Crucible for synthesizing silicon carbide powder and preparation process of silicon carbide powder for crystal growth
By using carbon powder and silicon powder with a specific particle size ratio in the synthesis of silicon carbide powder, and through multi-stage sintering reaction and crucible design, the problem of high β-SiC content caused by uneven particle size in traditional methods is solved, significantly improving The quality and output of the powder used for crystal growth are improved.
Patent Information
- Application Number
- CN202410667934.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-28
- Publication Date
- 2024-10-01
AI Technical Summary
Due to the uneven particle size during the synthesis of traditional silicon carbide powder, the β-SiC content is high, which affects the quality of silicon carbide crystal growth. It is also difficult to effectively control the particle size with existing technology, resulting in low crystal growth yield.
Using specific carbon powder and silicon powder particle size ratios (10μm ~ 80μm and 500μm ~ 6000μm) for mixing, and densifying and sintering through a multi-stage sintering reaction (600℃ ~ 2265℃, different pressures and times), combined with strict mixing Uniformity testing and crucible design to control the sintering process.
Significantly improved the particle size uniformity of silicon carbide powder, increased the proportion of 8-40 mesh powder to 77.77%, improved the quality of crystal growth, reduced the β-SiC content, and increased the output of powder for crystal growth. quantity.
Smart Images

Figure CN118723995A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of semiconductor material preparation, and specifically relates to a crucible device used for preparation and a process for preparing silicon carbide powder. Background Art
[0002] As a third-generation semiconductor material, silicon carbide has the advantages of wide bandgap, high thermal conductivity, high critical breakdown field, high electron saturation drift rate, etc., so it has great application prospects in the field of semiconductor manufacturing. At present, silicon carbide single crystals are grown by PVT method. The specific growth method is: bond the silicon carbide seed crystal to the seed crystal table at the top of the graphite crucible, place silicon carbide powder at the bottom of the crucible, and then place the graphite crucible in a crystal growth furnace for heating. As the temperature rises, the silicon carbide powder at the bottom of the crucible evaporates, and then crystallizes at the top of the graphite crucible to grow silicon carbide crystals. In this process, the purity, particle size, and crystal form of the silicon carbide powder have a great influence on the growth of silicon carbide crystals.
[0003] At present, the synthesis of silicon carbide powder mainly adopts the self-propagating method for growth, that is, high-purity carbon powder and silicon powder are fully mixed in a ratio of 1:1, and then put into a high-purity graphite crucible, and then put into a furnace, and then evacuate, and then introduce high-purity argon as a protective atmosphere, and then heat it up. When the reaction is completed, the silicon carbide powder is taken out, and then crushed, screened, decarbonized, screened, cleaned, and dried to obtain silicon carbide powder. When the traditional method is used to synthesize silicon carbide powder, β-SiC is easy to appear due to the low top temperature during synthesis, and silicon carbide powder containing β-SiC is not easy to grow 4H-SiC crystals during crystal growth, or it causes crystal phase change, reduces the crystal growth yield, and is not conducive to crystal growth.
[0004] In order to solve the above problems, a technical solution is provided in a public document with publication number CN117658142A, a silicon carbide powder material, a preparation method and an application thereof: S1, a first mixture of a first part of carbon powder and a first part of silicon powder is first mixed to form a first mixture; a second mixture of a second part of carbon powder and a second part of silicon powder is second mixed to form a second mixture; the carbon content in the first mixture is lower than the carbon content in the second mixture; S2, the second mixture is spread on the first mixture to form a third mixture, and the third mixture is subjected to a sintering reaction; S3, a decarbonization reaction is carried out on the material obtained by the sintering reaction.
[0005] During the applicant's experiments and production, it was found that the optimal state of silicon carbide powder for crystal growth process is that the particle size is evenly distributed between 8 mesh and 40 mesh, and the powder in this range accounts for more than 70%. However, in the prior art, the proportion of 20-mesh silicon carbide powder with low particle size in silicon carbide powder is relatively high, and the proportion of 20-mesh powder is significantly greater than that of 8-mesh coarse powder. This is the most critical reason for the above-mentioned existing problems. The most important factor in controlling the size of silicon carbide powder is to control the size of raw materials. In the public comparative documents, there is no mention of the particle size of the raw materials silicon powder and carbon powder. The applicant wants to reduce the β-SiC content by adjusting the ratio and arranging the carbon powder and silicon powder differently during sintering. The applicant believes that such a technical solution has limited effect on solving the above-mentioned problems. Summary of the invention
[0006] The purpose of the present invention is to provide a new preparation process and a crucible device used in the process to solve the existing problem that less silicon carbide powder is synthesized each time when the traditional method is used to synthesize silicon carbide powder.
