A preparation method and application of iron, nitrogen and sulfur doped carbon material
By introducing iron, nitrogen and sulfur doped carbon materials into nylon raw materials, and using specific chemical reactions to improve their molecular weight and porosity, the problem of carbon materials agglomeration and low yield in rubber is solved, and the mechanical properties and use of rubber are enhanced life.
Patent Information
- Application Number
- CN202411234538.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-09-04
AI Technical Summary
Existing carbon material reinforcement agents are prone to agglomeration in rubber, unable to fully exert their performance, and have high production costs and low yields, making it difficult to meet the different requirements of rubber products.
Using nylon as raw material, iron, nitrogen and sulfur doped carbon materials are prepared through reflux reaction, ball mill and muffle furnace calcination, and olefin thiolated, oxidizing agents and oxidizing agents using sodium lauryl glutamate, Lawson reagent and potassium ferrate. Sulfur coordination reaction increases molecular weight and porosity, and improves dispersion and yield.
It effectively reduces the agglomeration of carbon materials in rubber, improves the vulcanization degree of rubber, enhances the mechanical properties of rubber, solves the problems of uneven sulfur mixing and low doping in production, and improves the service life of rubber products.
Smart Images

Figure CN118723977B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of carbon materials, and in particular, relates to a preparation method and application of an iron, nitrogen and sulfur doped carbon material. Background Art
[0002] Rubber is a widely used industrial product. In order to meet the different requirements of rubber products in various fields, many additives with different functions are usually added during production to improve the rubber's tensile strength, wear resistance, tear strength, and tensile stress and other mechanical properties, improve performance, and extend the service life of the product. This effect is called rubber reinforcement, and these substances are called reinforcing agents.
[0003] As one of the most common elements in nature, carbon has a variety of bonding modes between atoms and is easy to form allotropes with very different structures and properties. From traditional carbon black to the latest two-dimensional graphene, carbon materials have always played an irreplaceable role in the field of materials science with their unique and excellent physical, electrical and thermal properties. Carbon materials, as rubber reinforcing fillers, can enhance its physical, thermal, electrical and gas / liquid barrier properties and reduce the production cost of rubber products. However, at present, carbon material reinforcing agents also have many problems, such as low yield, easy agglomeration in the rubber matrix during production and use, and cannot fully play their due functional role.
[0004] Therefore, the in-depth development of carbon material reinforcing agents is of great significance. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for preparing iron, nitrogen and sulfur doped carbon materials using nylon as raw material. The obtained carbon materials can be used as reinforcing agents in the field of rubber waterstops.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] In one aspect, the present invention provides a method for preparing an iron, nitrogen and sulfur doped carbon material, comprising the following steps:
[0008] S1: placing a carbon source, sodium lauroyl glutamate and Lawesson's reagent in toluene for reflux reaction to obtain an intermediate product mixed solution, and then drying the mixed solution to obtain an intermediate product;
[0009] S2: adding potassium ferrate to the intermediate product and ball milling;
[0010] S3: The ball-milled product is transferred to a muffle furnace under a protective gas atmosphere for calcination, and the temperature is kept at room temperature after stage heating. After calcination, the temperature is cooled to room temperature to obtain an iron, nitrogen, and sulfur-doped carbon material;
[0011] The carbon source is selected from nylon 6, nylon 11 and / or nylon 12.
[0012] As a further embodiment of the present invention, the reflux temperature in S1 is 110-120° C. and the reflux time is 1-5 hours.
[0013] As a further embodiment of the present invention, the mass ratio of the carbon source, sodium lauroyl glutamate and Lawesson's reagent in S1 is 3-8:1-5:7-12.
[0014] As a further embodiment of the present invention, the mass ratio of the carbon source, sodium lauroyl glutamate and Lawesson's reagent in S1 is 5:3:9.
[0015] As a further embodiment of the present invention, the drying method described in S1 is rotary evaporation.
[0016] As a further embodiment of the present invention, the ball milling speed in S2 is 300-500 rpm; and the ball milling time is 0.5-1.5 hours.
[0017] As a further embodiment of the present invention, the mass ratio of the intermediate product in S2 to potassium ferrate is 2:3-7, preferably 2:5.
[0018] As a further embodiment of the present invention, the protective gas in S3 is selected from nitrogen, argon and / or helium; the rate of introduction of the protective gas is 20-30 mL / min, preferably 26 mL / min.
[0019] As a further implementation scheme of the present invention, the calcination after heating in the stage S3 is: heating to 100-300°C at 3-5°C / min, keeping warm for 1-2 hours, continuing to heat to 800-1000°C at 5-8°C / min, keeping warm for 1-3 hours; the cooling to room temperature is: cooling to room temperature at 3-8°C / min.
