjunction with exemplary embodiments.

[0035] See also Figure 1 , Figure 1 The present invention provides a method for preparing a sodium ferric phosphate sulfate composite positive electrode material from industrial waste ferric sulfate, and the steps are as follows:

[0036] S1: Weigh a certain amount of industrial waste slag ferric sulfate, add deionized water to fully dissolve it, filter and remove impurities, add a certain amount of strong oxidant, react for a certain period of time, evaporate and concentrate, cool and crystallize, and obtain the impurity-free ferric sulfate Fe2(SO4)3; wherein the reaction time is 20min-30min, so that all the divalent iron ions are oxidized to trivalent iron ions.

[0037] S2: Sodium dihydrogen phosphate NaH2(PO4) and the impurity-removed iron sulfate Fe2(SO4)3 are weighed in a molar ratio of 1:1 and dissolved in deionized water, a carbon source is added, and stirred with a magnetic stirrer until it becomes a viscous gel. After drying and grinding in a forced air drying oven, a staged calcination treatment is performed under an inert atmosphere, first calcined at a constant temperature of 200-300°C for 4 hours, then heated to 500°C for constant temperature calcination for 8-12 hours, and then cooled to room temperature to obtain the target product, sodium ferric phosphate sulfate (NaFe2PO4(SO4)2) composite positive electrode material; wherein the carbon source is calculated based on the mass of the desired target product, sodium ferric phosphate sulfate positive electrode material.

[0038] Specifically, in step S1, the iron sulfate after impurities removal also contains magnesium, titanium, manganese, and aluminum impurities, which can be doped as heterogeneous heteroatoms inside the lattice of the sodium ferric phosphate sulfate positive electrode material to further improve the electrochemical properties of the material, specifically including 95% to 98% iron sulfate, 0.6% to 1.6% magnesium, 0.7% to 1.2% titanium, 0.4% to 0.8% manganese, and 0.3% to 1.4% aluminum.

[0039] The strong oxidant is at least one of NaCIO3, H2O2, HNO3, and KClO3, and the added amount is 0.5% to 10% of the mass of the industrial waste slag ferric sulfate. The added amount can be 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10% of the mass of the industrial waste slag ferric sulfate, or other values ​​within the above range.

[0040] In step S2, the rotation speed of the magnetic stirrer is 300-500 rpm, specifically 300 rpm, 350 rpm, 400 rpm, 450 rpm, 500 rpm, or other values ​​within the above range; the temperature of the magnetic stirrer is 80-120°C, specifically 80°C, 90°C, 100°C, 110°C, 120°C, or other values ​​within the above range.

[0041] In step S2, the inert gas is one of argon, nitrogen, and argon-hydrogen mixed gas.

[0042] In step S2, the carbon source is at least one of ascorbic acid, glucose, starch, citric acid, graphene, graphite, polyethylene glycol, and cyclodextrin, and the mass of the carbon source is 5% to 25% of the mass of the target product, sodium ferric phosphate sulfate positive electrode material, specifically 5%, 10%, 15%, 20%, 25%, or other percentages within the above range.

[0043] The sintering treatment in step S2 adopts a staged calcination treatment, firstly heating the temperature to 200-300°C at a heating rate of 1-5°C / min, and calcining at this temperature for 4-8h; then heating the temperature to 500°C at a heating rate of 1-5°C / min and calcining at this temperature for 8-12h.

[0044] That is, in the first stage, the temperature is first raised to 200-300°C at a heating rate of 1-5°C / min for constant temperature calcination for 4-8h, and in the second stage, the temperature is raised to 500°C at a heating rate of 1-5°C / min for constant temperature calcination for 8-12h. Among them, the heating rate in the first stage can be 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, or other heating rates within the above range; the temperature raised in the first stage can be 200°C, 220°C, 240°C, 260°C, 280°C, 300°C, or other temperature values ​​within the above temperature range. The heating rate in the second stage can be 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, or other heating rates within the above range; the constant temperature calcination time in the second stage is 8-12h, that is, it can be 8h, 9h, 10h, 11h, 12h, or other time values ​​within the above range.

