Three-dimensional graphene powder material and preparation method thereof
By using the spray drying method and one-step heat treatment method of polyvinylpyrrolidone and nitrate, three-dimensional graphene powder materials were successfully prepared, solving the problems of complex preparation and high impurities in the existing technology, and realizing efficient and low-cost graphene. The production of powder materials has expanded its application prospects.
Patent Information
- Application Number
- CN202410988489.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-23
AI Technical Summary
It is difficult to effectively prepare three-dimensional graphene powder materials with existing technology. The preparation process is complex and contains many impurities and defects, making it difficult to achieve large-scale production.
Polyvinylpyrrolidone and nitrate are used as carbon sources and foaming agents, which are transformed into solid powder precursors through spray drying, and three-dimensional graphene powder materials are formed in situ in a one-step heat treatment, avoiding the addition of pore-forming activators and pickling. Simplified process.
It achieves the efficient preparation of three-dimensional graphene powder materials, suppresses the problems of interlayer stacking agglomeration and high contact resistance, maintains the excellent characteristics of graphene, expands its functional applications, and has low-cost, environmentally friendly industrialization value.
Smart Images

Figure CN118723985A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of novel carbon materials, and in particular relates to a three-dimensional graphene powder material and a preparation method thereof. Background Art
[0002] As a new type of two-dimensional carbon material, graphene has shown outstanding performance in the fields of catalysis and batteries due to its excellent physical and chemical properties. However, due to the existence of van der Waals forces between the layers of the two-dimensional graphene sheet structure, it spontaneously aggregates and stacks, thereby losing the effective surface and limiting the excellent performance of graphene. Assembling two-dimensional graphene sheets into three-dimensional graphene structures can effectively inhibit the aggregation and stacking of two-dimensional graphene sheets and maintain the excellent properties of graphene. Moreover, three-dimensional graphene has a larger specific surface area and porous structure, which can further expand the functions of graphene and has broad market prospects.
[0003] Three-dimensional graphene materials can be divided into macroscopic three-dimensional graphene bulk materials (such as macroscopic graphene foam, graphene aerogel, etc.) and microscopic three-dimensional graphene powder materials (such as three-dimensional honeycomb graphene). Compared with three-dimensional graphene bulk materials, three-dimensional graphene powder materials can be modeled into arbitrary shapes or randomly dispersed, without considering the problem of restacking. They can be used in fields such as energy storage and conversion, environmental remediation and thermal management, with the largest market demand and the widest application. However, most of the existing preparation methods can only produce three-dimensional graphene bulk materials, such as template method (such as chemical vapor deposition method) and self-assembly method (such as solvent thermal method). Although a few preparation methods can produce three-dimensional graphene powder materials, the preparation process mostly involves strong acid etching, centrifugal cleaning and other processes, the steps are relatively complicated, and it is difficult to mass produce. More importantly, the three-dimensional graphene powder materials prepared by these methods have more impurities and defects, and there are solid carbon byproducts. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for preparing a three-dimensional graphene powder material in view of the deficiencies of the above-mentioned prior art. The method uses polyvinyl pyrrolidone as a carbon source and nitrate as a foaming agent and catalyst, and converts it into a solid powder precursor through spray drying. The process does not require the addition of a pore-forming activator and acid washing, and then a three-dimensional graphene powder material can be formed in situ through a one-step heat treatment. The preparation process is simple, efficient, low-cost, and easy to scale up. At the same time, it has the advantages of being green and environmentally friendly, and solves the problems of interlayer stacking agglomeration and high contact resistance existing in the three-dimensional assembly of discrete graphene sheets.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a three-dimensional graphene powder material, characterized in that the method comprises the following steps:
[0006] Step 1, dissolving polyvinyl pyrrolidone and nitrate in ultrapure water in sequence to form a mixed solution;
[0007] Step 2: Dewatering and granulating the mixed solution obtained in step 1 by spray drying to obtain a solid powder precursor;
[0008] Step three, spread the solid powder precursor obtained in step two in the inner cavity of the crucible and cover the crucible with a crucible cover, then place the crucible in an atmosphere tube furnace and heat it to 160°C~210°C at a heating rate of 1°C / min~3°C / min in a hydrogen-argon mixed atmosphere and keep it warm for 10min~20min, then heat it to 360°C~420°C at a heating rate of 5°C / min~8°C / min and keep it warm for 10min~30min, then heat it to 950°C~1250°C at a heating rate of 5°C / min~8°C / min and keep it warm for 60min~120min. After the tube furnace is cooled to room temperature, collect the black powder, which is the three-dimensional graphene powder material.
