Modified lithium oxide pre-lithiation cathode additive and preparation method thereof, electrode slurry and preparation method thereof, and lithium ion battery

By mixing lithium oxide with a transition metal ion source for high-temperature solid-state reaction, a modified lithium oxide prelithiation cathode additive is prepared, which solves the problem of excessive charging voltage of lithium oxide in lithium-ion batteries and realizes a low charging voltage platform and Improved electrochemical performance with high lithium replenishment capacity.

CN118724023APending Publication Date: 2024-10-01CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410887800.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the prelithiation application of lithium oxide in lithium-ion batteries, the charging voltage is too high, which makes it difficult to activate and release lithium ions, affecting the lithium replenishment effect.

Method used

By mixing lithium oxide and a transition metal ion source for high-temperature solid-state reaction, a modified lithium oxide prelithiation cathode additive is prepared, and impurity doping of transition metal elements is introduced to reduce the charging platform voltage and increase the lithium replenishment capacity.

Benefits of technology

It achieves a low charging voltage platform and high lithium replenishing capacity for lithium oxide, enhances the electrochemical performance of lithium-ion batteries, and is compatible with existing battery charging and discharging mechanisms.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724023A_ABST
    Figure CN118724023A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a modified lithium oxide pre-lithiation cathode additive, which comprises the following steps: mixing and grinding lithium oxide and a transition metal ion source to obtain a mixture; carrying out high-temperature solid-phase reaction on the mixture in an inert atmosphere to obtain a sintered product; and cooling and post-processing the sintered product to obtain the modified lithium oxide pre-lithiation cathode additive. The invention also provides the modified lithium oxide pre-lithiation cathode additive prepared by the preparation method. The transition metal ion doped lithium oxide prepared by the invention has excellent performances of low charging voltage platform, high lithium supplement capacity and the like, is an excellent cathode additive, and can be applied to lithium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion batteries, and in particular relates to the modification of lithium oxide pre-lithiation cathode additives. Background Art

[0002] The low energy density of the positive electrode is one of the key challenges that currently restricts the development of lithium-ion battery technology. In addition to being limited by the theoretical energy density of the positive electrode active material, during the first charge of the battery, lithium ions and the electrolyte react at the interface between the negative electrode and the electrolyte to form an SEI film, causing irreversible capacity loss, affecting the battery's energy density and cycle life. However, the current large-capacity new negative electrode materials such as silicon-based negative electrodes generally have a first coulomb efficiency that is much lower than that of traditional carbon-based negative electrodes, which means that the irreversible lithium loss during the first charge of the battery is more serious. Pre-lithiation technology is designed to improve this problem.

[0003] According to the different locations of lithium ion replenishment, it is divided into two major technologies: anode pre-lithiation and cathode pre-lithiation. Compared with anode pre-lithiation, the advantage of cathode pre-lithiation lies mainly in the high compatibility of production processes. It only needs to be added to the cathode material as an additive. During the first charging of the battery, excess lithium ions escape from the cathode and pass through the diaphragm. Initially, a part of them participates in the formation of SEI film on the anode surface and is consumed, avoiding the loss of reversible lithium ions in the cathode material. As one of the cathode pre-lithiation additives, lithium oxide has the greatest advantage of a theoretical lithium replenishment capacity of up to 1793.9 mAh / g and a high irreversibility of the lithium replenishment reaction. However, in actual pre-lithiation applications, lithium oxide also has the problem of too high a charging voltage, making it difficult for lithium ions to activate and release, and it is difficult to exert the lithium replenishment effect under the existing battery charging and discharging mechanism. Summary of the invention

[0004] In response to the above technical problems, the present application provides a modified lithium oxide pre-lithiation cathode additive and a preparation method thereof, an electrode slurry and a preparation method thereof, and a lithium-ion battery.

[0005] To achieve the above objectives, this application proposes the following technical solutions: In a first aspect, a method for preparing a modified lithium oxide pre-lithiation cathode additive is provided, comprising: S1, mixing and grinding lithium oxide and a transition metal ion source to obtain a mixture; S2. subjecting the mixture to a high-temperature solid-phase reaction under an inert atmosphere to obtain a sintered product; the sintered product is cooled and post-processed to obtain a modified lithium oxide pre-lithiation cathode additive.