[0020] Another aspect of the present invention provides an application of the iron, nitrogen and sulfur doped carbon material obtained according to the method in the field of rubber waterstop.
[0021] The beneficial effects of adopting the above technical solution are:
[0022] 1. A method for preparing iron, nitrogen and sulfur-doped carbon materials using nylon as a raw material is provided. Nylon is used as one of the carbon source and nitrogen source in the implementation method of the present invention, and can undergo ene-thiolation reaction with Lawesson's reagent to increase the molecular weight of the intermediate product and improve the yield of the final product.
[0023] 2. Sodium lauroyl glutamate can undergo ene-thiolation reaction with Lawesson's reagent, which increases the molecular weight of the intermediate product and improves the yield of the final product; at the same time, it can provide nitrogen and oxygen-containing functional groups for the carbon material, improve the dispersion of the carbon material in the rubber, and thus reduce the agglomeration of the carbon material in the rubber.
[0024] 3. Lawesson's reagent, as a sulfur source, undergoes an intermolecular oxygen-sulfur exchange reaction with the raw material to obtain a sulfide product, thereby playing a role in efficient and stable sulfur doping, while increasing the molecular weight of the intermediate product and improving the final yield of the product. In addition, sulfur has a strong coordination property to metals and can effectively coordinate metals, playing a role in effectively doping metals.
[0025] 4. Potassium ferrate acts as an oxidant, pore former and iron source. Potassium ferrate can directly oxidize amino groups to nitrate groups at high temperatures, preventing the release of nitrogen atoms, having a nitrogen fixation effect and increasing the nitrogen content of the product; potassium ferrate decomposes at high temperatures to produce oxygen, which has an etching effect on the material, can regulate the product morphology, increase porosity and increase specific surface area; potassium ferrate is also a good iron source and can coordinate sulfur with Lawesson's reagent to play the role of iron and sulfur doping.
[0026] 5. The iron, nitrogen and sulfur doped carbon material obtained according to the method of the present invention is used as a rubber reinforcing agent, which effectively reduces the agglomeration of the carbon material when used as a rubber reinforcing agent, improves the vulcanization degree of the rubber, and alleviates the problems of uneven sulfur mixing, low doping amount, easy shedding and easy volatilization caused by the use of elemental sulfur in the production process. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 is a particle size distribution diagram of the iron, nitrogen and sulfur doped carbon material of Example 1 of the present invention;
[0028] Figure 2 is a nitrogen adsorption-desorption curve diagram of the iron-, nitrogen- and sulfur-doped carbon material of Example 1 of the present invention;
[0029] Figure 3 is a SEM image of the iron, nitrogen and sulfur doped carbon material of Example 1 of the present invention;
[0030] Figure 4 This is a HR-TEM image of the iron-, nitrogen-, and sulfur-doped carbon material of Example 1 of the present invention (inset: iron oxide particle size distribution). DETAILED DESCRIPTION
[0031] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention is clearly and completely described below in conjunction with specific embodiments.
[0032] Example 1
[0033] S1: 5 g of nylon 6, 3 g of sodium lauroyl glutamate and 9 g of Lawesson's reagent were placed in 150 mL of toluene, and refluxed at 115° C. for 3 hours to obtain an intermediate product mixture, and then the mixture was rotary evaporated to dryness to obtain an intermediate product;
[0034] S2: Add 5 g potassium ferrate to 2 g of the intermediate product and ball mill at 400 rpm for 1 h;
[0035] S3: The ball-milled product was transferred into a muffle furnace into which nitrogen was introduced at a rate of 26 mL / min, and the temperature was raised to 200°C at a rate of 4°C / min. After being kept at this temperature for 1.5 hours, the temperature was further raised to 900°C at a rate of 6°C / min. After being kept at this temperature for 2 hours, the temperature was lowered to room temperature at a rate of 5°C / min to obtain iron-, nitrogen-, and sulfur-doped carbon materials with a yield of 35%;
[0036] The obtained iron, nitrogen and sulfur doped carbon materials were subjected to particle size analysis and nitrogen adsorption and desorption tests. The obtained particle size distribution and nitrogen adsorption and desorption results are shown as follows: Figure 1 and Figure 2 As shown, the specific surface area of the obtained iron, nitrogen and sulfur doped carbon material is 832 cm 2 / g, particle size distribution is 21-29nm;
[0037] The obtained iron, nitrogen and sulfur doped carbon materials were subjected to SEM experiments, and the results are as follows: Figure 3 As shown;
[0038] The obtained iron, nitrogen and sulfur doped carbon materials were subjected to HR-TEM experiments. Figure 4 shown.