[0045] See also Figure 2 , Figure 2 The present invention is a schematic flow chart of a method for manufacturing a sodium iron phosphate sulfate composite electrode sheet provided by an embodiment of the present invention. Based on the sodium iron phosphate sulfate-sodium ion battery positive electrode material obtained in this embodiment, the present invention also provides a method for manufacturing a sodium iron phosphate sulfate composite electrode sheet, and the specific steps include:

[0046] S10: adding a positive electrode active material, conductive carbon black, and polyvinylidene fluoride in a mass ratio of 8:1:1, dissolving the mixed materials in a dispersant N-methylpyrrolidone, and grinding for 20 to 30 minutes to obtain a slurry; wherein the positive electrode active material adopts the sodium iron phosphate sulfate positive electrode material obtained by the preparation method of this embodiment;

[0047] S20: The slurry is uniformly coated on the positive electrode current collector by a coating machine, wherein the positive electrode current collector is an aluminum foil, and the coating thickness of the slurry is 50-200 μm; the aluminum foil carrying the slurry is placed in a vacuum drying oven and dried at 50-120°C for 6-24 hours to obtain a sodium iron phosphate sulfate composite electrode sheet. It can be understood that in a specific embodiment, the coating thickness of the slurry can be 50 μm, 100 μm, 150 μm, 200 μm, or other values ​​within the above range. The temperature in the vacuum drying oven can be 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, or other temperature values ​​within the above range; the drying time can be 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h, 24h, or other time values ​​within the above drying time range.

[0048] On the basis of the foregoing, this embodiment also provides a composite sodium ion battery, comprising a positive electrode, a negative electrode, a diaphragm and an electrolyte, wherein the positive electrode and the negative electrode are located on both sides of the diaphragm, and the electrolyte is located between the positive electrode and the negative electrode. The positive electrode is a sodium iron phosphate sulfate composite electrode sheet prepared by the manufacturing method of the sodium iron phosphate sulfate composite electrode sheet described above, and the sodium iron phosphate sulfate composite electrode sheet is a round sheet with a diameter of 14 mm; the negative electrode is a sodium metal sheet, wherein the diameter of the sodium metal sheet is 16 mm and the thickness is 0.2 to 0.4 mm; the electrolyte is 0.1 mL of a sodium perchlorate / ethylene carbonate / propylene carbonate / fluoroethylene carbonate solution with a concentration of 1 mol / L; and the diaphragm is glass wool with a diameter of 19 mm.

[0049] The sodium iron phosphate sulfate-sodium ion battery positive electrode material prepared according to the preparation method of this embodiment is applied to electrode sheets and sodium ion batteries, so that the sodium iron phosphate sulfate composite electrode sheet prepared by the above preparation method also has the advantages of sodium iron phosphate-sodium ion battery positive electrode material.

[0050] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with specific examples, but the content of the present invention is not limited to the following examples.

[0051] Comparative Example 1

[0052] The method for preparing the uncarbon-modified sodium iron phosphate sulfate NaFe2PO4(SO4)2 positive electrode material comprises the following steps:

[0053] Step 1: Weigh a certain amount of ferric sulfate waste residue, add a certain amount of deionized water to fully dissolve it, filter and remove impurities, then add an appropriate amount of strong oxidant to the solution, react for 30 minutes to oxidize all the divalent iron into trivalent iron, then evaporate and concentrate the solution, cool and crystallize to obtain ferric sulfate Fe2(SO4)3.

[0054] Step 2: Weigh sodium dihydrogen phosphate NaH2(PO4) and impurity-removed industrial waste slag Fe2(SO4)3 in a molar ratio of 1:1 and dissolve them in 80 ml of deionized water, and use a magnetic stirrer to put the above substances into a beaker and mix them. Set the magnetic stirrer to 80-120°C and 300-500rmp, stir until the solution is a viscous gel, dry and grind in a forced air drying oven, and calcine at a constant temperature of 200-300°C for 4 hours under an inert atmosphere, then heat to 500°C and calcine at a constant temperature for 8-12 hours, and cool to room temperature to obtain sodium iron phosphate sulfate (NaFe2PO4(SO4)2) positive electrode material.