[0006] Furthermore, the transition metal ion source and lithium oxide are mixed in a mass ratio of 1:99 to 3:5.

[0007] Furthermore, the transition metal ion source is selected from one or more of a nickel source, a cobalt source, and an iron source; the particle size of the transition metal source is D50 not greater than 10 μm; the nickel source is selected from one or more of NiO, Li2NiO2, and LiNiO2; the cobalt source is selected from one or more of Co3O4, Co2O3, LiCoO2, and Co3(PO4)2; the iron source is selected from one or more of FeO, Fe3O4, and Li5FeO4.

[0008] Furthermore, in step S1, the temperature of the high temperature solid phase reaction is 650-950° C.; and the time of the high temperature solid phase reaction is 8-10 hours.

[0009] Furthermore, in step S1, the mixed grinding is dry ball milling.

[0010] Furthermore, in step S1, an inert atmosphere is always maintained in the grinding tank during the mixed grinding.

[0011] Furthermore, in step S1, the rotation speed of the mixed grinding is 350-1000 rpm.

[0012] Furthermore, in step S1, the mixed grinding is intermittent grinding; preferably, in step S1, the mixed grinding is performed for 900-1200 min according to a procedure of working for 1-20 min and resting for 1-15 min.

[0013] Furthermore, in step S2, the post-processing includes the steps of crushing, grinding and screening the cooled product.

[0014] Furthermore, in step S2, the grinding is dry ball milling.

[0015] Furthermore, in step S2, the grinding speed is 350-1000 rpm.

[0016] Furthermore, in step S2, the grinding is intermittent grinding; preferably, in step S2, the grinding is performed for 100 to 200 minutes according to a procedure of working for 1 to 20 minutes and resting for 1 to 20 minutes.

[0017] Furthermore, in step S2, the sieve mesh specification is 200-400 mesh; the particle size of the modified lithium oxide pre-lithiation cathode additive is 200-400 mesh.

[0018] In a second aspect, a modified lithium oxide pre-lithiation cathode additive is provided, which is prepared using the aforementioned preparation method.

[0019] In a third aspect, a method for preparing an electrode slurry is provided, comprising: mixing the aforementioned modified lithium oxide pre-lithiation cathode additive, positive electrode active material, conductive agent, binder and organic solvent into a slurry to obtain an electrode slurry; the binder is a sol prepared by adding hydrogenated nitrile rubber to an organic solvent.

[0020] Furthermore, the positive electrode active material includes but is not limited to at least one of lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, and lithium nickel cobalt manganese oxide.

[0021] Furthermore, in the sol, the mass fraction of hydrogenated nitrile rubber is 5-8wt.%.

[0022] Furthermore, the organic solvent includes but is not limited to N-methylpyrrolidone.

[0023] In a fourth aspect, an electrode slurry is provided, which is prepared using the aforementioned preparation method.

[0024] In a fifth aspect, a lithium-ion battery is provided, comprising the aforementioned modified lithium oxide pre-lithiation cathode additive or an electrode prepared by the aforementioned electrode slurry.

[0025] Compared with the prior art, one or more of the above technical solutions can achieve at least one of the following beneficial effects: The present application uses transition metal oxides or lithium transition metal oxides as dopants to mix with lithium oxide, and a transition metal ion-doped modified lithium oxide pre-lithiation cathode additive can be prepared through a high-temperature solid phase reaction. Using transition metal oxides or lithium transition metal oxides as dopants, the impurity doping energy level of the transition metal element is introduced to produce a catalytic effect, which is beneficial to solving the problem of excessively high lithium release voltage of lithium oxide. The use of ball milling technology to fully premix and subsequently crush the raw materials is beneficial to increase the contact area between the reactants so that the doping reaction can proceed fully. The transition metal ion-doped lithium oxide prepared by this method has excellent properties such as a low charging voltage platform and a high lithium replenishment capacity.

[0026] Further crushing and grinding the pre-lithiation additive obtained by the high-temperature solid-phase reaction can avoid the problem of coating difficulty caused by excessively large particles, further improve the kinetics of the positive electrode reaction, and reduce the lithium release voltage of lithium oxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1The X-ray diffraction patterns of the materials prepared in Example 1 and the comparative example are shown.