[0039] Example 2
[0040] S1: 3 g of nylon 6, 1 g of sodium lauroyl glutamate and 7 g of Lawesson's reagent were placed in 150 mL of toluene, and refluxed at 115° C. for 3 hours to obtain an intermediate product mixture, and then the mixture was rotary evaporated to dryness to obtain an intermediate product;
[0041] S2: Add 5 g potassium ferrate to 2 g of the intermediate product and ball mill at 400 rpm for 1 h;
[0042] S3: The ball-milled product was transferred into a muffle furnace into which nitrogen was introduced at a rate of 26 mL / min, and the temperature was raised to 200°C at a rate of 4°C / min. After being kept at this temperature for 1.5 hours, the temperature was further raised to 900°C at a rate of 6°C / min. After being kept at this temperature for 2 hours, the temperature was lowered to room temperature at a rate of 5°C / min to obtain iron-, nitrogen-, and sulfur-doped carbon materials with a yield of 32%;
[0043] The obtained iron, nitrogen, and sulfur doped carbon materials were subjected to particle size analysis and nitrogen adsorption and desorption tests, and the specific surface area was 795 cm 2 / g, and the particle size distribution is 20-33nm.
[0044] Example 3
[0045] S1: 8 g of nylon 6, 5 g of sodium lauroyl glutamate and 12 g of Lawesson's reagent were placed in 150 mL of toluene, and refluxed at 115° C. for 3 hours to obtain an intermediate product mixture, and then the mixture was rotary evaporated to dryness to obtain an intermediate product;
[0046] S2: Add 5 g potassium ferrate to 2 g of the intermediate product and ball mill at 400 rpm for 1 h;
[0047] S3: The ball-milled product was transferred into a muffle furnace into which nitrogen was introduced at a rate of 26 mL / min, and the temperature was raised to 200°C at a rate of 4°C / min. After being kept at this temperature for 1.5 hours, the temperature was further raised to 900°C at a rate of 6°C / min. After being kept at this temperature for 2 hours, the temperature was lowered to room temperature at a rate of 5°C / min to obtain iron-, nitrogen-, and sulfur-doped carbon materials with a yield of 28%;
[0048] The obtained iron, nitrogen, and sulfur doped carbon materials were subjected to particle size analysis and nitrogen adsorption and desorption tests, and the specific surface area was 801 cm 2 / g, and the particle size distribution is 18-37nm.
[0049] Example 4
[0050] S1: 5 g of nylon 6, 3 g of sodium lauroyl glutamate and 9 g of Lawesson's reagent were placed in 150 mL of toluene, and refluxed at 110° C. for 5 hours to obtain an intermediate product mixture, and then the mixture was rotary evaporated to dryness to obtain an intermediate product;
[0051] S2: Add 5 g potassium ferrate to 2 g of the intermediate product and ball mill at 300 rpm for 1.5 h;
[0052] S3: The ball-milled product was transferred into a muffle furnace into which nitrogen was introduced at a rate of 20 mL / min, and the temperature was raised to 100°C at a rate of 3°C / min. After being kept at this temperature for 2 hours, the temperature was further raised to 800°C at a rate of 5°C / min. After being kept at this temperature for 3 hours, the temperature was lowered to room temperature at a rate of 3°C / min to obtain iron-, nitrogen-, and sulfur-doped carbon materials with a yield of 29%;
[0053] The obtained iron, nitrogen, and sulfur doped carbon materials were subjected to particle size analysis and nitrogen adsorption and desorption tests, and the specific surface area was 784 cm 2 / g, and the particle size distribution is 22-44nm.
[0054] Example 5
[0055] S1: 5 g of nylon 6, 3 g of sodium lauroyl glutamate and 9 g of Lawesson's reagent were placed in 150 mL of toluene, and refluxed at 120° C. for 1 hour to obtain an intermediate product mixture, and then the mixture was rotary evaporated to dryness to obtain an intermediate product;
[0056] S2: Add 5 g potassium ferrate to 2 g of the intermediate product and ball mill at 500 rpm for 0.5 h;
[0057] S3: The ball-milled product was transferred into a muffle furnace into which nitrogen was introduced at a rate of 30 mL / min, and the temperature was raised to 300°C at a rate of 5°C / min. After being kept at this temperature for 1 hour, the temperature was further raised to 1000°C at a rate of 8°C / min. After being kept at this temperature for 1 hour, the temperature was lowered to room temperature at a rate of 8°C / min to obtain iron, nitrogen, and sulfur-doped carbon materials with a yield of 31%;
[0058] The obtained iron, nitrogen, and sulfur doped carbon materials were subjected to particle size analysis and nitrogen adsorption and desorption tests, and the specific surface area was 763 cm 2 / g, and the particle size distribution is 30-49nm.