[0007] In order to achieve the above technical objectives, the following first technical solution is now provided: a process for preparing silicon carbide powder for crystal growth, comprising the following steps:
[0008] In the first step, carbon powder with a particle size of 10 μm to 80 μm and silicon powder with a particle size of 500 μm to 6000 μm are mixed at a molar ratio of 1:1 to obtain a first mixed material;
[0009] The second step is to spread the first mixed material in the first step on the inner surface of the crucible;
[0010] The third step is to place the crucible with the first mixed material in the second step into a synthesis furnace for high temperature and low pressure sintering to obtain a second mixed material;
[0011] In the fourth step, the second mixed material in the third step is taken out for crushing and screening and then stored in the form of several mixed material sets.
[0012] This technical solution selects the particle size of the raw materials and uses large-particle silicon powder for sintering, so that the powder in the crucible after sintering is coarser, and the powder used for crystal growth after grinding and screening accounts for a large proportion. In addition, in this application, the amount of carbon powder and silicon powder stirred at one time is large, and the preferred carbon powder and silicon powder are tens of kilograms each.
[0013] In an practicable manner, the sintering reaction in the third step includes:
[0014] In the first heating reaction stage, the temperature is 600°C to 800°C, the time is 2h to 10h, and the pressure is 0.1mbar to 550mbar;
[0015] The second heating reaction stage is at a temperature of 1200°C to 1950°C, a time of 1h to 8h, and a pressure of 5mbar to 430mbar;
[0016] The third heating reaction stage has a temperature of 2000°C to 2265°C, a time of 20h to 80h, and a pressure of 1mbar to 245mbar.
[0017] The above reaction stage is to enhance the plasticity and viscosity of the particles and promote the densification sintering of silicon carbide through the interaction of pressure and temperature. The densification principle of this embodiment is: the temperature of the first heating reaction stage is lower than that of the comparative documents and the prior art, the pressure is higher than that of the comparative documents and the prior art, and the time is longer than that of the comparative documents and the prior art. This is because the silicon powder particles in this embodiment are larger, and the carbon powder needs to be filled into the gaps between the silicon powder particles in the first heating reaction stage. However, the first stage reaction temperature in the comparative documents and the prior art exceeds 1000°C, and even directly reaches 1350°C to 1400°C. At this temperature, the carbon particles and the silicon particles will be directly sintered together, and the gaps between the silicon powder particles cannot be filled completely.
[0018] Then, the time of the second heating reaction stage in this embodiment is reduced, which enables the already filled carbon powder particles and silicon powder particles to quickly enter the third heating reaction stage for sintering. The time of the third heating reaction stage is increased, that is, after high temperature and pressure, the pores between the silicon carbide particles are rapidly reduced, the density is greatly increased, and sliding behavior occurs between the particles, thereby increasing the contact area between the silicon carbide particles. As time goes by, the rate of density increase begins to decrease, and eventually approaches the process of ordinary sintering; the reaction time is further extended, so that the generated β-SiC will be converted into a large amount of more stable α-SiC crystal when it exceeds 2000°C.
[0019] In an practicable manner, the first mixed material in the second step is laid on the crucible to a thickness of 190 mm to 350 mm, which can ensure that the mixed material is heated evenly during sintering.
[0020] In an operative manner, the mixed material set in the fourth step includes silicon carbide particles with a size of 8-40 mesh for crystal growth, which accounts for more than 75% of the mixed material set.
