Preparation method of flame-retardant modified waterborne polyurethane coating

By using a combination of guanidine-containing pentaerythritol phosphate intermediate and polyurethane raw materials, the phosphorus and nitrogen content of the polyurethane coating is improved, and the problems of flammable and antibacterial properties of the coating are solved, achieving significant flame retardant and antibacterial effects.

CN118995031APending Publication Date: 2024-11-22FUJIAN ZHUANLI ELECTRIC TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411153533.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing polyurethane coatings are flammable after curing and have poor antibacterial properties, which cannot effectively improve their application areas.

Method used

Using guanidine-containing pentaerythritol phosphate intermediates, polytetrahydrofuran polyether glycol, toluene diisocyanate and other raw materials, a modified aqueous polyurethane coating is prepared through specific reaction steps and additives, and the content of phosphorus and nitrogen is increased, so as to Improve flame retardant and antibacterial properties.

Benefits of technology

The prepared polyurethane coating not only has excellent flame retardant effect, but also significantly improves antibacterial properties. Through the formation of phosphoric acid and flame retardant gases, a dense carbon layer and electrostatic adsorption are formed, effectively inhibiting combustion and bacterial growth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995031A_ABST
    Figure CN118995031A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of coatings, and discloses a preparation method of a flame-retardant modified waterborne polyurethane coating, which comprises the following steps: taking pentaerythritol, phosphorus oxychloride, p-nitrophenol, dicyandiamide and the like as raw materials, and reacting to obtain a guanidyl-containing pentaerythritol phosphate intermediate; the preparation method comprises the following steps: by taking polytetrahydrofuran polyether glycol, toluene diisocynate, a guanidyl-containing pentaerythritol phosphate intermediate and the like as raw materials, reacting to obtain a modified waterborne polyurethane dispersion, finally adding a wetting agent, a defoaming agent and the like into the modified waterborne polyurethane dispersion, and uniformly stirring to obtain the flame-retardant modified waterborne polyurethane coating. The waterborne polyurethane coating prepared by the preparation method disclosed by the invention has a relatively good antibacterial effect and a relatively good flame-retardant effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, in particular to a method for preparing a flame retardant modified waterborne polyurethane coating. Background Art

[0002] The full name of polyurethane is polyurethane, which is a polymer material prepared by condensation reaction of polyols and polyisocyanates. Waterborne polyurethane has excellent mechanical properties, wear resistance and bonding properties, and is widely used in adhesives, finishing agents, coatings and other fields. Waterborne polyurethane coatings prepared from waterborne polyurethane are environmentally friendly, non-toxic, and have excellent mechanical properties. They are widely used in the coating of various industrial products. However, polyurethane coatings are easy to burn after curing, and their flame retardancy is poor. In addition, the antibacterial properties of polyurethane coatings are also poor, so they need to be modified to improve their antibacterial and flame retardant properties, thereby improving their application areas.

[0003] Guanidine compounds are a class of compounds that are widely present in nature and have multiple biological activities. They play an important role in the research and development of anti-tumor, anti-viral and other drugs. For example, the patent application publication number CN 104530951A discloses a method for preparing a phosphorus-containing waterborne polyurethane resin flame-retardant coating. The invention uses phosphorus-containing waterborne polyurethane resin, defoaming agent and the like as raw materials. The coating prepared has good flame retardant properties, but does not improve its antibacterial properties. Based on this, a polyurethane coating prepared by the present invention has excellent antibacterial and flame retardant properties. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] In view of the deficiencies in the prior art, the present invention provides a method for preparing a flame-retardant modified waterborne polyurethane coating. The prepared waterborne polyurethane coating has good antibacterial and flame-retardant effects.

[0006] (II) Technical solution

[0007] A method for preparing a flame retardant modified waterborne polyurethane coating, the preparation method is as follows:

[0008] Step (1), under nitrogen conditions, polytetrahydrofuran polyether diol and toluene diisocyanate are added to a flask, reacted at 70-80° C. for 2 hours, then 2,2-dihydroxymethyl propionic acid is added thereto, reacted for 1-3 hours, then 1,4-butanediol is added thereto, chain extension reaction is carried out for 1-2 hours, after the reaction is completed, the temperature is reduced to 60-70° C., a guanidine-containing pentaerythritol phosphate intermediate is added thereto, the reaction is continued for 40-80 minutes, the temperature is reduced to 40° C., stirred and emulsified for 20-40 minutes, and finally triethylamine is added thereto for neutralization to obtain a modified waterborne polyurethane dispersion.