[0055] The waste residue obtained after the industrial waste slag ferric sulfate described in this comparative example is dissolved in water, filtered, impurity removed, oxidized, evaporated, crystallized and dried, includes 95% to 98% ferric sulfate, 0.6% to 1.6% magnesium, 0.7% to 1.2% titanium, 0.4% to 0.8% manganese, and 0.3% to 1.4% aluminum in terms of mass percentage. These impurities can be doped as heterogeneous heteroatoms inside the lattice of the sodium ferric phosphate sulfate positive electrode material to further improve the electrochemical properties of the material.

[0056] The prepared sodium iron phosphate sulfate-sodium ion battery positive electrode material is used to prepare the positive electrode sheet. The positive electrode sheet is made of the slurry coated on the aluminum foil and dried at 120°C in vacuum and then cut into pieces. The slurry is made by mixing the positive electrode material with conductive carbon black and polyvinylidene fluoride in a mass ratio of 8:1:1, and then adding N-methylpyrrolidone dispersant. 1MNaClO4 dissolved in ethylene carbonate (EC) / propylene carbonate (PC) / fluoroethylene carbonate (FEC) is used as the electrolyte, the outer shell is made of stainless steel, the negative electrode is made of metal sodium sheet, and the positive electrode and the negative electrode are separated by a glass fiber diaphragm to assemble into a traditional button battery. The material test and electrochemical performance diagram are shown in the figure:

[0057] Figure 3 This is the X-ray diffraction (XRD) pattern of the sodium iron phosphate sulfate (NaFe2PO4(SO4)2) material prepared in Comparative Example 1. It can match the standard X-ray diffraction standard card of NaFe2PO4(SO4)2, that is, NaFe2PO4(SO4)2 is synthesized.

[0058] Figure 4 This is a cycle performance diagram of a sodium ion battery prepared using NaFe2PO4(SO4)2 prepared in Example 1 as the positive electrode material within a voltage range of 2.0 to 4.4 V and at a rate of C / 5. The first discharge capacity can achieve 70.2 mAh / g, the coulombic efficiency reaches 90%, and the discharge specific capacity can still reach 60 mAh / g after 90 cycles.

[0059] Figure 5 This is a scanning electron microscope (SEM) image of the sodium iron phosphate sulfate positive electrode material prepared in Comparative Example 1. It can be seen that the sodium iron phosphate sulfate has a layered structure.

[0060] Example 1

[0061] The method for preparing the sodium iron phosphate sulfate NaFe2PO4(SO4)2 / C composite positive electrode material provided in the embodiment of the present invention comprises the following steps:

[0062] Step 1: Weigh a certain amount of ferric sulfate waste residue, add a certain amount of deionized water to fully dissolve it, filter and remove impurities, add an appropriate amount of strong oxidant to the solution, react for 30 minutes to oxidize all the divalent iron into trivalent iron, then evaporate and concentrate the solution, cool and crystallize to obtain ferric sulfate (Fe2(SO4)3).

[0063] Step 2: Weigh NaH2(PO4) and the impurity-removed industrial waste slag Fe2(SO4)3 in a molar ratio of 1:1 and fully dissolve them in deionized water, add citric acid accounting for 5% of the mass of the target product sodium ferric phosphate sulfate, set the magnetic stirrer to 80-120°C and 300-500rmp, stir until the solution is a viscous gel, dry and grind in a forced air drying oven, calcine at a constant temperature of 200-300°C for 4h under an inert atmosphere, then heat to 500°C for constant temperature calcination for 8-12h, cool to room temperature, and obtain sodium ferric phosphate sulfate (NaFe2PO4(SO4)2) positive electrode material.

[0064] The waste residue obtained after the industrial waste slag ferric sulfate described in this embodiment is dissolved in water, filtered, impurity removed, oxidized, evaporated, crystallized and dried, includes 95% to 98% ferric sulfate, 0.6% to 1.6% magnesium, 0.7% to 1.2% titanium, 0.4% to 0.8% manganese, and 0.3% to 1.4% aluminum in terms of mass percentage. These impurities can be doped as heterogeneous heteroatoms inside the lattice of the sodium ferric phosphate sulfate positive electrode material to further improve the electrochemical properties of the material.