[0029] Figure 2 First charge curves of button batteries assembled with materials prepared in Example 1 and Comparative Example 1.

[0030] Figure 3 First charge curve of button batteries assembled with materials prepared in Example 6 and Comparative Example 2.

[0031] Figure 4 First charge curve of button batteries assembled with materials prepared in Example 7 and Comparative Example 3. DETAILED DESCRIPTION

[0032] In view of the problem that the lithium oxide release voltage is too high and the lithium replenishment effect is poor when lithium oxide is used as a pre-lithiation cathode additive, or lithium oxide and transition metal oxide are mixed as pre-lithiation cathode additives, the applicant has found through research that the modified lithium oxide pre-lithiation cathode additive obtained by mixing lithium oxide with a transition metal ion source and grinding it and then performing high-temperature heat treatment has the excellent performance of low charging voltage platform and high lithium replenishment capacity. Based on this, the present invention is completed.

[0033] The present invention provides a method for preparing a modified lithium oxide pre-lithiation cathode additive, comprising: S1, mixing and grinding lithium oxide and a transition metal ion source to obtain a mixture; S2. subjecting the mixture to a high-temperature solid-phase reaction under an inert atmosphere to obtain a sintered product; the sintered product is cooled and post-processed to obtain a modified lithium oxide pre-lithiation cathode additive.

[0034] In some preferred embodiments, the transition metal ion source and lithium oxide are mixed in a mass ratio of 1:99 to 3:5.

[0035] In order to enhance the reactivity of the process of lithium oxide releasing lithium ions and reduce the charging platform voltage of pre-lithiation, a catalyst is introduced to reduce the activation energy required for the reaction. However, studies have found that simple solid-phase mixing may be limited by the contact area between the catalyst and the lithium oxide and is difficult to play a catalytic role. The present invention utilizes transition metal elements to be doped into the lithium oxide lattice to directly modify the physical and chemical properties of lithium oxide. The doping energy level can play a catalytic role, reduce the difficulty of the reaction, and thus reduce the charging platform voltage of pre-lithiation, making it one step closer to actual production application.

[0036] A transition metal ion source with a particle size that is too large will result in uneven distribution of the transition metal elements in lithium oxide, affecting the catalytic performance; in some preferred embodiments, the transition metal ion source is selected from one or more of a nickel source, a cobalt source, and an iron source; the particle size of the transition metal source is not greater than 10 μm.

[0037] In some preferred embodiments, the nickel source is selected from one or more of NiO, Li2NiO2, and LiNiO2; the cobalt source is selected from one or more of Co3O4, Co2O3, LiCoO2, and Co3(PO4)2; and the iron source is selected from one or more of FeO, Fe3O4, and Li5FeO4.

[0038] In some preferred embodiments, in step S1, the temperature of the high temperature solid phase reaction is 650-950°C; the time of the high temperature solid phase reaction is 8-10 hours; and the heating rate is 1-2°C / min.

[0039] It has been found that when an inert solvent such as NMP, DMC, ethanol, etc. is used as a solvent for wet grinding, the phase will change. In some preferred embodiments, in step S1, the mixed grinding is dry ball milling; during the grinding, an inert atmosphere is always maintained in the grinding tank.

[0040] In some preferred embodiments, in step S1, the rotation speed of the mixing and grinding is 350-1000 pm.

[0041] In some preferred embodiments, in step S1, the mixed grinding is performed by intermittent grinding. The applicant has found through research that intermittent grinding is beneficial to avoiding agglomeration and improving material uniformity; the intermittent grinding is performed for 900 to 1200 minutes according to a procedure of working for 1 to 20 minutes and resting for 1 to 15 minutes; further preferably, the grinding is performed for 900 to 1200 minutes according to a procedure of working for 6 to 10 minutes and resting for 4 to 8 minutes.

[0042] In some preferred embodiments, in step S2, the post-treatment includes the steps of crushing, grinding and sieving the cooling product. Further crushing, grinding and sieving the obtained cooling product can avoid the problem of coating difficulty caused by excessive particle size, improve the kinetics of the positive electrode reaction, and reduce the lithium release voltage of lithium oxide.

[0043] In some preferred embodiments, in step S2, the grinding is dry ball milling.

[0044] In some preferred embodiments, in step S2, the grinding speed is 350-1000 rpm.