[0009] Step (2), adding the modified waterborne polyurethane dispersion into a high-speed stirrer, stirring and dispersing, and then adding a photoinitiator, a wetting agent, a leveling agent, a defoaming agent, and deionized water thereto, stirring at a stirring speed of 800-1000 r / min for 10-20 minutes to obtain a flame retardant modified waterborne polyurethane coating.

[0010] Preferably, in the step (1), the mass ratio of polytetramethylene glycol, toluene diisocyanate, 2,2-dihydroxymethylpropionic acid, 1,4-butanediol, guanidine-containing pentaerythritol phosphate intermediate, and triethylamine is 100:35-50:6-8:2-5:5-25:2-5.

[0011] Preferably, in step (2), the mass ratio of the modified aqueous polyurethane dispersion, the photoinitiator, the wetting agent, the leveling agent, the defoaming agent and the deionized water is 100:2-5:0.1-0.5:0.1-0.5:0.1-0.3:2-5.

[0012] Preferably, in step (1), the preparation method of the guanidine-containing pentaerythritol phosphate intermediate is:

[0013] S1. Add pentaerythritol and phosphorus oxychloride into a flask, stir and disperse, heat to 75-90°C, react for 12-24h. After the reaction is completed, cool to room temperature, filter, wash with ethanol, and dry to obtain intermediate 1.

[0014] S2. Add intermediate 1 and p-nitrophenol into a flask filled with acetonitrile solvent, stir and disperse, then add triethylamine, heat to 70-85°C, react for 8-15h, after the reaction is completed, cool to room temperature, filter, wash with ethanol, and dry to obtain intermediate 2.

[0015] S3. Under nitrogen conditions, add intermediate 2 and Pd / C into a flask filled with ethanol solvent, stir and disperse, heat to 40-50°C, add 85% by mass of hydrazine hydrate, reflux for 2-5h, filter, rotary evaporate, wash with deionized water, and dry to obtain intermediate 3.

[0016] S4, adding intermediate 3 to deionized water, stirring and dispersing, adding 30-40% hydrochloric acid aqueous solution thereto, stirring and mixing evenly, adding dicyandiamide thereto, heating to 75-90°C, reacting for 5-10 hours, and after the reaction is completed, concentrating, precipitating with acetone, filtering, and drying to obtain a guanidine-containing pentaerythritol phosphate intermediate.

[0017] Preferably, in S1, the molar ratio of pentaerythritol to phosphorus oxychloride is 1:4.5-6.

[0018] Preferably, in S2, the molar ratio of intermediate 1, p-nitrophenol and triethylamine is 1:2.5-3.5:2.5-4.

[0019] Preferably, in S4, the molar ratio of intermediate 3 to dicyandiamide is 1:0.8-1.

[0020] (III) Beneficial technical effects

[0021] The invention uses pentaerythritol and phosphorus oxychloride as raw materials and adopts a solvent-free method to obtain an intermediate 1. The intermediate 1 is reacted with p-nitrophenol under the catalysis of triethylamine to obtain an intermediate 2, and the intermediate 2 is reduced to obtain an intermediate 3, and an amino group contained in the intermediate 3 is reacted with dicyandiamide to obtain a guanidine-containing pentaerythritol phosphate intermediate. Polytetrahydrofuran polyether diol, toluene diisocyanate, and a guanidine-containing pentaerythritol phosphate intermediate are used as raw materials, and a modified waterborne polyurethane dispersion is obtained through reaction, and finally a wetting agent, a defoaming agent, etc. are added to the modified waterborne polyurethane dispersion, and the mixture is stirred evenly to obtain a flame-retardant modified waterborne polyurethane coating.

[0022] The polyurethane coating prepared by the present invention contains a large amount of phosphorus and nitrogen, which are flame retardant elements. When the phosphorus is heated, it can produce strong dehydrating substances such as phosphoric acid and metaphosphoric acid, which can promote the dehydration of the material into carbon, and form a dense carbon layer on the surface of the material to isolate material transportation and energy transfer. When the nitrogen contained therein is heated, it can produce flame-retardant gas, thereby diluting the content of flammable gas in the air and hindering the combustion. The two act synergistically to jointly improve the flame retardant performance of the material.