[0009] The above-mentioned method for preparing a three-dimensional graphene powder material is characterized in that the K value of the polyvinyl pyrrolidone in step 1 is 13 or 30; and the nitrate is ammonium nitrate and / or zinc nitrate hexahydrate.
[0010] The above-mentioned method for preparing a three-dimensional graphene powder material is characterized in that the mass ratio of polyvinyl pyrrolidone to nitrate in step 1 is 1:5.0-10.0.
[0011] The above-mentioned method for preparing a three-dimensional graphene powder material is characterized in that the spray drying temperature in step 2 is 100° C. to 150° C., and the flow rate is 80 mL / min to 120 mL / min.
[0012] The above-mentioned method for preparing a three-dimensional graphene powder material is characterized in that the ratio of the volume of the solid powder precursor to the volume of the inner cavity of the crucible in step 3 is 1:5 to 8. Since the heat treatment process of the solid powder precursor in the present invention is a foaming process, which will produce a large volume expansion effect, by limiting the ratio of the volume to the inner cavity of the crucible, a foaming space is reserved to obtain a three-dimensional graphene with a good structure.
[0013] The above-mentioned method for preparing a three-dimensional graphene powder material is characterized in that the flow rate of the hydrogen-argon mixed atmosphere in step three is 0.1L / min to 0.2L / min, and the volume proportion of hydrogen in the hydrogen-argon mixed atmosphere does not exceed 10%.
[0014] At the same time, the present invention also discloses a three-dimensional graphene powder material prepared by the above method, characterized in that the three-dimensional graphene powder material is composed of honeycomb three-dimensional graphene monomer particles, and the particle size of the monomer particles is 50μm~150μm, the monomer particles are open-pore structures and have a three-dimensional continuous pore structure inside, without solid carbon by-products, and the pore size is 5μm~15μm.
[0015] Compared with the prior art, the present invention has the following advantages:
[0016] 1. The present invention uses polyvinyl pyrrolidone as a carbon source and nitrate as a foaming agent and catalyst, which are converted into a solid powder precursor through spray drying. This process does not require the addition of a pore-forming activator and acid washing, and a three-dimensional graphene powder material can be formed in situ through a one-step heat treatment, thereby solving the problems of interlayer stacking agglomeration and high contact resistance existing in the three-dimensional assembly of discrete graphene sheets, and has broad application prospects in the fields of catalysis, hydrogen energy, etc.
[0017] 2. The three-dimensional graphene powder material prepared in situ by the present invention suppresses the common agglomeration and stacking pain point problem of lamellar graphene powder, maintains the excellent properties of graphene, and expands the functional application of graphene powder.
[0018] 3. The preparation method of the present invention has strong controllability. By adjusting the mass ratio of the carbon source and the nitrate and the heat treatment parameters, the number of graphene layers and the three-dimensional pore structure in the three-dimensional graphene powder material can be accurately controlled, and the particle size of the monomer particles in the material can be controlled.
[0019] 4. When ammonium nitrate is used as the foaming agent in the present invention, the decomposition products are all gases without residue; when zinc nitrate hexahydrate is used as the foaming agent, the zinc element can be directly volatilized at high temperature and produce a stratification effect without destroying the structure of the three-dimensional graphene, thereby avoiding the introduction of impurity elements and the generation of by-products such as solid carbon or bulk carbon, so that the product three-dimensional graphene powder material has high chemical purity.