[0065] The NaFe2PO4(SO4)2 sodium ion battery composite positive electrode material prepared in this embodiment is used to prepare a positive electrode sheet, which is made by cutting a slurry coated on an aluminum foil and drying it at 120°C in vacuum. The slurry is made by mixing the positive electrode material with conductive carbon black and polyvinylidene fluoride in a mass ratio of 8:1:1, and then adding N-methylpyrrolidone dispersant. 1M NaClO4 is dissolved in ethylene carbonate (EC) / propylene carbonate (PC) / fluoroethylene carbonate (FEC) as the electrolyte, a stainless steel shell is used for the outer shell, a metal sodium sheet is used for the negative electrode, and a glass fiber separator is used to separate the positive electrode from the negative electrode to assemble into a composite button battery.

[0066] like Figure 6 As shown in the figure, the rate performance of the battery in the voltage range of 2.0 to 4.4 V, the first discharge capacity at C / 5 rate is about 72 mAh / g, and the first discharge capacity at 1C rate is about 61 mAh / g. Compared with comparative example 1, the discharge capacity of the material has been improved very little. The rate performance of the material is also relatively poor, which may be due to the presence of impurities in the positive electrode material.

[0067] Example 2

[0068] The method for preparing the sodium iron phosphate sulfate NaFe2PO4(SO4)2 / C composite positive electrode material provided in the embodiment of the present invention comprises the following steps:

[0069] Step 1: Weigh a certain amount of ferric sulfate waste residue, add a certain amount of deionized water to fully dissolve it, filter and remove impurities, add an appropriate amount of strong oxidant to the solution, react for 30 minutes to oxidize all the divalent iron into trivalent iron, then evaporate and concentrate the solution, cool and crystallize to obtain ferric sulfate (Fe2(SO4)3).

[0070] Step 2: Weigh NaH2(PO4) and the impurity-removed industrial waste slag Fe2(SO4)3 in a molar ratio of 1:1 and dissolve them in 80 ml of deionized water, add citric acid accounting for 10% of the mass of the target product sodium ferric phosphate sulfate, set the magnetic stirrer to 80-120°C and 300-500rmp, stir until the solution is a viscous gel, dry and grind in a forced air drying oven, calcine at a constant temperature of 200-300°C for 4h under an inert atmosphere, then raise the temperature to 500°C for constant temperature calcination for 8-12h, cool to room temperature, and obtain sodium ferric phosphate sulfate (NaFe2PO4(SO4)2) positive electrode material.

[0071] The waste residue obtained after the industrial waste slag ferric sulfate described in this embodiment is dissolved in water, filtered, impurity removed, oxidized, evaporated, crystallized and dried, includes 95% to 98% ferric sulfate, 0.6% to 1.6% magnesium, 0.7% to 1.2% titanium, 0.4% to 0.8% manganese, and 0.3% to 1.4% aluminum in terms of mass percentage. These impurities can be doped as heterogeneous heteroatoms inside the lattice of the sodium ferric phosphate sulfate positive electrode material to further improve the electrochemical properties of the material.

[0072] The NaFe2PO4(SO4)2 sodium ion battery composite positive electrode material prepared in this embodiment is used to prepare a positive electrode sheet. The positive electrode sheet is made by cutting a slurry coated on an aluminum foil and drying it at 120°C in vacuum. The slurry is made by mixing the positive electrode material with conductive carbon black and polyvinylidene fluoride in a mass ratio of 8:1:1, and then adding N-methylpyrrolidone dispersant. 1M NaClO4 is dissolved in ethylene carbonate (EC) / propylene carbonate (PC) / fluoroethylene carbonate (FEC) as the electrolyte, the outer shell is made of stainless steel, the negative electrode is made of metal sodium sheet, and the positive electrode is separated from the negative electrode by a glass fiber separator to assemble into a composite button battery.

[0073] like Figure 7As shown in the figure, the battery has a voltage range of 2.0 to 4.4 V and a cycle performance at a rate of 0.5 C. It can be seen that the initial discharge capacity can reach 65.8 mAh / g. After 100 cycles, the discharge capacity is still 57 mAh / g. It can be seen that compared with Comparative Example 1, the addition of carbon source increases the discharge capacity of the material, and greatly improves the capacity and cycle stability of the sodium ion battery.