[0059] Example 6
[0060] S1: 5 g of nylon 6, 3 g of sodium lauroyl glutamate and 9 g of Lawesson's reagent were placed in 150 mL of toluene, and refluxed at 115° C. for 3 hours to obtain an intermediate product mixture, and then the mixture was rotary evaporated to dryness to obtain an intermediate product;
[0061] S2: Add 3 g potassium ferrate to 2 g of the intermediate product and ball mill at 400 rpm for 1 h;
[0062] S3: The ball-milled product was transferred into a muffle furnace into which nitrogen was introduced at a rate of 26 mL / min, and the temperature was raised to 200°C at a rate of 4°C / min. After being kept at this temperature for 1.5 hours, the temperature was further raised to 900°C at a rate of 6°C / min. After being kept at this temperature for 2 hours, the temperature was lowered to room temperature at a rate of 5°C / min to obtain iron-, nitrogen-, and sulfur-doped carbon materials with a yield of 26%.
[0063] The obtained iron, nitrogen, and sulfur doped carbon materials were subjected to particle size analysis and nitrogen adsorption and desorption tests, and the specific surface area was 742 cm 2 / g, and the particle size distribution is 15-34nm.
[0064] Example 7
[0065] S1: 5 g of nylon 6, 3 g of sodium lauroyl glutamate and 9 g of Lawesson's reagent were placed in 150 mL of toluene, and refluxed at 115° C. for 3 hours to obtain an intermediate product mixture, and then the mixture was rotary evaporated to dryness to obtain an intermediate product;
[0066] S2: Add 7 g potassium ferrate to 2 g of the intermediate product and ball mill at 400 rpm for 1 h;
[0067] S3: The ball-milled product was transferred into a muffle furnace into which nitrogen was introduced at a rate of 26 mL / min, and the temperature was raised to 200°C at a rate of 4°C / min. After being kept at this temperature for 1.5 hours, the temperature was further raised to 900°C at a rate of 6°C / min. After being kept at this temperature for 2 hours, the temperature was lowered to room temperature at a rate of 5°C / min to obtain iron-, nitrogen-, and sulfur-doped carbon materials with a yield of 25%;
[0068] The obtained iron, nitrogen, and sulfur doped carbon materials were subjected to particle size analysis and nitrogen adsorption and desorption tests, and the specific surface area was 805 cm 2 / g, and the particle size distribution is 31-56nm.
[0069] Example 8
[0070] S1: 5 g of nylon 11, 3 g of sodium lauroyl glutamate and 9 g of Lawesson's reagent were placed in 150 mL of toluene, and refluxed at 115° C. for 3 hours to obtain an intermediate product mixture, and then the mixture was rotary evaporated to dryness to obtain an intermediate product;
[0071] S2: Add 5 g potassium ferrate to 2 g of the intermediate product and ball mill at 400 rpm for 1 h;
[0072] S3: The ball-milled product was transferred into a muffle furnace into which nitrogen was introduced at a rate of 26 mL / min, and the temperature was raised to 200°C at a rate of 4°C / min. After being kept at this temperature for 1.5 hours, the temperature was further raised to 900°C at a rate of 6°C / min. After being kept at this temperature for 2 hours, the temperature was lowered to room temperature at a rate of 5°C / min to obtain iron-, nitrogen-, and sulfur-doped carbon materials with a yield of 27%;
[0073] The obtained iron, nitrogen, and sulfur doped carbon materials were subjected to particle size analysis and nitrogen adsorption and desorption tests, and the specific surface area was 721 cm 2 / g, and the particle size distribution is 35-53nm.