[0020] 5. The preparation process of the present invention is simple and easy to operate, has a short production cycle, low cost, is easy to scale up, and is environmentally friendly, and has industrial value.
[0021] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a macroscopic physical picture of the three-dimensional graphene powder material prepared in Example 1 of the present invention.
[0023] Figure 2 This is a SEM image of the three-dimensional graphene powder material prepared in Example 1 of the present invention.
[0024] Figure 3 These are the AFM images and line scanning analysis images of the three-dimensional graphene powder material prepared in Example 1 of the present invention.
[0025] Figure 4 This is the Raman spectrum of the three-dimensional graphene powder material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0026] Example 1
[0027] This embodiment includes the following steps:
[0028] Step 1: dissolving polyvinyl pyrrolidone with a K value of 30 and zinc nitrate hexahydrate in ultrapure water in a mass ratio of 1:5 to form a mixed solution;
[0029] Step 2: Dewatering and granulating the mixed solution obtained in step 1 by spray drying at a temperature of 120° C. and a flow rate of 80 mL / min to obtain a solid powder precursor;
[0030] Step three, spread the solid powder precursor obtained in step two in the inner cavity of the crucible and cover the crucible with a crucible lid, and the ratio of the volume of the solid powder precursor to the volume of the inner cavity of the crucible is 1:5, and then place the crucible in an atmosphere tube furnace in a hydrogen-argon mixed atmosphere, the flow rate of the hydrogen-argon mixed atmosphere is 0.2L / min, and the volume proportion of hydrogen in the hydrogen-argon mixed atmosphere is 10%, heat to 210°C at a heating rate of 3°C / min and keep warm for 10 minutes, then heat to 360°C at a heating rate of 5°C / min and keep warm for 10 minutes, and then heat to 950°C at a heating rate of 5°C / min and keep warm for 60 minutes. After the tube furnace is cooled to room temperature, collect the black powder, which is the three-dimensional graphene powder material.
[0031] Figure 1 This is a macroscopic physical picture of the three-dimensional graphene powder material prepared in this embodiment. Figure 1 It can be seen that the three-dimensional graphene powder material has a loose powdery appearance.
[0032] Figure 2 The SEM images of the three-dimensional graphene powder material prepared in this embodiment, wherein Figure a is a low-magnification image (×900), and Figures b and c are high-magnification images (×1800) of different parts in Figure a. Figure 2 It can be seen that the three-dimensional graphene powder material is composed of honeycomb three-dimensional graphene monomer particles with a particle size of about 100μm. The surface of the monomer particles is an open-pore structure, and the interior is a three-dimensional continuous pore structure with a pore size of about 10μm, and there is no solid carbon by-product.
[0033] Figure 3The AFM image and line scan analysis image of the three-dimensional graphene powder material prepared in this embodiment are shown in FIG. Figure 3 The left picture is the AFM picture, and the right picture is the line scan analysis picture. Figure 3 It can be seen that the graphene thickness in the three-dimensional graphene powder material is about 1 nm, that is, about 3 layers, which belongs to a few-layer graphene.
[0034] Figure 4 The Raman spectrum of the three-dimensional graphene powder material prepared in this embodiment is Figure 4 It can be seen that the three-dimensional graphene powder material has a high degree of graphitization and the 2D characteristic peak of graphene is significant.
[0035] The nitrate in this embodiment can also be replaced by ammonium nitrate and zinc nitrate hexahydrate.