[0074] Example 3

[0075] The method for preparing the sodium iron phosphate sulfate NaFe2PO4(SO4)2 / C composite positive electrode material provided in the embodiment of the present invention comprises the following steps:

[0076] Step 1: Weigh a certain amount of ferric sulfate waste residue, add a certain amount of deionized water to fully dissolve it, filter and discard the insoluble matter, remove impurities, add an appropriate amount of strong oxidant to the solution, react for 30 minutes, so that the divalent iron is completely oxidized into trivalent iron, then evaporate and concentrate the solution, cool and crystallize to obtain ferric sulfate (Fe2(SO4)3).

[0077] Step 2: Weigh NaH2(PO4) and the impurity-removed industrial waste slag Fe2(SO4)3 in a molar ratio of 1:1 and dissolve them in 80 ml of deionized water, add citric acid accounting for 15% of the mass of the target product sodium iron phosphate sulfate, set the magnetic stirrer to 80-120°C and 300-500rmp, stir until the solution is a viscous gel, dry and grind in a forced air drying oven, calcine at a constant temperature of 200-300°C for 4h under an inert atmosphere, then heat to 500°C for constant temperature calcination for 8-12h, cool to room temperature, and obtain iron phosphate sulfate (NaFe2PO4(SO4)2) positive electrode material.

[0078] The waste residue obtained after the industrial waste slag ferric sulfate described in this embodiment is dissolved in water, filtered, impurity removed, oxidized, evaporated, crystallized and dried, includes 95% to 98% ferric sulfate, 0.6% to 1.6% magnesium, 0.7% to 1.2% titanium, 0.4% to 0.8% manganese, and 0.3% to 1.4% aluminum in terms of mass percentage. These impurities can be doped as heterogeneous heteroatoms inside the lattice of the sodium ferric phosphate sulfate positive electrode material to further improve the electrochemical properties of the material.

[0079] The NaFe2PO4(SO4)2 sodium ion battery composite positive electrode material prepared in this embodiment is used to prepare a positive electrode sheet. The positive electrode sheet is made by drying the slurry coated on aluminum foil at 120°C in vacuum and cutting the slurry. The slurry is made by mixing the positive electrode material with conductive carbon black and polyvinylidene fluoride in a mass ratio of 8:1:1, and then adding N-methylpyrrolidone dispersant. 1M NaClO4 is dissolved in ethylene carbonate (EC) / propylene carbonate (PC) / fluoroethylene carbonate (FEC) as the electrolyte, the outer shell is made of stainless steel, the negative electrode is made of metal sodium sheet, and the positive electrode is separated from the negative electrode by a glass fiber separator to assemble into a composite button battery.

[0080] like Figure 8 As shown in the figure, the first discharge capacity of the battery is about 75.6 mAh / g at C / 5 rate in the voltage range of 2.0 to 4.4 V. Thanks to the addition of carbon source, the discharge specific capacity of the material is significantly improved.

[0081] Example 4

[0082] The method for preparing the sodium iron phosphate sulfate NaFe2PO4(SO4)2 / C composite positive electrode material provided in the embodiment of the present invention comprises the following steps:

[0083] Step 1: Weigh a certain amount of ferric sulfate waste residue, add a certain amount of deionized water to fully dissolve it, filter and remove impurities, add an appropriate amount of strong oxidant to the solution, react for 30 minutes to oxidize all the divalent iron into trivalent iron, then evaporate and concentrate the solution, cool and crystallize to obtain ferric sulfate (Fe2(SO4)3).

[0084] Step 2: Weigh NaH2(PO4) and the impurity-removed industrial waste slag Fe2(SO4)3 in a molar ratio of 1:1 and dissolve them in 80 ml of deionized water, add citric acid accounting for 20% of the mass of the target product sodium ferric phosphate sulfate, set the magnetic stirrer to 80-120°C and 300-500rmp, stir until the solution is a viscous gel, dry and grind in a forced air drying oven, calcine at a constant temperature of 200-300°C for 4h under an inert atmosphere, then heat to 500°C for constant temperature calcination for 8-12h, cool to room temperature, and obtain sodium ferric phosphate sulfate (NaFe2PO4(SO4)2) positive electrode material.

[0085] The waste residue obtained after the industrial waste slag ferric sulfate described in this embodiment is dissolved in water, filtered, impurity removed, oxidized, evaporated, crystallized and dried, includes 95% to 98% ferric sulfate, 0.6% to 1.6% magnesium, 0.7% to 1.2% titanium, 0.4% to 0.8% manganese, and 0.3% to 1.4% aluminum in terms of mass percentage. These impurities can be doped as heterogeneous heteroatoms inside the lattice of the sodium ferric phosphate sulfate positive electrode material to further improve the electrochemical properties of the material.