[0074] Example 9
[0075] S1: 5 g of nylon 12, 3 g of sodium lauroyl glutamate and 9 g of Lawesson's reagent were placed in 150 mL of toluene, refluxed at 115° C. for 3 hours to obtain an intermediate product mixture, and then the mixture was rotary evaporated to dryness to obtain an intermediate product;
[0076] S2: Add 5 g potassium ferrate to 2 g of the intermediate product and ball mill at 400 rpm for 1 h;
[0077] S3: The ball-milled product was transferred into a muffle furnace into which nitrogen was introduced at a rate of 26 mL / min, and the temperature was raised to 200°C at a rate of 4°C / min. After being kept at this temperature for 1.5 hours, the temperature was further raised to 900°C at a rate of 6°C / min. After being kept at this temperature for 2 hours, the temperature was lowered to room temperature at a rate of 5°C / min to obtain iron-, nitrogen-, and sulfur-doped carbon materials with a yield of 29%;
[0078] The obtained iron, nitrogen, and sulfur doped carbon materials were subjected to particle size analysis and nitrogen adsorption and desorption tests, and the specific surface area was 713 cm 2 / g, and the particle size distribution is 29-50nm.
[0079] Comparative Example 1
[0080] S1: 5 g of nylon 6 and 9 g of Lawesson's reagent were placed in 150 mL of toluene, and refluxed at 115° C. for 3 hours to obtain an intermediate product mixture, which was then rotary evaporated to dryness to obtain an intermediate product;
[0081] S2: Add 5 g potassium ferrate to 2 g of the intermediate product and ball mill at 400 rpm for 1 h;
[0082] S3: The ball-milled product was transferred into a muffle furnace into which nitrogen was introduced at a rate of 26 mL / min, and the temperature was raised to 200°C at a rate of 4°C / min. After being kept at this temperature for 1.5 hours, the temperature was further raised to 900°C at a rate of 6°C / min. After being kept at this temperature for 2 hours, the temperature was lowered to room temperature at a rate of 5°C / min to obtain iron-, nitrogen-, and sulfur-doped carbon materials with a yield of 21%;
[0083] The obtained iron, nitrogen, and sulfur doped carbon materials were subjected to particle size analysis and nitrogen adsorption and desorption tests, and the specific surface area was 534 cm 2 / g, and the particle size distribution is 23-62nm.
[0084] Comparative Example 2
[0085] S1: 5 g of nylon 6, 3 g of sodium L-glutamate and 9 g of Lawesson's reagent were placed in 150 mL of toluene, refluxed at 115° C. for 3 hours to obtain an intermediate product mixture, and then the mixture was rotary evaporated to dryness to obtain an intermediate product;
[0086] S2: Add 5 g potassium ferrate to 2 g of the intermediate product and ball mill at 400 rpm for 1 h;
[0087] S3: The ball-milled product was transferred into a muffle furnace into which nitrogen was introduced at a rate of 26 mL / min, and the temperature was raised to 200°C at a rate of 4°C / min. After being kept at this temperature for 1.5 hours, the temperature was further raised to 900°C at a rate of 6°C / min. After being kept at this temperature for 2 hours, the temperature was lowered to room temperature at a rate of 5°C / min to obtain iron-, nitrogen-, and sulfur-doped carbon materials with a yield of 18%;
[0088] The obtained iron, nitrogen, and sulfur doped carbon materials were subjected to particle size analysis and nitrogen adsorption and desorption tests, and the specific surface area was 511 cm 2 / g, and the particle size distribution is 14-59nm.
[0089] Comparative Example 3
[0090] S1: 5 g of nylon 6, 3 g of 3-[3-(cholamidopropyl)dimethylammonium]-1-propanesulfonic acid inner salt and 9 g of Lawesson's reagent were placed in 150 mL of toluene, refluxed at 115° C. for 3 hours to obtain an intermediate product mixture, and then the mixture was rotary evaporated to dryness to obtain an intermediate product;
[0091] S2: Add 5 g potassium ferrate to 2 g of the intermediate product and ball mill at 400 rpm for 1 h;
[0092] S3: The ball-milled product was transferred into a muffle furnace into which nitrogen was introduced at a rate of 26 mL / min, and the temperature was raised to 200°C at a rate of 4°C / min. After being kept at this temperature for 1.5 hours, the temperature was further raised to 900°C at a rate of 6°C / min. After being kept at this temperature for 2 hours, the temperature was lowered to room temperature at a rate of 5°C / min to obtain iron-, nitrogen-, and sulfur-doped carbon materials with a yield of 19%;
[0093] The obtained iron, nitrogen, and sulfur doped carbon materials were subjected to particle size analysis and nitrogen adsorption and desorption tests, and the specific surface area was 572 cm 2 / g, and the particle size distribution is 28-77nm.