[0036] Example 2
[0037] This embodiment includes the following steps:
[0038] Step 1: dissolving polyvinyl pyrrolidone with a K value of 30 and zinc nitrate hexahydrate in ultrapure water in a mass ratio of 1:10 to form a mixed solution;
[0039] Step 2: Dewatering and granulating the mixed solution obtained in step 1 by spray drying at a temperature of 150° C. and a flow rate of 120 mL / min to obtain a solid powder precursor;
[0040] Step three, spread the solid powder precursor obtained in step two in the inner cavity of the crucible and cover the crucible with a crucible lid, and the ratio of the volume of the solid powder precursor to the volume of the inner cavity of the crucible is 1:8, and then place the crucible in an atmosphere tube furnace in a hydrogen-argon mixed atmosphere, the flow rate of the hydrogen-argon mixed atmosphere is 0.1L / min, and the volume proportion of hydrogen in the hydrogen-argon mixed atmosphere is 10%, heat to 160°C at a heating rate of 1°C / min and keep warm for 10 minutes, then heat to 420°C at a heating rate of 8°C / min and keep warm for 10 minutes, and then heat to 1250°C at a heating rate of 8°C / min and keep warm for 60 minutes. After the tube furnace is cooled to room temperature, collect the black powder, which is the three-dimensional graphene powder material.
[0041] Example 3
[0042] This embodiment includes the following steps:
[0043] Step 1: dissolving polyvinyl pyrrolidone with a K value of 13 and zinc nitrate hexahydrate in ultrapure water in a mass ratio of 1:8 to form a mixed solution;
[0044] Step 2: Dewatering and granulating the mixed solution obtained in step 1 by spray drying at a temperature of 120° C. and a flow rate of 100 mL / min to obtain a solid powder precursor;
[0045] Step three, spread the solid powder precursor obtained in step two in the inner cavity of the crucible and cover the crucible with a lid, and the ratio of the volume of the solid powder precursor to the volume of the inner cavity of the crucible is 1:6, and then place the crucible in an atmosphere tube furnace in a hydrogen-argon mixed atmosphere, the flow rate of the hydrogen-argon mixed atmosphere is 0.1L / min, and the volume proportion of hydrogen in the hydrogen-argon mixed atmosphere is 10%, heat to 190°C at a heating rate of 2°C / min and keep warm for 10 minutes, then heat to 400°C at a heating rate of 6°C / min and keep warm for 10 minutes, and then heat to 1150°C at a heating rate of 6°C / min and keep warm for 60 minutes. After the tube furnace is cooled to room temperature, collect the black powder, which is the three-dimensional graphene powder material.
[0046] Example 4
[0047] This embodiment includes the following steps:
[0048] Step 1: dissolving polyvinyl pyrrolidone with a K value of 30 and ammonium nitrate in ultrapure water in a mass ratio of 1:6 to form a mixed solution;
[0049] Step 2: Dewatering and granulating the mixed solution obtained in step 1 by spray drying at a temperature of 100° C. and a flow rate of 100 mL / min to obtain a solid powder precursor;
[0050] Step three, spread the solid powder precursor obtained in step two in the inner cavity of the crucible and cover the crucible with a lid, and the ratio of the volume of the solid powder precursor to the volume of the inner cavity of the crucible is 1:8, and then place the crucible in an atmosphere tube furnace in a hydrogen-argon mixed atmosphere, the flow rate of the hydrogen-argon mixed atmosphere is 0.1L / min, and the volume proportion of hydrogen in the hydrogen-argon mixed atmosphere is 5%, heat to 200°C at a heating rate of 3°C / min and keep warm for 10 minutes, then heat to 400°C at a heating rate of 5°C / min and keep warm for 10 minutes, and then heat to 1250°C at a heating rate of 5°C / min and keep warm for 60 minutes. After the tube furnace is cooled to room temperature, collect the black powder, which is the three-dimensional graphene powder material.