[0086] The NaFe2PO4(SO4)2 sodium ion battery composite positive electrode material prepared in this embodiment is used to prepare a positive electrode sheet. The positive electrode sheet is made by cutting a slurry coated on an aluminum foil and drying it at 120°C in vacuum. The slurry is made by mixing the positive electrode material with conductive carbon black and polyvinylidene fluoride in a mass ratio of 8:1:1, and then adding N-methylpyrrolidone dispersant. 1M NaClO4 is dissolved in ethylene carbonate (EC) / propylene carbonate (PC) / fluoroethylene carbonate (FEC) as the electrolyte, the outer shell is made of stainless steel, the negative electrode is made of metal sodium sheet, and the positive electrode is separated from the negative electrode by a glass fiber separator to assemble into a composite button battery.

[0087] like Fig. 9 As shown in the figure, the first discharge capacity of the battery under C / 5 rate conditions in the voltage range of 2.0-4.4V is about 76.8mAh / g. After 100 cycles, the capacity of the material is still about 60mAh / g, indicating that the addition of carbon source effectively improves the electronic conductivity and cycle stability of the material. Compared with comparative example 1, the discharge specific capacity of the material is significantly increased. Therefore, adding the appropriate amount of carbon is crucial to improving the performance of the material.

[0088] Example 5

[0089] The preparation method of the sodium iron phosphate sulfate NaFe2PO4(SO4)2 / C composite positive electrode material and the steps of assembling button batteries provided in the embodiment of the present invention, adding citric acid accounting for 25% of the mass of the target product sodium iron phosphate sulfate, include the following steps as in Example 4:

[0090] like Fig.10 As shown, the first discharge capacity of the battery under C / 5 rate conditions in the voltage range of 2.0 to 4.4 V is about 70.2 mAh / g, indicating that adding excessive carbon does not improve the performance of the material. Therefore, adding the right amount of carbon is crucial to improving the performance of the material.

[0091] Although the present invention has been described above in conjunction with the exemplary embodiments and the accompanying drawings, it should be apparent to those skilled in the art that various modifications may be made to the above-described embodiments without departing from the spirit and scope of the claims.

Claims

1. A method for preparing sodium iron phosphate sulfate composite positive electrode material using industrial waste slag iron sulfate, comprising the following steps: Step 1: Weigh a certain amount of industrial waste slag iron sulfate, add deionized water to fully dissolve, filter and remove impurities, add a certain amount of strong oxidant, react for a certain period of time, evaporate and concentrate, cool and crystallize, and obtain iron sulfate Fe2(SO4)3 after impurities are removed; Step 2: Weigh sodium dihydrogen phosphate NaH2(PO4) and the impurity-removed iron sulfate Fe2(SO4)3 in a molar ratio of 1:1 and dissolve them in deionized water, add a carbon source, use a magnetic stirrer to stir until it becomes a viscous gel, and after drying and grinding in a forced air drying oven, use a staged calcination treatment under an inert atmosphere, first calcining at a constant temperature of 200-300°C for 4h, then heating to 500°C for constant temperature calcination for 8-12h, and cooling to room temperature to obtain the target product, sodium iron phosphate sulfate (NaFe2PO4(SO4)2) composite positive electrode material; wherein the carbon source is calculated based on the mass of the required target product, sodium iron phosphate sulfate positive electrode material.

2. The method for preparing sodium iron phosphate sulfate composite positive electrode material using industrial waste slag iron sulfate according to claim 1, characterized in that: Step 1: The iron sulfate after impurities removal includes 95% to 98% iron sulfate, 0.6% to 1.6% magnesium, 0.7% to 1.2% titanium, 0.4% to 0.8% manganese, and 0.3% to 1.4% aluminum.

3. The method for preparing sodium iron phosphate sulfate composite positive electrode material using industrial waste slag iron sulfate according to claim 1, characterized in that: In step 1, the strong oxidant is at least one of NaCIO3, H2O2, HNO3, and KClO3; the amount of the strong oxidant added is 0.5% to 10% of the mass of the industrial waste slag ferric sulfate.