[0021] In an practicable manner, there is also a first mixing uniformity detection step between the first step and the second step, which step includes:
[0022] S1. After mixing for 8h-15h, stop the mixing device and take out 500g~600g of the first mixture at at least two locations in the mixing device;
[0023] S2. Spread the first mixture taken out in S1 in a flat-bottomed container and mark them as A and B in order;
[0024] S3. In container A, select at least three points of the first mixture to determine the carbon content by spectral analysis and record them as A1, A2, and A3;
[0025] S4. Synchronously with S3, in container B, select at least three points of the first mixture to determine the carbon content by spectral analysis, and record B1, B2, B3;
[0026] S5. Compare the data in S3 and S4 with the theoretical value. If the carbon content fluctuates above or below the theoretical value, the first mixture in the mixing tank has been mixed evenly.
[0027] S6. Put the first mixture after S5 back into the mixing tank, and then wait for the second step;
[0028] S7. In S5, if the carbon content fluctuates between the theoretical value, the first mixture in the stirring tank has not been stirred evenly;
[0029] S8. Put the first mixed material after S7 back into the mixing tank and perform the mixing operation in the first step again.
[0030] When selecting materials, the carbon powder particles and silicon powder are screened, and in order to make the sintered particles more uniform in size, the carbon powder and silicon powder need to be strictly mixed. In addition to increasing the mixing time, the mixed material needs to be tested to ensure that the mixture at each position in the mixing device is uniform. Through such strict mixing, the uniformity of the sintering reaction particle size can be achieved, so that the content of silicon carbide powder used for crystal growth after crushing and screening after the reaction is higher than that of the prior art.
[0031] In a second aspect, a crucible for synthesizing silicon carbide powder is used for preparing the silicon carbide powder for crystal growth as described in any one of the first aspects.
[0032] In an practicable manner, the crucible comprises a crucible body, wherein the crucible body has a receiving cavity, and above the receiving cavity there is a sealing cover connected to the crucible body.
[0033] A circular shell is provided on the side and a bottom plate is provided below, the shell and the bottom plate are integrally formed, and a partition is provided inside the shell and the bottom plate, and the partition is hollow inside;
[0034] The bottom plate is provided with an air inlet communicating with the partition, and the shell is provided with an air outlet communicating with the partition;
[0035] The cross section of the partition in the bottom plate is conical, the air inlet is arranged at the apex of the cone, and a sealing ball is provided at the air inlet to prevent the air in the partition from flowing out of the air inlet; the sealing ball is a metal-ceramic composite and weighs 200g to 500g.
[0036] In an practicable manner, the crucible comprises a crucible body, the crucible body is provided with a crucible cover, and below the crucible cover there is a partition plate arranged in the crucible body and cross-cutting the crucible body; the total weight of the crucible body and the crucible cover is 6500g-9000g.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] The particle size of the raw materials is screened in the technical solution of this application. Compared with the general technicians in this field who only weigh how many grams to make the proportion and ignore the problem of the particle size of the raw materials, this technical solution performs the sintering reaction under the condition of controlling the particle size of the raw materials. The proportion of the desired size of the particles obtained by grinding and screening after sintering is much higher than the output of the prior art. Among them, by using the sintering process used in this patent to sinter the mixed powder through the raw material synthesis furnace, the output powder with a particle size of 8 to 40 mesh accounts for 77.77% of the total powder output.
[0039] Moreover, after the raw materials are screened, they are further stirred to be absolutely uniform. This is also a step that is easily overlooked by technical personnel in this field. Generally, carbon powder and silicon powder are taken out for use as long as they are mixed. However, no matter how long the mixing is carried out during the mixing process, it is still difficult to achieve absolute uniformity. In order to achieve this effect, the applicant conducts intermittent random sampling of the mixed materials in the mixing barrel for testing, and proceeds to the next step of crucible coating when the values of each sampling and each sampling location are the same.
[0040] In the present technical solution, the temperature of the first heating reaction stage is lower than 1000°C. To ensure uniform heating of the mixture, the mixture needs to be spread in a certain thickness in the crucible, so as to ensure uniform heating in this stage and enable the carbon particles to be fully filled between the silicon particles.