[0094] Comparative Example 4
[0095] S1: 5 g of nylon 6, 3 g of cyclopropaneamide and 9 g of Lawesson's reagent were placed in 150 mL of toluene, refluxed at 115° C. for 3 hours to obtain an intermediate product mixture, and then the mixture was rotary evaporated to dryness to obtain an intermediate product;
[0096] S2: Add 5 g potassium ferrate to 2 g of the intermediate product and ball mill at 400 rpm for 1 h;
[0097] S3: The ball-milled product was transferred into a muffle furnace into which nitrogen was introduced at a rate of 26 mL / min, and the temperature was raised to 200°C at a rate of 4°C / min. After being kept at this temperature for 1.5 hours, the temperature was further raised to 900°C at a rate of 6°C / min. After being kept at this temperature for 2 hours, the temperature was lowered to room temperature at a rate of 5°C / min to obtain iron-, nitrogen-, and sulfur-doped carbon materials with a yield of 15%;
[0098] The obtained iron, nitrogen, and sulfur doped carbon materials were subjected to particle size analysis and nitrogen adsorption and desorption tests, and the specific surface area was 562 cm 2 / g, and the particle size distribution is 24-69nm.
[0099] Comparative Example 5
[0100] S1: 5 g of nylon 6, 3 g of sodium lauroyl glutamate and 9 g of phosphorus pentasulfide were placed in 150 mL of toluene, and refluxed at 115° C. for 3 hours to obtain an intermediate product mixture, and then the mixture was rotary evaporated to dryness to obtain an intermediate product;
[0101] S2: Add 5 g potassium ferrate to 2 g of the intermediate product and ball mill at 400 rpm for 1 h;
[0102] S3: The ball-milled product was transferred into a muffle furnace into which nitrogen was introduced at a rate of 26 mL / min, and the temperature was raised to 200°C at a rate of 4°C / min. After being kept at this temperature for 1.5 hours, the temperature was further raised to 900°C at a rate of 6°C / min. After being kept at this temperature for 2 hours, the temperature was lowered to room temperature at a rate of 5°C / min to obtain iron-, nitrogen-, and sulfur-doped carbon materials with a yield of 14%;
[0103] The obtained iron, nitrogen, and sulfur doped carbon materials were subjected to particle size analysis and nitrogen adsorption and desorption tests, and the specific surface area was 549 cm 2 / g, and the particle size distribution is 23-58nm.
[0104] Comparative Example 6
[0105] S1: 5 g of nylon 6, 3 g of sodium lauroyl glutamate and 9 g of Lawesson's reagent were placed in 150 mL of toluene, and refluxed at 115° C. for 3 hours to obtain an intermediate product mixture, and then the mixture was rotary evaporated to dryness to obtain an intermediate product;
[0106] S2: Add 5 g of ferric sulfate to 2 g of the intermediate product and ball mill at 400 rpm for 1 hour;
[0107] S3: The ball-milled product was transferred into a muffle furnace into which nitrogen was introduced at a rate of 26 mL / min, and the temperature was raised to 200°C at a rate of 4°C / min. After being kept at this temperature for 1.5 hours, the temperature was further raised to 900°C at a rate of 6°C / min. After being kept at this temperature for 2 hours, the temperature was lowered to room temperature at a rate of 5°C / min to obtain iron-, nitrogen-, and sulfur-doped carbon materials with a yield of 16%;
[0108] The obtained iron, nitrogen, and sulfur doped carbon materials were subjected to particle size analysis and nitrogen adsorption and desorption tests, and the specific surface area was 347 cm 2 / g, and the particle size distribution is 36-57nm.
[0109] Comparative Example 7
[0110] S1: 5 g of palmitic acid amide, 3 g of sodium lauroyl glutamate and 9 g of Lawesson's reagent were placed in 150 mL of toluene, and refluxed at 115° C. for 3 hours to obtain an intermediate product mixture, and then the mixture was rotary evaporated to dryness to obtain an intermediate product;
[0111] S2: Add 5 g potassium ferrate to 2 g of the intermediate product and ball mill at 400 rpm for 1 h;
[0112] S3: The ball-milled product was transferred into a muffle furnace into which nitrogen was introduced at a rate of 26 mL / min, and the temperature was raised to 200°C at a rate of 4°C / min. After being kept at this temperature for 1.5 hours, the temperature was further raised to 900°C at a rate of 6°C / min. After being kept at this temperature for 2 hours, the temperature was lowered to room temperature at a rate of 5°C / min to obtain iron-, nitrogen-, and sulfur-doped carbon materials with a yield of 13%;
[0113] The obtained iron, nitrogen, and sulfur doped carbon materials were subjected to particle size analysis and nitrogen adsorption and desorption tests, and the specific surface area was 433 cm 2 / g, and the particle size distribution is 25-54nm.