4. The method for preparing sodium iron phosphate sulfate composite positive electrode material using industrial waste slag iron sulfate according to claim 1, characterized in that: Step 2: The carbon source is at least one of ascorbic acid, glucose, starch, citric acid, graphene, graphite, polyethylene glycol, and cyclodextrin; in terms of mass percentage, the mass of the carbon source is 5% to 25% of the mass of the desired target product, sodium ferric phosphate sulfate positive electrode material.

5. The method for preparing sodium iron phosphate sulfate composite positive electrode material using industrial waste slag iron sulfate as claimed in claim 1, characterized in that: In step 2, the rotation speed of the magnetic stirrer is 300-500 rpm, and the temperature of the magnetic stirrer is 80-120°C.

6. The method for preparing sodium iron phosphate sulfate composite positive electrode material using industrial waste slag iron sulfate as claimed in claim 1, characterized in that: In the step 2, the staged calcination treatment is firstly to increase the temperature to 200-300°C at a heating rate of 1-5°C / min and calcine at a constant temperature for 4 hours; then to increase the temperature to 500°C at a heating rate of 1-5°C / min and calcine at a constant temperature for 8-12 hours.

7. The method for preparing sodium iron phosphate sulfate composite positive electrode material using industrial waste slag iron sulfate according to claim 1, characterized in that: In step 2, the inert gas is one of argon, nitrogen, and argon-hydrogen mixed gas.

8. A sodium iron phosphate sulfate composite positive electrode material prepared using industrial waste slag iron sulfate, characterized in that: The sodium iron phosphate sulfate composite positive electrode material prepared using industrial waste slag iron sulfate is prepared using the preparation method for the sodium iron phosphate sulfate composite positive electrode material using industrial waste slag iron sulfate as claimed in any one of claims 1 to 7.

9. A method for manufacturing a sodium iron phosphate sulfate composite positive electrode sheet, characterized in that: include Step 1: Mix the positive electrode active material, conductive carbon black, and polyvinylidene fluoride in a mass ratio of 8:1:1, dissolve in a dispersant N-methylpyrrolidone after mixing, and grind for 20 to 30 minutes to obtain a slurry; wherein the positive electrode material is a sodium iron phosphate sulfate-sodium ion battery positive electrode material obtained by the preparation method of the sodium iron phosphate sulfate composite positive electrode material prepared by the industrial waste iron sulfate as claimed in any one of claims 1 to 7, or a sodium iron phosphate sulfate composite positive electrode material prepared by using the industrial waste iron sulfate as claimed in claim 8; Step 2: uniformly coating the slurry on the positive electrode current collector by a coating machine, wherein the positive electrode current collector is aluminum foil, and the coating thickness of the slurry is 50 to 200 μm; placing the aluminum foil carrying the slurry in a vacuum drying oven and drying it at 50 to 120° C. for 6 to 24 hours to obtain a sodium iron phosphate sulfate composite electrode sheet.

10. A composite sodium ion battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode and the negative electrode are located on both sides of the separator, and the electrolyte is located between the positive electrode and the negative electrode, characterized in that: The positive electrode is a sodium iron phosphate sulfate composite electrode sheet prepared by the manufacturing method of the sodium iron phosphate sulfate composite electrode sheet as claimed in claim 9, and the sodium iron phosphate sulfate composite electrode sheet is a round sheet with a diameter of 14 mm; the negative electrode is a sodium metal sheet, wherein the diameter of the sodium metal sheet is 16 mm and the thickness is 0.2-0.4 mm; the electrolyte is 0.1 mL of a sodium perchlorate / ethylene carbonate / propylene carbonate / fluoroethylene carbonate solution with a concentration of 1 mol / L; and the diaphragm is glass wool with a diameter of 19 mm.

Citation Information

Cited By

  • Multi-metal element in-situ doped sodium ferric sulfate positive electrode material prepared from byproduct sulfate, method thereof and sodium ion battery

    CN119219066A

  • Method for preparing multi-element uniformly-doped sodium ferric sulfate porous sodium battery positive electrode material by using mixed alcohol precipitation method

    CN119503889A

  • A method for preparing a multi-element uniformly doped sodium ferric sulfate porous sodium electric positive electrode material by a mixed alcohol precipitation method

    CN119503889B