[0023] In addition, the waterborne polyurethane coating prepared by the present invention contains guanidine groups, and the positive charges contained in the guanidine groups can be adsorbed to the surface of negatively charged microorganisms through electrostatic action, thereby hindering the action of bacterial lysozyme, causing the cell surface structure to denature and then rupture, thereby achieving the purpose of killing bacteria. The waterborne polyurethane coating prepared by the present invention has good antibacterial and flame retardant effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a preparation route for a guanidine-containing pentaerythritol phosphate intermediate. DETAILED DESCRIPTION

[0025] The flame retardant thermoplastic composition, preparation method and application of the present invention are further described below in conjunction with some specific embodiments. The specific embodiments are for further illustrating the present invention in detail, but do not limit the protection scope of the present invention.

[0026] Photoinitiator: photoinitiator 184;

[0027] Wetting agent: Wetting agent 250;

[0028] Leveling agent: leveling agent 3580;

[0029] Defoamer: Defoamer BYK011.

[0030] Example 1

[0031] (1) 0.5 mol of pentaerythritol and 3 mol of phosphorus oxychloride were added to a flask, stirred and dispersed, heated to 80° C., and reacted for 24 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed with ethanol, and dried to obtain intermediate 1.

[0032] (2) 0.2 mol of intermediate 1 and 0.6 mol of p-nitrophenol were added to a flask containing acetonitrile solvent, stirred and dispersed, and then 0.6 mol of triethylamine was added thereto. The temperature was raised to 85° C. and the reaction was carried out for 15 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed with ethanol, and dried to obtain intermediate 2.

[0033] (3) Under nitrogen conditions, 0.1 mol of intermediate 2 and 8 g of Pd / C were added to a flask filled with ethanol solvent, stirred and dispersed, and the temperature was raised to 45°C. Then, 85% by mass of hydrazine hydrate was added thereto, and refluxed for 4 h. After the reaction was completed, the mixture was filtered, rotary evaporated, washed with deionized water, and dried to obtain intermediate 3.

[0034] (4) 0.2 mol of intermediate 3 was added to deionized water, stirred and dispersed, 40% hydrochloric acid aqueous solution was added thereto, stirred and mixed evenly, and then 0.18 mol of dicyandiamide was added thereto, the temperature was raised to 75° C., and the reaction was carried out for 10 hours. After the reaction was completed, the mixture was concentrated, precipitated with acetone, filtered, and dried to obtain a guanidine-containing pentaerythritol phosphate intermediate.

[0035] (5) Under nitrogen conditions, 50 g of polytetrahydrofuran polyether diol and 17.5 g of toluene diisocyanate were added to a flask, and the reaction was carried out at 75° C. for 2 h. Then, 4 g of 2,2-dihydroxymethylpropionic acid was added thereto and the reaction was carried out for 1 h. Then, 1 g of 1,4-butanediol was added thereto and the chain extension reaction was carried out for 2 h. After the reaction was completed, the temperature was lowered to 60° C., 2.5 g of a guanidine-containing pentaerythritol phosphate intermediate was added thereto, the reaction was continued for 60 min, the temperature was lowered to 40° C., and the mixture was stirred and emulsified for 40 min. Finally, 1 g of triethylamine was added thereto for neutralization to obtain a modified waterborne polyurethane dispersion.

[0036] (6) Add 100 g of the modified waterborne polyurethane dispersion into a high-speed mixer and stir to disperse it. Then add 3 g of a photoinitiator, 0.4 g of a wetting agent, 0.5 g of a leveling agent, 0.3 g of a defoaming agent, and 2 g of deionized water. Stir for 18 min at a stirring speed of 1000 r / min to obtain a flame retardant modified waterborne polyurethane coating.

[0037] Example 2

[0038] (1) 0.5 mol of pentaerythritol and 3 mol of phosphorus oxychloride were added to a flask, stirred and dispersed, heated to 90° C., and reacted for 12 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed with ethanol, and dried to obtain intermediate 1.