[0041] In order to solve the problems of uniform heating in the early stage and the need to maintain the temperature for a long time at high temperature in the later stage, the crucible designed for this process can solve the above problems well; because a gas temperature regulation system is arranged inside the crucible in the technical solution, the gas regulation system can help to make the temperature regulation in the crucible more flexible, and hot gas can be introduced to assist in the introduction of hot gas if it needs to heat up quickly, and cold gas can be introduced to assist in the introduction of cold gas if it needs to heat up slowly; cold gas can be introduced to assist in the introduction of cold gas if it needs to cool down quickly, and hot gas can be introduced to assist in the introduction of hot gas if it needs to cool down slowly. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] 1 crucible body, 2 containing cavity, 3 sealing cover, 4 shell, 5 bottom plate, 6 partition, 7 air inlet, 8 air outlet, 9 composite material ring, 10 sealing ball, 11 air inlet pipe;
[0043] Figure 1 is a cross-sectional schematic diagram of a crucible;
[0044] Figure 2 is a cross-sectional schematic diagram of another crucible;
[0045] Figure 3 This is a working diagram of another type of crucible; DETAILED DESCRIPTION
[0046] In the description of the present invention, it should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0047] The present application discloses a first aspect to provide a process for preparing silicon carbide powder for crystal growth, comprising the following steps:
[0048] In the first step, carbon powder with a particle size of 10 μm to 80 μm and silicon powder with a particle size of 500 μm to 6000 μm are mixed at a molar ratio of 1:1 to obtain a first mixed material;
[0049] Wherein, S1. After mixing for 8h-15h, stop the mixing device and take out 500g~600g of the first mixed material from at least two places in the mixing device;
[0050] S2. Spread the first mixture taken out in S1 in a flat-bottomed container and mark them as A and B in order;
[0051] S3. In container A, select at least three points of the first mixture to determine the carbon content by spectral analysis and record them as A1, A2, and A3;
[0052] S4. Synchronously with S3, in container B, select at least three points of the first mixture to determine the carbon content by spectral analysis, and record B1, B2, B3;
[0053] S5. Compare the data in S3 and S4 with the theoretical value. If the carbon content fluctuates above or below the theoretical value, the first mixture in the mixing tank has been mixed evenly.
[0054] S6. Put the first mixture after S5 back into the mixing tank and wait for the next operation;
[0055] S7. In S5, if the carbon content fluctuates between the theoretical value, the first mixture in the stirring tank has not been stirred evenly;
[0056] S8. Put the first mixed material after S7 back into the mixing tank and perform mixing operation again.
[0057] The second step is to spread the first mixed material in the first step on the inner surface of the crucible; the spreading thickness is 190 mm to 350 mm.
[0058] The third step is to place the crucible with the first mixed material in the second step into a synthesis furnace for high temperature and low pressure sintering to obtain a second mixed material;
[0059] The sintering reaction in this step includes: a first heating reaction stage, a temperature of 600°C to 800°C, a time of 2h to 10h, and a pressure of 0.1mbar to 550mbar;
[0060] The second heating reaction stage is at a temperature of 1200°C to 1950°C, a time of 1h to 8h, and a pressure of 5mbar to 430mbar;
[0061] The third heating reaction stage has a temperature of 2000°C to 2265°C, a time of 20h to 80h, and a pressure of 1mbar to 245mbar.
[0062] In the fourth step, the second mixed material in the third step is taken out for crushing and screening and then stored in a plurality of mixed material sets; wherein the silicon carbide particles with a size of 8-40 mesh used for crystal growth account for more than 75% of the mixed material set.
[0063] In order to make the sintering in the third step of the first aspect more in line with the needs, the following is now disclosed: Figure 1 The crucible device of the second aspect shown is used for preparing synthetic silicon carbide powder; it comprises a crucible body 1, the crucible body 1 has a receiving chamber 2, and the upper part of the receiving chamber 2 has a sealing cover 3 connected to the crucible body 1,
[0064] A circular shell 4 is provided on the side, and a bottom plate 5 is provided below. The shell 4 and the bottom plate 5 are integrally formed, and a partition 6 is provided inside the shell 4 and the bottom plate 5, and the partition 6 is hollow inside.
[0065] The bottom plate 5 is provided with an air inlet 7 communicating with the partition 6 , and the shell 4 is provided with an air outlet 8 communicating with the partition 6 .