[0114] Comparative Example 8
[0115] S1: 5 g of 2-buteneamide, 3 g of sodium lauroyl glutamate and 9 g of Lawesson's reagent were placed in 150 mL of toluene, and refluxed at 115° C. for 3 hours to obtain an intermediate product mixture, and then the mixture was rotary evaporated to dryness to obtain an intermediate product;
[0116] S2: Add 5 g potassium ferrate to 2 g of the intermediate product and ball mill at 400 rpm for 1 h;
[0117] S3: The ball-milled product was transferred into a muffle furnace into which nitrogen was introduced at a rate of 26 mL / min, and the temperature was raised to 200°C at a rate of 4°C / min. After being kept at this temperature for 1.5 hours, the temperature was further raised to 900°C at a rate of 6°C / min. After being kept at this temperature for 2 hours, the temperature was lowered to room temperature at a rate of 5°C / min to obtain iron-, nitrogen-, and sulfur-doped carbon materials with a yield of 12%;
[0118] The obtained iron, nitrogen, and sulfur doped carbon materials were subjected to particle size analysis and nitrogen adsorption and desorption tests, and the specific surface area was 408 cm 2 / g, and the particle size distribution is 22-58nm.
[0119] Table 1 Heteroatom doping amount of carbon materials obtained in Examples 1 to 9 and Comparative Examples 1 to 8
[0120]
[0121] Example 10
[0122] 100 parts of natural rubber, 30 parts of reinforcing agent (carbon material obtained in Example 1), 6 parts of activator (zinc oxide), 1 part of stearic acid, 17 parts of softener (petroleum resin), 3 parts of antioxidant (MB), 2 parts of accelerator (CZ), 25 parts of filler (FD170) and 16 parts of vulcanizing agent (sulfur).
[0123] S1: Plasticizing
[0124] Set the initial temperature of the internal mixer to 70℃ and the speed to 40 rpm, cut the natural rubber into small pieces and add them into the internal mixer, plasticate for 6 minutes, and discharge when the temperature of the internal mixer reaches 100℃. Pass it on the open mixer, make triangle bags 4 times, and leave it for at least 8 hours before use.
[0125] S2: One-stage mixing
[0126] Set the initial temperature of the internal mixer to 85℃ and the speed to 35 rpm. Add the plasticized natural rubber to the internal mixer. After about 45 seconds, lift the top plug to add reinforcing agent, filler, activator, stearic acid, softener and antioxidant, press the top plug, mix for 160 seconds, lift the plug once in the middle, and discharge the rubber at a temperature of 110℃. After a section of mixed rubber falls into the open mixer, adjust the roller distance to 5mm, automatically pour the rubber 4 times, and the roller temperature of the open mixer does not exceed 60℃. After pouring the rubber, unload the sheet and leave it for at least 8 hours before use.
[0127] S3: Second stage mixing
[0128] Set the initial temperature of the internal mixer to 85℃ and the speed to 35 rpm. Fill the first-stage mixed rubber into the internal mixer. After pressurizing for 45 seconds, lift the top plug to add the vulcanizer and accelerator. Press the top plug, mix for 80 seconds, mix at 110℃, and discharge the rubber. After the second-stage mixed rubber falls into the open mixer, adjust the roller distance to 5mm, automatically pour the rubber 4 times, and the roller temperature of the open mixer does not exceed 60℃. After pouring the rubber, unload the sheet and leave it for at least 8 hours before use.
[0129] Embodiment 11
[0130] The preparation method of this embodiment is the same as that of embodiment 10, the only difference being that the carbon material used is the one obtained in embodiment 2.
[0131] Example 12
[0132] The preparation method of this embodiment is the same as that of embodiment 10, the only difference being that the carbon material used is the one obtained in embodiment 3.
[0133] Example 13
[0134] The preparation method of this embodiment is the same as that of embodiment 10, the only difference being that the carbon material used is the one obtained in embodiment 4.
[0135] Embodiment 14
[0136] The preparation method of this embodiment is the same as that of embodiment 10, the only difference being that the carbon material used is that obtained in embodiment 5.
[0137] Embodiment 15
[0138] The preparation method of this embodiment is the same as that of embodiment 10, the only difference being that the carbon material used is that obtained in embodiment 6.
[0139] Example 16
[0140] The preparation method of this embodiment is the same as that of embodiment 10, the only difference being that the carbon material used is that obtained in embodiment 7.
[0141] Embodiment 17
[0142] The preparation method of this embodiment is the same as that of embodiment 10, the only difference being that the carbon material used is that obtained in embodiment 8.
[0143] Embodiment 18
[0144] The preparation method of this embodiment is the same as that of embodiment 10, the only difference being that the carbon material used is that obtained in embodiment 9.