[0039] (2) 0.2 mol of intermediate 1 and 0.6 mol of p-nitrophenol were added to a flask containing acetonitrile solvent, stirred and dispersed, and then 0.7 mol of triethylamine was added thereto. The temperature was raised to 85° C. and the reaction was carried out for 10 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed with ethanol, and dried to obtain intermediate 2.

[0040] (3) Under nitrogen conditions, 0.1 mol of intermediate 2 and 6 g of Pd / C were added to a flask filled with ethanol solvent, stirred and dispersed, and the temperature was raised to 45°C. Then, 85% by mass of hydrazine hydrate was added thereto, and refluxed for 4 h. After the reaction was completed, the mixture was filtered, rotary evaporated, washed with deionized water, and dried to obtain intermediate 3.

[0041] (4) 0.2 mol of intermediate 3 was added to deionized water, stirred and dispersed, 35% hydrochloric acid aqueous solution was added thereto, stirred and mixed evenly, and then 0.16 mol of dicyandiamide was added thereto, the temperature was raised to 90° C., and the reaction was carried out for 5 hours. After the reaction was completed, the mixture was concentrated, precipitated with acetone, filtered, and dried to obtain a guanidine-containing pentaerythritol phosphate intermediate.

[0042] (5) Under nitrogen conditions, 50 g of polytetrahydrofuran polyether diol and 20 g of toluene diisocyanate were added to a flask, and the reaction was carried out at 75° C. for 2 h. Then, 4 g of 2,2-dihydroxymethylpropionic acid was added thereto and the reaction was carried out for 1 h. Then, 2.5 g of 1,4-butanediol was added thereto and the chain extension reaction was carried out for 1 h. After the reaction was completed, the temperature was lowered to 70° C., 5 g of a guanidine-containing pentaerythritol phosphate intermediate was added thereto, the reaction was continued for 80 min, the temperature was lowered to 40° C., and the mixture was stirred and emulsified for 20 min. Finally, 2 g of triethylamine was added thereto for neutralization to obtain a modified waterborne polyurethane dispersion.

[0043] (6) Add 100 g of the modified waterborne polyurethane dispersion into a high-speed mixer and stir to disperse it. Then add 4 g of a photoinitiator, 0.5 g of a wetting agent, 0.3 g of a leveling agent, 0.2 g of a defoaming agent, and 4 g of deionized water. Stir at a stirring speed of 1000 r / min for 15 min to obtain a flame retardant modified waterborne polyurethane coating.

[0044] Example 3

[0045] (1) 0.5 mol of pentaerythritol and 2.25 mol of phosphorus oxychloride were added to a flask, stirred and dispersed, heated to 75° C., and reacted for 24 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed with ethanol, and dried to obtain intermediate 1.

[0046] (2) 0.2 mol of intermediate 1 and 0.5 mol of p-nitrophenol were added to a flask containing acetonitrile solvent, stirred and dispersed, and then 0.6 mol of triethylamine was added thereto. The temperature was raised to 85° C. and the reaction was carried out for 10 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed with ethanol, and dried to obtain intermediate 2.

[0047] (3) Under nitrogen conditions, 0.1 mol of intermediate 2 and 8 g of Pd / C were added to a flask filled with ethanol solvent, stirred and dispersed, and the temperature was raised to 45°C. Then, 85% by mass of hydrazine hydrate was added thereto, and refluxed for 4 h. After the reaction was completed, the mixture was filtered, rotary evaporated, washed with deionized water, and dried to obtain intermediate 3.

[0048] (4) 0.2 mol of intermediate 3 was added to deionized water, stirred and dispersed, 30% hydrochloric acid aqueous solution was added thereto, stirred and mixed evenly, and then 0.2 mol of dicyandiamide was added thereto, the temperature was raised to 80° C., and the reaction was carried out for 6 hours. After the reaction was completed, the mixture was concentrated, precipitated with acetone, filtered, and dried to obtain a guanidine-containing pentaerythritol phosphate intermediate.