[0066] A high temperature resistant composite material ring 9 is arranged in the gap between the sealing cover 3 and the accommodating chamber 2. The preferred material of the composite material ring 9 is carbon fiber. The cross-sectional structure of the composite material ring 9 is "L" shaped, with a vertical side and a horizontal side. The vertical side is fixed on the accommodating chamber 2. The horizontal side is in contact with the sealing cover 3, and a layer of high temperature glue is also laid on the horizontal side. When laid, it is in a flowing state. After the sealing cover 3 is in close contact with the accommodating chamber 2, the high temperature glue enters and fills the gap, and becomes an elastic body after curing at room temperature.
[0067] In the crucible, the cross section of the partition 6 in the bottom plate 5 is conical, and an air inlet 7 is provided at the apex of the cone. A sealing ball 10 is provided at the air inlet 7 to prevent the air in the partition 6 from flowing out of the air inlet 7. The sealing ball 10 is a metal-ceramic composite, weighing 200 g to 500 g, and preferably weighing 300 g.
[0068] The interlayer 6 in the crucible of the present application is formed by carbon fiber using 3D printing technology. After the interlayer 6 is manufactured, a graphite mixture is coated on it, and then pressed, and then manufactured according to the graphite crucible manufacturing steps in the prior art. The sealing ball is placed when the base plate is printed when the interlayer is manufactured.
[0069] The setting of the interlayer 6 can control the temperature in the crucible to prevent the temperature in the crucible from being too high during the heating process, or the temperature in the crucible from dropping too fast when the heating is stopped. Its use method is that during the heating process, room temperature air is introduced into the interlayer 6, and the pressure generated by the air is sufficient to open the sealing ball 10, and the air entering the interlayer 6 will take away part of the heat and flow out from the air outlet 8 into the sintering furnace. When the heating is stopped, the sintering furnace in the interlayer 6 and the air in the interlayer 6 will press the sealing ball 10 more tightly against the air inlet 7 to prevent the hot gas from escaping, thereby ensuring that the temperature of the entire sintering furnace will not drop too fast. When the crucible needs to be taken out quickly after the later sintering is completed, cold air can be introduced into the air inlet 7 to achieve rapid cooling. The air inlet 7 in the present application is provided with an air inlet pipe 11 extending from the crucible to the outside of the sintering furnace, and the air inlet pipe 11 is a graphite tube.
[0070] In the sintering of the present application, it is also possible to use Figure 2 The crucible device shown is used for preparing synthetic silicon carbide powder; it comprises a crucible body, a crucible cover on the crucible body, and a partition plate arranged in the crucible body and cross-cutting the crucible body under the crucible cover; the total weight of the crucible body and the crucible cover is 6500g-9000g, preferably the total weight of the crucible body and the crucible cover is 6500g. By placing the above-mentioned crucible body as shown in Figure 3 Calcination takes place in the furnace shown.
[0071] The disclosure of the first aspect of the present application is further illustrated below by way of examples, but the disclosure is not limited thereby.
[0072] In the first embodiment, carbon powder with a particle size of 10 μm and silicon powder with a particle size of 500 μm are mixed at a molar ratio of 1:1. When the mixture reaches absolute uniformity after detection, the first mixture is loaded into the crucible of the second aspect, and the laying thickness is 190 mm. Then the sintering reaction is carried out. In the first heating reaction stage, the temperature is 600°C, the time is 10 hours, and the pressure is 550 mbar; in the second heating reaction stage, the temperature is 1950°C, the time is 1 hour, and the pressure is 430 mbar; in the third heating reaction stage, the temperature is 2265°C, the time is 80 hours, and the pressure is 245 mbar. After cooling, the silicon carbide powder is taken out and crushed and sieved by a crusher and a sieving machine. The particle size of the crushed material is 600 μm. After the crushing is completed, the sieving machine is used for sieving. Silicon carbide particles with a size of 8-40 mesh are selected by sieving, and this part of silicon carbide particles accounts for more than 75% of the entire silicon carbide particles.