[0051] Example 5
[0052] This embodiment includes the following steps:
[0053] Step 1: dissolving polyvinyl pyrrolidone with a K value of 13 and zinc nitrate hexahydrate in ultrapure water in a mass ratio of 1:5 to form a mixed solution;
[0054] Step 2: Dewatering and granulating the mixed solution obtained in step 1 by spray drying at a temperature of 150° C. and a flow rate of 120 mL / min to obtain a solid powder precursor;
[0055] Step three, spread the solid powder precursor obtained in step two in the inner cavity of the crucible and cover the crucible with a lid, and the ratio of the volume of the solid powder precursor to the volume of the inner cavity of the crucible is 1:5, and then place the crucible in an atmosphere tube furnace in a hydrogen-argon mixed atmosphere, the flow rate of the hydrogen-argon mixed atmosphere is 0.2L / min, and the volume proportion of hydrogen in the hydrogen-argon mixed atmosphere is 10%, heat to 210°C at a heating rate of 3°C / min and keep warm for 20 minutes, then heat to 360°C at a heating rate of 5°C / min and keep warm for 30 minutes, and then heat to 950°C at a heating rate of 5°C / min and keep warm for 120 minutes. After the tube furnace is cooled to room temperature, collect the black powder, which is the three-dimensional graphene powder material.
[0056] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a three-dimensional graphene powder material, characterized in that: The method comprises the following steps: Step 1, dissolving polyvinyl pyrrolidone and nitrate in ultrapure water in sequence to form a mixed solution; Step 2: Dewatering and granulating the mixed solution obtained in step 1 by spray drying to obtain a solid powder precursor; Step three, spread the solid powder precursor obtained in step two in the inner cavity of the crucible and cover the crucible with a crucible cover, then place the crucible in an atmosphere tube furnace and heat it to 160°C~210°C at a heating rate of 1°C / min~3°C / min in a hydrogen-argon mixed atmosphere and keep it warm for 10min~20min, then heat it to 360°C~420°C at a heating rate of 5°C / min~8°C / min and keep it warm for 10min~30min, then heat it to 950°C~1250°C at a heating rate of 5°C / min~8°C / min and keep it warm for 60min~120min. After the tube furnace is cooled to room temperature, collect the black powder, which is the three-dimensional graphene powder material.
2. The method for preparing a three-dimensional graphene powder material according to claim 1, characterized in that: In step 1, the K value of the polyvinyl pyrrolidone is 13 or 30; the nitrate is ammonium nitrate and / or zinc nitrate hexahydrate.
3. The method for preparing a three-dimensional graphene powder material according to claim 1, characterized in that: In step 1, the mass ratio of polyvinyl pyrrolidone to nitrate is 1:5.0-10.
0.
4. The method for preparing a three-dimensional graphene powder material according to claim 1, characterized in that: The spray drying temperature in step 2 is 100° C. to 150° C., and the flow rate is 80 mL / min to 120 mL / min.
5. The method for preparing a three-dimensional graphene powder material according to claim 1, characterized in that: The ratio of the volume of the solid powder precursor to the volume of the inner cavity of the crucible in step 3 is 1:5-8.
6. The method for preparing a three-dimensional graphene powder material according to claim 1, characterized in that: The flow rate of the hydrogen-argon mixed atmosphere in step 3 is 0.1 L / min to 0.2 L / min, and the volume proportion of hydrogen in the hydrogen-argon mixed atmosphere does not exceed 10%.
7. A three-dimensional graphene powder material prepared by the method according to any one of claims 1 to 6, characterized in that: The three-dimensional graphene powder material is composed of honeycomb three-dimensional graphene monomer particles, and the particle size of the monomer particles is 50μm to 150μm, the monomer particles are open-pore structures and the interior is a three-dimensional continuous pore structure, there is no solid carbon byproduct, and the pore size is 5μm to 15μm.
Citation Information
Patent Citations
High-power lithium-ion battery anode material, preparation method thereof and negative plate
CN102623685A
Preparation method of ferrothiofluorine or chloride modified three-dimensinoal graphene composite material
CN108163900A
Three-dimensional porous nitrogen-doped graphene composite material and preparation method of nitrogen-doped graphene
CN108264037A
Pyrrhotite type iron sulfide negative electrode material for potassium ion battery and preparation method
CN110828819A
Three-dimensional graphene / carbon nanotube composite material and preparation method thereof
CN111170310A
Cited By
Graphene powder preparation method, graphene powder and application
CN120589743A