[0145] Embodiment 19
[0146] The preparation method of this embodiment is the same as that of Example 10, the only difference being that the carbon material used is the one obtained in Comparative Example 1.
[0147] Embodiment 20
[0148] The preparation method of this embodiment is the same as that of Example 10, the only difference being that the carbon material used is that obtained in Comparative Example 2.
[0149] Embodiment 21
[0150] The preparation method of this embodiment is the same as that of Example 10, the only difference being that the carbon material used is the one obtained in Comparative Example 3.
[0151] Embodiment 22
[0152] The preparation method of this embodiment is the same as that of Example 10, the only difference being that the carbon material used is the one obtained in Comparative Example 4.
[0153] Embodiment 23
[0154] The preparation method of this embodiment is the same as that of Example 10, the only difference being that the carbon material used is that obtained in Comparative Example 5.
[0155] Embodiment 24
[0156] The preparation method of this embodiment is the same as that of Example 10, the only difference being that the carbon material used is that obtained in Comparative Example 6.
[0157] Embodiment 25
[0158] The preparation method of this embodiment is the same as that of Example 10, the only difference being that the carbon material used is that obtained in Comparative Example 7.
[0159] Embodiment 26
[0160] The preparation method of this embodiment is the same as that of Example 10, the only difference being that the carbon material used is that obtained in Comparative Example 8.
[0161] Effect example 1: Rubber waterstop performance test
[0162] According to Q / CR 562.2-2017 "Railway Tunnel Drainage Materials Part 2: Waterstop", the performance of waterstop samples 1 to 17 obtained in Examples 10 to 26 was tested, and the results are shown in Table 2.
[0163] Table 2 Performance of Samples 1 to 17
[0164]
[0165] Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art may still modify the technical solutions described in the aforementioned embodiments, or make equivalent substitutions for some of the technical features therein; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing iron, nitrogen and sulfur doped carbon materials, characterized in that: The following steps are involved: S1: placing a carbon source, sodium lauroyl glutamate and Lawesson's reagent in toluene for reflux reaction to obtain an intermediate product mixed solution, and then drying the mixed solution to obtain an intermediate product; S2: adding potassium ferrate to the intermediate product and ball milling; S3: The ball-milled product is transferred to a muffle furnace under a protective gas atmosphere for calcination, and the temperature is kept at room temperature after stage heating. After calcination, the temperature is cooled to room temperature to obtain an iron, nitrogen, and sulfur-doped carbon material; The carbon source is selected from nylon 6, nylon 11 and / or nylon 12.
2. The method for preparing an iron, nitrogen and sulfur doped carbon material according to claim 1, characterized in that: The reflux temperature in S1 is 110-120° C. and the reflux time is 1-5 hours.
3. The method for preparing an iron, nitrogen and sulfur doped carbon material according to claim 1, characterized in that: The mass ratio of the carbon source, sodium lauroyl glutamate and Lawesson's reagent in S1 is 3-8:1-5:7-12.
4. The method for preparing an iron, nitrogen and sulfur doped carbon material according to claim 1, characterized in that: The mass ratio of the carbon source, sodium lauroyl glutamate and Lawesson's reagent in S1 is 5:3:
9.
5. The method for preparing an iron, nitrogen and sulfur doped carbon material according to claim 1, characterized in that: The drying method described in S1 is rotary evaporation.
6. The method for preparing an iron, nitrogen and sulfur doped carbon material according to claim 1, characterized in that: The ball milling speed in S2 is 300-500 rpm; the ball milling time is 0.5-1.5 hours.
7. The method for preparing an iron, nitrogen and sulfur doped carbon material according to claim 1, characterized in that: The mass ratio of the intermediate product in S2 to potassium ferrate is 2:3-7.
8. The method for preparing an iron, nitrogen and sulfur doped carbon material according to claim 1, characterized in that: S3 The protective gas is selected from nitrogen, argon and / or helium; the rate of introduction of the protective gas is 20-30 mL / min.
9. The method for preparing an iron, nitrogen and sulfur doped carbon material according to claim 1, characterized in that: The calcination after heating in the step S3 is as follows: heating to 100-300°C at 3-5°C / min, keeping warm for 1-2 hours, and then heating to 800-1000°C at 5-8°C / min, keeping warm for 1-3 hours; cooling to room temperature is as follows: cooling to room temperature at 3-8°C / min.
10. Use of the iron, nitrogen and sulfur doped carbon material obtained according to the method according to any one of claims 1 to 9 in the field of rubber waterstop.