[0073] In the second embodiment, carbon powder with a particle size of 80 μm and silicon powder with a particle size of 6000 μm are mixed at a molar ratio of 1:1. When the mixture reaches absolute uniformity after detection, the first mixture is loaded into the crucible of the second aspect, and the laying thickness is 190 mm. Then the sintering reaction is carried out. In the first heating reaction stage, the temperature is 600°C, the time is 10 hours, and the pressure is 550 mbar; in the second heating reaction stage, the temperature is 1950°C, the time is 1 hour, and the pressure is 430 mbar; in the third heating reaction stage, the temperature is 2265°C, the time is 80 hours, and the pressure is 245 mbar. After cooling, the silicon carbide powder is taken out and crushed and sieved by a crusher and a sieving machine. The particle size of the crushed material is 600 μm. After the crushing is completed, the sieving machine is used for sieving. Silicon carbide particles with a size of 8-40 mesh are selected by sieving. This part of silicon carbide particles accounts for more than 77% of the entire silicon carbide particles.
[0074] In the third embodiment, carbon powder with a particle size of 30 μm and silicon powder with a particle size of 1500 μm are mixed at a molar ratio of 1:1. When the mixture reaches absolute uniformity after detection, the first mixture is loaded into the crucible of the second aspect, and the laying thickness is 190 mm. Then the sintering reaction is carried out. In the first heating reaction stage, the temperature is 600°C, the time is 10 hours, and the pressure is 550 mbar; in the second heating reaction stage, the temperature is 1950°C, the time is 1 hour, and the pressure is 430 mbar; in the third heating reaction stage, the temperature is 2265°C, the time is 80 hours, and the pressure is 245 mbar. After cooling, the silicon carbide powder is taken out and crushed and sieved by a crusher and a sieving machine. The particle size of the crushed material is 600 μm. After the crushing is completed, the sieving machine is used for sieving. Silicon carbide particles with a size of 8-40 mesh are selected by sieving. This part of silicon carbide particles accounts for more than 76% of the entire silicon carbide particles.
[0075] In the fourth embodiment, carbon powder with a particle size of 60 μm and silicon powder with a particle size of 4000 μm are mixed at a molar ratio of 1:1. When the mixture reaches absolute uniformity after detection, the first mixture is loaded into the crucible of the second aspect, and the laying thickness is 190 mm. Then the sintering reaction is carried out. In the first heating reaction stage, the temperature is 600°C, the time is 10 hours, and the pressure is 550 mbar; in the second heating reaction stage, the temperature is 1950°C, the time is 1 hour, and the pressure is 430 mbar; in the third heating reaction stage, the temperature is 2265°C, the time is 80 hours, and the pressure is 245 mbar. After cooling, the silicon carbide powder is taken out and crushed and sieved by a crusher and a sieving machine. The particle size of the crushed material is 600 μm. After the crushing is completed, the sieving machine is used for sieving. Silicon carbide particles with a size of 8-40 mesh are selected by sieving. This part of silicon carbide particles accounts for more than 78% of the entire silicon carbide particles.
[0076] It can be concluded from the above embodiments that the particle size of the raw materials has a very important influence on the size of the silicon carbide particles after the reaction, but the technicians in the prior art have ignored this technical problem and usually think that the desired particle size of silicon carbide can be obtained by later crushing and grinding. In fact, the silicon carbide particles with a size of 8-40 mesh obtained after grinding, crushing and screening for crystal growth have a small content. As an enterprise that has only developed crystal growth technology at this stage, the cost of such silicon carbide sintering process is too high. In order to increase the output of 8-40 mesh silicon carbide particles, the R&D personnel of this application studied the sintering process of the prior art and found that only by screening the particle size of the raw materials can the output of 8-40 mesh silicon carbide particles be as high as 70% to 85%.
[0077] The above will clearly and completely describe the concept, specific structure and technical effects of the present invention in combination with the embodiments and drawings, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by technicians in this field without creative work are all within the scope of protection of the present invention. In addition, all the connection / connection relationships mentioned in the text do not refer to the direct connection of components, but refer to the fact that a better connection structure can be formed by adding or reducing connection accessories according to the specific implementation situation.
[0078] The specific description of the present invention in the above embodiments is only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Technical engineers in this field may make some non-essential improvements and adjustments to the present invention based on the contents of the above invention, which fall within the scope of protection of the present invention.