[0045] In some preferred embodiments, in step S2, the grinding is performed by intermittent grinding; the intermittent grinding is performed for 100 to 200 minutes according to a procedure of working for 1 to 20 minutes and resting for 1 to 20 minutes; further preferably, the grinding is performed for 100 to 200 minutes according to a procedure of working for 6 to 10 minutes and resting for 4 to 8 minutes.

[0046] In some preferred embodiments, in step S2, the sieve mesh specification is 200-400 mesh.

[0047] In some preferred embodiments, in step S2, the particle size of the modified lithium oxide pre-lithiation cathode additive is 200-400 mesh.

[0048] Some embodiments of the present invention provide a method for preparing an electrode slurry, comprising: mixing the aforementioned modified lithium oxide pre-lithiation cathode additive, positive electrode active material, conductive agent, binder and organic solvent into a slurry to obtain an electrode slurry; the binder is a sol prepared by adding hydrogenated nitrile rubber to an organic solvent.

[0049] The positive electrode active material includes but is not limited to at least one of lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, and lithium nickel cobalt manganese oxide.

[0050] Furthermore, in the sol, the mass fraction of hydrogenated nitrile rubber is 5-8wt.%.

[0051] Furthermore, the organic solvent includes but is not limited to N-methylpyrrolidone.

[0052] Some embodiments of the present invention provide electrode slurry, which is prepared by the aforementioned preparation method.

[0053] Some embodiments of the present invention provide a modified lithium oxide pre-lithiation cathode additive, which is prepared using the aforementioned preparation method.

[0054] A lithium-ion battery, characterized in that it comprises the aforementioned modified lithium oxide pre-lithiation cathode additive.

[0055] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the specification, but the protection scope of the present invention is not limited to the following specific embodiments.

[0056] Example 1 A method for preparing a pre-lithiation cathode additive comprises the following steps: Step S1: Mix and grind lithium oxide and NiO (30 nm) at a mass ratio of 98:2. In step S1, the nickel source selected is NiO, and one or more of Li2NiO2 and LiNiO2 can also be selected. In this step, the mixing method preferably adopts ball milling, which is a grinding method that achieves material crushing by impact, extrusion and friction of grinding balls. Generally speaking, dry ball milling sets the ball-to-material ratio to 10:1, and the rotation speed is 400 rpm, and the program of working for 6 min and resting for 4 min is ground for 1040 min.

[0057] Step S2: subjecting the mixed and ground materials in step S1 to a high-temperature solid phase reaction in an argon atmosphere, heating the temperature to 850° C. at a rate of 1° C. / min and continuing for 8 h to obtain a nickel-ion-doped lithium oxide composite solid material; Step S3: Cool, crush, grind and sieve the composite solid material after the high-temperature solid phase reaction in step S2 to obtain a nickel-ion-doped lithium oxide pre-lithiation cathode additive. The grinding process in this step is dry ball milling with a ball-to-material ratio of 10:1, and the rotation speed is 400 rpm, working for 6 min and resting for 4 min for 200 min. The ground powder is passed through a 300-mesh sieve. In this step, the sieve used for screening is preferably 300 mesh. Of course, any one of 200, 250, 350, and 400 mesh can also be selected. The selection of these types of sieves will not destroy the structure of nickel-ion-doped lithium oxide during the screening process, and the best screening result can be achieved.

[0058] Comparative Example 1 Li2O and Li2NiO2 (D50≤8 μm) were manually ground and mixed at the same Li / Ni molar ratio as in Example 1, i.e., at a mass ratio of Li2O to Li2NiO2 of 243:7, to obtain a mixed material.

[0059] Example 2 A method for preparing a pre-lithiation cathode additive comprises the following steps: Step S1: Lithium oxide and NiO (30 nm) are mixed and ground at a mass ratio of 97:3. In this step, the mixing method is preferably dry ball milling, and the ball-to-material ratio is set to 10:1, and the grinding is carried out at a speed of 400 rpm, working for 6 minutes and resting for 4 minutes for 1040 minutes.