[0049] (5) Under nitrogen conditions, 50 g of polytetrahydrofuran polyether diol and 25 g of toluene diisocyanate were added to a flask, and the reaction was carried out at 80° C. for 2 h. Then, 3 g of 2,2-dihydroxymethylpropionic acid was added thereto and the reaction was carried out for 3 h. Then, 1.5 g of 1,4-butanediol was added thereto and the chain extension reaction was carried out for 1 h. After the reaction was completed, the temperature was lowered to 65° C., 7.5 g of a guanidine-containing pentaerythritol phosphate intermediate was added thereto, the reaction was continued for 40 min, the temperature was lowered to 40° C., and the mixture was stirred and emulsified for 30 min. Finally, 2.5 g of triethylamine was added thereto for neutralization to obtain a modified waterborne polyurethane dispersion.

[0050] (6) Add 100 g of the modified waterborne polyurethane dispersion into a high-speed mixer and stir to disperse it. Then add 2 g of a photoinitiator, 0.5 g of a wetting agent, 0.4 g of a leveling agent, 0.3 g of a defoaming agent, and 2 g of deionized water. Stir at a stirring speed of 900 r / min for 15 min to obtain a flame retardant modified waterborne polyurethane coating.

[0051] Example 4

[0052] (1) 0.5 mol of pentaerythritol and 3 mol of phosphorus oxychloride were added to a flask, stirred and dispersed, heated to 80° C., and reacted for 20 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed with ethanol, and dried to obtain intermediate 1.

[0053] (2) 0.2 mol of intermediate 1 and 0.6 mol of p-nitrophenol were added to a flask filled with acetonitrile solvent, stirred and dispersed, and then 0.8 mol of triethylamine was added thereto. The temperature was raised to 70° C. and the reaction was carried out for 15 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed with ethanol, and dried to obtain intermediate 2.

[0054] (3) Under nitrogen conditions, 0.1 mol of intermediate 2 and 10 g of Pd / C were added to a flask filled with ethanol solvent, stirred and dispersed, and the temperature was raised to 40°C. Then, 85% by mass of hydrazine hydrate was added thereto, and refluxed for 2 h. After the reaction was completed, the mixture was filtered, rotary evaporated, washed with deionized water, and dried to obtain intermediate 3.

[0055] (4) 0.2 mol of intermediate 3 was added to deionized water, stirred and dispersed, 35% hydrochloric acid aqueous solution was added thereto, stirred and mixed evenly, and then 0.18 mol of dicyandiamide was added thereto, the temperature was raised to 80° C., and the reaction was carried out for 6 hours. After the reaction was completed, the mixture was concentrated, precipitated with acetone, filtered, and dried to obtain a guanidine-containing pentaerythritol phosphate intermediate.

[0056] (5) Under nitrogen conditions, 50 g of polytetrahydrofuran polyether diol and 22 g of toluene diisocyanate were added to a flask, and the reaction was carried out at 70° C. for 2 h. Then, 4 g of 2,2-dihydroxymethylpropionic acid was added thereto and the reaction was carried out for 2 h. Then, 2.5 g of 1,4-butanediol was added thereto and the chain extension reaction was carried out for 1.5 h. After the reaction was completed, the temperature was lowered to 65° C., 10 g of a guanidine-containing pentaerythritol phosphate intermediate was added thereto, the reaction was continued for 60 min, the temperature was lowered to 40° C., and the mixture was stirred and emulsified for 30 min. Finally, 2.5 g of triethylamine was added thereto for neutralization to obtain a modified waterborne polyurethane dispersion.

[0057] (6) Add 100 g of the modified waterborne polyurethane dispersion into a high-speed mixer and stir to disperse it. Then add 5 g of a photoinitiator, 0.1 g of a wetting agent, 0.1 g of a leveling agent, 0.2 g of a defoaming agent, and 5 g of deionized water. Stir for 10 min at a stirring speed of 1000 r / min to obtain a flame retardant modified waterborne polyurethane coating.

[0058] Example 5

[0059] (1) 0.5 mol of pentaerythritol and 2.5 mol of phosphorus oxychloride were added to a flask, stirred and dispersed, heated to 80° C., and reacted for 20 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed with ethanol, and dried to obtain intermediate 1.

[0060] (2) 0.2 mol of intermediate 1 and 0.7 mol of p-nitrophenol were added to a flask containing acetonitrile solvent, stirred and dispersed, and then 0.5 mol of triethylamine was added thereto. The temperature was raised to 75° C. and the reaction was carried out for 8 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed with ethanol, and dried to obtain intermediate 2.