Claims
1. A process for preparing silicon carbide powder for crystal growth, characterized in that: The steps include: In the first step, carbon powder with a particle size of 10 μm to 80 μm and silicon powder with a particle size of 500 μm to 6000 μm are mixed at a molar ratio of 1:1 to obtain a first mixed material; The second step is to spread the first mixed material in the first step on the inner surface of the crucible; The third step is to place the crucible with the first mixed material in the second step into a synthesis furnace for high temperature and low pressure sintering to obtain a second mixed material; In the fourth step, the second mixed material in the third step is taken out for crushing and screening and then stored in the form of several mixed material sets.
2. The process for preparing silicon carbide powder for crystal growth according to claim 1, characterized in that: The sintering reaction in the third step includes: In the first heating reaction stage, the temperature is 600°C to 800°C, the time is 2h to 10h, and the pressure is 0.1mbar to 550mbar; The second heating reaction stage is at a temperature of 1200°C to 1950°C, a time of 1h to 8h, and a pressure of 5mbar to 430mbar; The third heating reaction stage has a temperature of 2000°C to 2265°C, a time of 20h to 80h, and a pressure of 1mbar to 245mbar.
3. The process for preparing silicon carbide powder for crystal growth according to claim 1, characterized in that: The thickness of the first mixed material in the second step on the crucible is 190 mm to 350 mm.
4. The process for preparing silicon carbide powder for crystal growth according to claim 1, characterized in that: The mixed material set in the fourth step includes silicon carbide particles with a size of 8-40 mesh for crystal growth, which accounts for more than 75% of the mixed material set.
5. The process for preparing silicon carbide powder for crystal growth according to claim 1, characterized in that: There is also a first mixing uniformity detection step between the first step and the second step, which comprises: S1. After mixing for 8h to 15h, stop the mixing device and take out 500g to 600g of the first mixture from at least two locations in the mixing device; S2. Spread the first mixture taken out in S1 in a flat-bottomed container and mark them as A and B in order; S3. In container A, select at least three points of the first mixture to determine the carbon content by spectral analysis and record them as A1, A2, and A3; S4. Synchronously with S3, in container B, select at least three points of the first mixture to determine the carbon content by spectral analysis, and record B1, B2, B3; S5. Compare the data in S3 and S4 with the theoretical value. If the carbon content fluctuates above or below the theoretical value, the first mixture in the mixing tank has been mixed evenly. S6. Put the first mixture after S5 back into the mixing tank, and then wait for the second step; S7. In S5, if the carbon content fluctuates between the theoretical value, the first mixture in the stirring tank has not been stirred evenly; S8. Put the first mixed material after S7 back into the mixing tank and perform the mixing operation in the first step again.
6. A crucible for synthesizing silicon carbide powder, characterized in that: Used for preparing silicon carbide powder for crystal growth as claimed in any one of claims 1 to 5.
7. The crucible for synthesizing silicon carbide powder according to claim 6, characterized in that: The crucible comprises a crucible body, wherein the crucible body has a containing cavity, and above the containing cavity there is a sealing cover connected to the crucible body. A circular shell is provided on the side and a bottom plate is provided below, the shell and the bottom plate are integrally formed, and a partition is provided inside the shell and the bottom plate, and the partition is hollow inside; The bottom plate is provided with an air inlet connected to the partition, and the shell is provided with an air outlet connected to the partition; wherein, the cross-section of the partition in the bottom plate is conical, the air inlet is provided at the apex of the cone, and a sealing ball is provided at the air inlet, and the sealing ball prevents the air in the partition from flowing out of the air inlet; the sealing ball is a metal-ceramic composite and weighs 200g to 500g.
8. The crucible for synthesizing silicon carbide powder according to claim 6, characterized in that: The crucible comprises a crucible body, the crucible body is provided with a crucible cover, and a partition plate is provided below the crucible cover and is arranged inside the crucible body and crosses the crucible body; the total weight of the crucible body and the crucible cover is 6500g-9000g.
Citation Information
Patent Citations
High-purity silicon carbide preparation device and method
CN109137077A
Device and method for preparing silicon carbide powder with uniform granularity
CN116654940A
Crucible for silicon carbide crystal growth
CN209144318U
Device for preparing silicon carbide through PVT method
CN218089892U