[0060] Step S2: subjecting the mixed and ground materials in step S1 to a high-temperature solid phase reaction in an argon atmosphere, heating the temperature to 650° C. at a rate of 1° C. / min and continuing for 7 h to obtain a nickel-ion-doped lithium oxide composite solid material; Step S3: Cool, crush, grind and sieve the composite solid material after the high temperature solid phase reaction in step S2 to obtain a nickel ion-doped lithium oxide pre-lithiation cathode additive. The grinding process in this step is dry ball milling with a ball-to-material ratio of 10:1, and the grinding process is performed at a speed of 400 rpm, working for 6 minutes and resting for 4 minutes for 200 minutes. The ground powder is passed through a 300 mesh screen.

[0061] Example 3 A method for preparing a pre-lithiation cathode additive comprises the following steps: Step S1: Lithium oxide and NiO (30 nm) are mixed and ground at a mass ratio of 97:3. In this step, the mixing method is preferably dry ball milling, and the ball-to-material ratio is set to 10:1, and the grinding is carried out at a speed of 400 rpm, working for 6 minutes and resting for 4 minutes for 1040 minutes.

[0062] Step S2: subjecting the mixed and ground materials in step S1 to a high-temperature solid phase reaction in an argon atmosphere, heating the temperature to 650° C. at a rate of 1° C. / min and continuing for 8 h to obtain a nickel-ion-doped lithium oxide composite solid material; Step S3: Cool, crush, grind and sieve the composite solid material after the high temperature solid phase reaction in step S2 to obtain a nickel ion-doped lithium oxide pre-lithiation cathode additive. The grinding process in this step is dry ball milling with a ball-to-material ratio of 10:1, and the grinding process is performed at a speed of 400 rpm, working for 6 minutes and resting for 4 minutes for 200 minutes. The ground powder is passed through a 300 mesh screen.

[0063] Example 4 A method for preparing a pre-lithiation cathode additive comprises the following steps: Step S1: Lithium oxide and NiO (30 nm) are mixed and ground at a mass ratio of 97:3. In this step, the mixing method is preferably dry ball milling, and the ball-to-material ratio is set to 10:1, and the grinding is carried out at a speed of 400 rpm, working for 6 minutes and resting for 4 minutes for 1040 minutes.

[0064] Step S2: subjecting the mixed and ground materials in step S1 to a high-temperature solid-phase reaction in an argon atmosphere, heating the temperature to 650° C. at a rate of 1° C. / min and continuing for 10 h to obtain a nickel-ion-doped lithium oxide composite solid material; Step S3: Cool, crush, grind and sieve the composite solid material after the high temperature solid phase reaction in step S2 to obtain a nickel ion-doped lithium oxide pre-lithiation cathode additive. The grinding process in this step is dry ball milling with a ball-to-material ratio of 10:1, and the grinding process is performed at a speed of 400 rpm, working for 6 minutes and resting for 4 minutes for 200 minutes. The ground powder is passed through a 300 mesh screen.

[0065] Example 5 A method for preparing a pre-lithiation cathode additive comprises the following steps: Step S1: Lithium oxide and Co3O4 (30 nm) are mixed and ground in a mass ratio of 5:3. In this step, the mixing method is preferably dry ball milling, and the ball-to-material ratio is set to 10:1, and the grinding is carried out at a speed of 400 rpm, working for 6 minutes and resting for 4 minutes for 1200 minutes.

[0066] Step S2: subjecting the mixed and ground materials in step S1 to a high-temperature solid phase reaction in an argon atmosphere, heating the temperature to 950° C. at a rate of 2° C. / min and continuing for 9 h to obtain a cobalt ion-doped lithium oxide composite solid material; Step S3: Cool, crush, grind and sieve the composite solid material after the high temperature solid phase reaction in step S2 to obtain a cobalt ion-doped lithium oxide pre-lithiation cathode additive. The grinding process in this step is dry ball milling with a ball-to-material ratio of 10:1, and the speed is 400 rpm for 6 minutes and rest for 4 minutes for 120 minutes. The ground powder is passed through a 300 mesh screen.

[0067] Example 6 The main difference between this embodiment and embodiment 5 is that the cobalt source is different and the proportion of each substance is also different. The other points not mentioned are the same as those of embodiment 5. The preparation method comprises the following steps: Step S1: Lithium oxide and LiCoO2 (8 μm) are mixed and ground at a mass ratio of 5:2. In this step, the mixing method is preferably dry ball milling, and the ball-to-material ratio is set to 10:1, and the grinding is carried out at a speed of 400 rpm, working for 6 minutes and resting for 4 minutes for 1200 minutes.