[0061] (3) Under nitrogen conditions, 0.1 mol of intermediate 2 and 5 g of Pd / C were added to a flask filled with ethanol solvent, stirred and dispersed, and the temperature was raised to 50° C. Then, 85% by mass of hydrazine hydrate was added thereto, and refluxed for 5 h. After the reaction was completed, the mixture was filtered, rotary evaporated, washed with deionized water, and dried to obtain intermediate 3.

[0062] (4) 0.2 mol of intermediate 3 was added to deionized water, stirred and dispersed, 35% hydrochloric acid aqueous solution was added thereto, stirred and mixed evenly, and then 0.2 mol of dicyandiamide was added thereto, the temperature was raised to 80° C., and the reaction was carried out for 6 hours. After the reaction was completed, the mixture was concentrated, precipitated with acetone, filtered, and dried to obtain a guanidine-containing pentaerythritol phosphate intermediate.

[0063] (5) Under nitrogen conditions, 50 g of polytetrahydrofuran polyether diol and 18 g of toluene diisocyanate were added to a flask, and the reaction was carried out at 75° C. for 2 h. Then, 3.5 g of 2,2-dihydroxymethylpropionic acid was added thereto, and the reaction was carried out for 2 h. Then, 1.5 g of 1,4-butanediol was added thereto, and the chain extension reaction was carried out for 2 h. After the reaction was completed, the temperature was lowered to 65° C., 12.5 g of a guanidine-containing pentaerythritol phosphate intermediate was added thereto, and the reaction was continued for 80 min. The temperature was lowered to 40° C., and the mixture was stirred and emulsified for 30 min. Finally, 2.5 g of triethylamine was added thereto for neutralization to obtain a modified waterborne polyurethane dispersion.

[0064] (6) Add 100 g of the modified waterborne polyurethane dispersion into a high-speed mixer and stir to disperse it. Then add 4 g of a photoinitiator, 0.3 g of a wetting agent, 0.5 g of a leveling agent, 0.1 g of a defoaming agent, and 4 g of deionized water. Stir at a stirring speed of 800 r / min for 20 min to obtain a flame retardant modified waterborne polyurethane coating.

[0065] The coating was poured onto a polytetrafluoroethylene plate and dried at room temperature for 24 hours. It was then placed in a drying oven at 40°C and dried for another 12 hours to obtain a polyurethane coating film.

[0066] Use an oxygen index tester to test the oxygen index of polyurethane coating.

[0067] Table 1: Flame retardant effect test results of various examples

[0068] Oxygen index (%) Example 1 27.9 Example 2 29.1 Example 3 30.4 Example 4 33.6 Example 5 34.8

[0069] It can be seen from the table that the polyurethane coating prepared by the present invention has a relatively excellent flame retardant effect.

[0070] The antibacterial effect of the coating on Escherichia coli was tested by the inhibition zone method. The specific operation is as follows: Escherichia coli was placed in 200mL LB broth medium, incubated at 37℃ for 24h, the suspension was diluted to 106cfu / mL, and then the coating was cut into 12mm small pieces for sterilization. After completion, 200μL of bacterial suspension was taken and applied to PDA flat culture medium, and the coating slice was placed in the center of the culture dish, incubated at 37℃ for 24h, and the diameter of the inhibition zone was measured.

[0071] Table 2: Antibacterial effect test results of each embodiment

[0072] Diameter of inhibition zone (mm) Example 1 21.44 Example 2 24.35 Example 3 27.06 Example 4 29.45 Example 5 30.10

[0073] It can be seen from the table that the polyurethane coating prepared by the present invention has a good antibacterial effect.

[0074] The above-described embodiment is only a preferred solution of the present invention and does not limit the present invention in any form. There are other variations and modifications without exceeding the technical solution described in the claims.