[0068] Step S2: subjecting the mixed and ground materials in step S1 to a high-temperature solid phase reaction in an argon atmosphere, heating the temperature to 950° C. at a rate of 2° C. / min and continuing for 9 h to obtain a cobalt ion-doped lithium oxide composite solid material; Step S3: Cool, crush, grind and sieve the composite solid material after the high temperature solid phase reaction in step S2 to obtain a cobalt ion-doped lithium oxide pre-lithiation cathode additive. The grinding process in this step is dry ball milling with a ball-to-material ratio of 10:1, and the speed is 400 rpm for 6 minutes and rest for 4 minutes for 120 minutes. The ground powder is passed through a 300 mesh screen.

[0069] Comparative Example 2 Li2O and Li6CoO4 (D50≤8 μm) were manually ground and mixed at the same Li / Co molar ratio as in Example 6, i.e., at a mass ratio of Li2O to Li6CoO4 of 103:100, to obtain a mixed material.

[0070] Example 7 A method for preparing a pre-lithiation cathode additive comprises the following steps: Step S1: Lithium oxide and Fe3O4 (30 nm) are mixed and ground in a mass ratio of 5:2. In this step, the mixing method is preferably dry ball milling, and the ball-to-material ratio is set to 10:1, and the grinding is carried out at a speed of 400 rpm, working for 6 minutes and resting for 4 minutes for 1200 minutes.

[0071] Step S2: subjecting the mixed and ground materials in step S1 to a high-temperature solid phase reaction in an argon atmosphere, heating the temperature to 950° C. at a rate of 2° C. / min and continuing for 9 h to obtain an iron ion-doped lithium oxide composite solid material; Step S3: Cool, crush, grind and sieve the composite solid material after the high temperature solid phase reaction in step S2 to obtain an iron ion doped lithium oxide pre-lithiation cathode additive. The grinding process in this step is dry ball milling with a ball-to-material ratio of 10:1, and the speed is 400 rpm for 6 minutes and rest for 4 minutes for 120 minutes. The ground powder is passed through a 300 mesh screen.

[0072] Comparative Example 3 Li2O and Li5FeO4 (D50≤8 μm) were manually ground and mixed at the same Li / Fe molar ratio as in Example 7, i.e., at a mass ratio of Li2O to Li5FeO4 of 206.4:309, to obtain a mixed material.

[0073] Example 8 A method for preparing a pre-lithiation cathode additive comprises the following steps: Step S1: Lithium oxide and FeO (50 nm) are mixed and ground in a mass ratio of 5:3. In this step, the mixing method is preferably dry ball milling, and the ball-to-material ratio is set to 10:1, and the grinding is carried out at a speed of 400 rpm, working for 6 min and resting for 4 min for 1200 min.

[0074] Step S2: subjecting the mixed and ground materials in step S1 to a high-temperature solid phase reaction in an argon atmosphere, heating the temperature to 950° C. at a rate of 2° C. / min and continuing for 9 h to obtain an iron ion-doped lithium oxide composite solid material; Step S3: Cool, crush, grind and sieve the composite solid material after the high temperature solid phase reaction in step S2 to obtain an iron ion doped lithium oxide pre-lithiation cathode additive. The grinding process in this step is dry ball milling with a ball-to-material ratio of 10:1, and the speed is 400 rpm for 6 minutes and rest for 4 minutes for 120 minutes. The ground powder is passed through a 300 mesh screen.

[0075] The samples obtained in each embodiment and comparative example were assembled into lithium button half-cells according to the following method: Preparation of electrode slurry: HNBR (hydrogenated nitrile rubber) was added to NMP (N-methylpyrrolidone) at 6 wt.% to prepare NMP sol of HNBR; the active material prepared in each embodiment, Super P and binder (NMP sol of HNBR) were mixed into slurry at a mass ratio of 6:3:1, and NMP solvent was added to adjust the viscosity to an appropriate viscosity for electrode slurry preparation to obtain electrode slurry.

[0076] Battery assembly: Scrape the slurry onto the surface of aluminum foil, dry it in an inert atmosphere, and punch it into a 10 mm diameter electrode (loading is 0.8-1.3 mg / cm 2 ) and assemble a pair of lithium button half-cells in the order of positive electrode shell, positive electrode sheet, separator, lithium metal sheet, gasket, spring and negative electrode shell.

[0077] The prepared lithium button half-cell was subjected to the positive electrode first charge capacity test at 25°C, in the voltage range of 2-5V, and at 0.1C. The test results are shown in Table 1.

[0078] Table 1 Group First charge specific capacity (mAh / g) Charging platform voltage (V) Example 1 1104 4.00 Example 2 1155 3.97 Example 3 1198 4.01 Example 4 1048 3.92 Example 5 1006 4.25 Example 6 931 4.23 Example 7 472 4.12 Example 8 206 4.09 Comparative Example 1 40 No typical charging platform Comparative Example 2 60 No typical charging platform Comparative Example 3 33 No typical charging platform It can be seen from the data in Table 1 that the transition metal ion-doped lithium oxide described in Examples 1-8 has significantly improved electrochemical performance compared to the cathode battery using pure lithium oxide in the comparative example, and the theoretical lithium replenishment capacity of lithium oxide is fully utilized, with the nickel-based lithium replenishment capacity being >1000 mAh / g, the cobalt-based lithium replenishment capacity being >900 mAh / g, and the iron-based lithium replenishment capacity being >400 mAh / g. At the same time, the three element dopings all have a lower charging platform voltage (<4.3 V), which is compatible with the existing battery charging and discharging mechanism, which fully demonstrates that the doping of transition metal ions makes it easier for lithium oxide to release lithium ions.

[0079] Figure 1 They are the X-ray diffraction patterns of the materials prepared in Example 1 and Comparative Example 1, respectively. It can be seen from the figures that the prepared materials correspond to two phases of Li2O and Li2NiO2, and the diffraction peaks of each crystal plane of lithium oxide in Example 1 are shifted by 0.2~0.3° to the large angle direction as a whole, indicating that the nickel element is doped into the lithium oxide lattice in Example 1, and the nickel ion radius is smaller than the lithium ion radius. This doping causes the lithium oxide unit cell parameters to become smaller.

[0080] from Figure 2 From the first charging curve at 25°C@0.1C, it can be analyzed that the charging platform of the battery assembled in Example 1 is about 4.0 V, and the first lithium replenishment charging capacity reaches 1104 mAh / g. However, the electrochemical curve measured by the battery assembled with simply mixed materials shows that there is almost no lithium replenishment effect at a cut-off voltage of 4.3V.

[0081] from Figure 3From the first charging curve at 25°C@0.1C, it can be analyzed that the charging platform of the battery assembled in Example 6 is about 4.2 V, and the first lithium replenishment charging capacity reaches 931 mAh / g. However, the electrochemical curve measured by the battery assembled with simply mixed materials shows that there is almost no lithium replenishment effect at a cutoff voltage of 4.3V.

[0082] from Figure 4 From the first charging curve at 25°C@0.1C, it can be analyzed that the charging platform of the battery assembled in Example 7 is about 4.1 V, and the first lithium replenishment charging capacity reaches 472 mAh / g. However, the electrochemical curve measured by the battery assembled with simply mixed materials shows that there is almost no lithium replenishment effect at a cut-off voltage of 4.3V.

[0083] From the comparison of the first charging curves of the above-mentioned embodiments and comparative examples, it can be found that the battery assembled by the samples prepared in each embodiment has a significantly higher charging capacity than the battery assembled by the mixed sample of lithium oxide and the corresponding lithium metal oxide lithium supplement material, and the batteries assembled in each embodiment have a clear charging platform, while the mixture does not exist. The reasons for this phenomenon may be: on the one hand, the lattice doping of lithium oxide by a part of the transition metal ion source is achieved through high-temperature solid-phase reaction, which can reduce the lithium supplement charging platform voltage of lithium oxide. After the initial release of lithium, the valence state of the transition metal element of the lithium-rich transition metal oxide generated by the reaction of the remaining part of the transition metal and lithium oxide increases to form a local catalytic center, further enhancing the reaction activity of the lattice oxygen in the lithium oxide, so that the high theoretical lithium supplement capacity of the lithium oxide can be activated and exerted; on the other hand, the ball milling technology is used to fully premix and subsequently crush the precursor, which is conducive to increasing the contact area between the reactants to fully carry out the doping reaction and improve the kinetics of the positive electrode reaction.