Claims

1. A method for preparing a flame retardant modified waterborne polyurethane coating, characterized in that: The preparation method is as follows: Step (1), under nitrogen conditions, polytetrahydrofuran polyether diol and toluene diisocyanate are added to a flask, reacted at 70-80° C. for 2 hours, then 2,2-dihydroxymethyl propionic acid is added thereto, reacted for 1-3 hours, then 1,4-butanediol is added thereto, chain extension reaction is carried out for 1-2 hours, after the reaction is completed, the temperature is lowered to 60-70° C., a guanidine-containing pentaerythritol phosphate intermediate is added thereto, the temperature is lowered to 40° C., stirred and emulsified for 20-40 minutes, and finally triethylamine is added thereto for neutralization to obtain a modified waterborne polyurethane dispersion; Step (2), adding the modified waterborne polyurethane dispersion into a high-speed stirrer, stirring and dispersing, and then adding a photoinitiator, a wetting agent, a leveling agent, a defoaming agent, and deionized water thereto, stirring at a stirring speed of 800-1000 r / min for 10-20 minutes to obtain a flame retardant modified waterborne polyurethane coating.

2. The method for preparing the flame retardant modified waterborne polyurethane coating according to claim 1, characterized in that: In the step (1), the mass ratio of polytetramethylene glycol, toluene diisocyanate, 2,2-dihydroxymethyl propionic acid, 1,4-butanediol, guanidine-containing pentaerythritol phosphate intermediate, and triethylamine is 100:35-50:6-8:2-5:5-25:2-5.

3. The method for preparing the flame retardant modified waterborne polyurethane coating according to claim 1, characterized in that: In the step (2), the mass ratio of the modified aqueous polyurethane dispersion, the photoinitiator, the wetting agent, the leveling agent, the defoaming agent and the deionized water is 100:2-5:0.1-0.5:0.1-0.5:0.1-0.3:2-5.

4. The method for preparing the flame retardant modified waterborne polyurethane coating according to claim 1, characterized in that: In the step (1), the preparation method of the guanidine-containing pentaerythritol phosphate intermediate is: S1. Add pentaerythritol and phosphorus oxychloride into a flask, stir and disperse, heat to 75-90°C, react for 12-24h, and after the reaction, cool to room temperature, filter, wash with ethanol, and dry to obtain intermediate 1; S2, adding intermediate 1 and p-nitrophenol into a flask filled with acetonitrile solvent, stirring and dispersing, then adding triethylamine, heating to 70-85°C, reacting for 8-15h, after the reaction is completed, cooling to room temperature, filtering, washing with ethanol, and drying to obtain intermediate 2; S3. Under nitrogen conditions, add intermediate 2 and Pd / C to a flask filled with ethanol solvent, stir and disperse, heat to 40-50°C, add 85% by mass of hydrazine hydrate, reflux for 2-5h, filter, rotary evaporate, wash with deionized water, and dry to obtain intermediate 3; S4, adding intermediate 3 to deionized water, stirring and dispersing, adding 30-40% hydrochloric acid aqueous solution thereto, stirring and mixing evenly, adding dicyandiamide thereto, heating to 75-90°C, reacting for 5-10 hours, and after the reaction is completed, concentrating, precipitating with acetone, filtering, and drying to obtain a guanidine-containing pentaerythritol phosphate intermediate.

5. The method for preparing the flame retardant modified waterborne polyurethane coating according to claim 4, characterized in that: In the S1, the molar ratio of pentaerythritol to phosphorus oxychloride is 1:4.5-6.

6. The method for preparing the flame retardant modified waterborne polyurethane coating according to claim 4, characterized in that: In S2, the molar ratio of intermediate 1, p-nitrophenol and triethylamine is 1:2.5-3.5:2.5-4.

7. The method for preparing the flame retardant modified waterborne polyurethane coating according to claim 4, characterized in that: In the S4, the molar ratio of the intermediate 3 to dicyandiamide is 1:0.8-1.

Citation Information

Patent Citations

  • Preparation method of pentaerythritol diphosphite dinitroguanidine salt

    CN102516305A

  • Triazine ring containing caged organic phosphate flame retardant and preparation method thereof

    CN103113619A

  • Phosphorus-nitrogen-silicon-containing titanium dioxide hybrid nanoparticle flame retardant as well as preparation method and application thereof

    CN112521660A

  • Intumescent flame retardant containing triazine ring, and preparation method thereof

    CN113372616A

  • Waterborne polyurethane fireproof coating and preparation process thereof

    CN117363193A

Cited By

  • Preparation method of antibacterial wear-resistant waterborne polyurethane coating

    CN119639328A

  • Flame-retardant aerogel polyurethane thermal insulation material

    CN119684565A

  • Preparation method of antibacterial wear-resistant waterborne polyurethane coating

    CN120464310A