[0084] Furthermore, through the analysis of the electrochemical data of the assembled batteries in each embodiment to determine the influence of various factors on the electrochemical properties of the materials, it was found that the order of influence on the electrochemical properties of the materials from large to small is the type of transition metal ions, high-temperature solid-phase reaction temperature, high-temperature solid-phase reaction time, and the ratio of lithium to transition metal elements.

[0085] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a modified lithium oxide pre-lithiation cathode additive, characterized in that: include: S1, mixing and grinding lithium oxide and a transition metal ion source to obtain a mixture; S2, subjecting the mixture to a high-temperature solid-phase reaction under an inert atmosphere to obtain a sintered product; The sintered product is cooled and post-treated to obtain a modified lithium oxide pre-lithiation cathode additive.

2. The method for preparing the modified lithium oxide pre-lithiation cathode additive according to claim 1, characterized in that: The transition metal ion source and lithium oxide are mixed in a mass ratio of 1:99 to 3:5; Preferably, the transition metal ion source is selected from one or more of a nickel source, a cobalt source, and an iron source; preferably, the nickel source, the cobalt source, and the iron source are oxides or lithium transition metal oxides; Preferably, the nickel source is selected from one or more of NiO, Li2NiO2, LiNiO2; preferably, the cobalt source is selected from one or more of Co3O4, Co2O3, LiCoO2, Co3(PO4)2; preferably, the iron source is selected from one or more of FeO, Fe3O4, Li5FeO4; Preferably, the particle size D50 of the transition metal source is not greater than 10 μm.

3. The method for preparing the modified lithium oxide pre-lithiation cathode additive according to claim 1 or 2, characterized in that: In step S1, the temperature of the high temperature solid phase reaction is 650-950° C.; and the time of the high temperature solid phase reaction is 8-10 hours.

4. The method for preparing the modified lithium oxide pre-lithiation cathode additive according to claim 1 or 2, characterized in that: In step S1, the mixed grinding is dry ball milling; Preferably, in step S1, an inert atmosphere is always maintained in the grinding tank during the mixed grinding; Preferably, in step S1, the rotation speed of the mixed grinding is 350-1000 rpm; Preferably, in step S1, the mixed grinding is intermittent grinding; Preferably, in step S1, the mixed grinding is carried out for 900-1200 min according to a procedure of working for 1-20 min and resting for 1-15 min.

5. The method for preparing the modified lithium oxide pre-lithiation cathode additive according to claim 1 or 2, characterized in that: In step S2, the post-processing includes the steps of crushing, grinding and screening the cooled product; Preferably, in step S2, the grinding is dry ball milling; Preferably, in step S2, the grinding speed is 350-1000 rpm; Preferably, in step S2, the grinding is intermittent grinding; Preferably, in step S2, the grinding is performed for 100 to 200 minutes according to a procedure of working for 1 to 20 minutes and resting for 1 to 20 minutes; Preferably, in step S2, the sieve mesh specification is 200-400 mesh; the particle size of the modified lithium oxide pre-lithiation cathode additive is 200-400 mesh.

6. A modified lithium oxide pre-lithiation cathode additive, characterized in that: The method is prepared by any one of claims 1 to 5.

7. A method for preparing an electrode slurry, characterized in that: include: The modified lithium oxide pre-lithiation cathode additive according to claim 6, the positive electrode active material, the conductive agent, the binder and the organic solvent are mixed into a slurry to obtain an electrode slurry; the binder is a sol prepared by adding hydrogenated nitrile rubber to an organic solvent.

8. The method for preparing the electrode slurry according to claim 7, characterized in that: In the sol, the mass fraction of hydrogenated nitrile rubber is 5-8wt.%; The organic solvent is N-methylpyrrolidone. The positive electrode active material is at least one of lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, and nickel cobalt lithium manganese oxide.

9. An electrode slurry, characterized in that: The product is prepared by the preparation method as claimed in claim 7 or 8.

10. A lithium ion battery, characterized in that An electrode comprising the modified lithium oxide pre-lithiation cathode additive as claimed in claim 6 or comprising the electrode slurry as claimed in claim 9.