Positive electrode material magnesium gallate of rechargeable magnesium battery, and preparation method and application of positive electrode material magnesium gallate
Preparing cubic phase spinel magnesium gallate through a low-temperature combustion method solves the problems of low specific capacity and poor cycle performance of magnesium battery cathode materials, achieves high specific capacity and good cycle stability, and significantly improves the power of magnesium batteries. chemical properties.
Patent Information
- Application Number
- CN202410720902.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-01
AI Technical Summary
The cathode material of magnesium batteries has low specific capacity and poor cycle performance, which causes the specific capacity of magnesium batteries to decay rapidly during cycling.
After grinding hexahydrated magnesium nitrate, hydrated gallium nitrate and urea using a low-temperature combustion method, the temperature is raised to 400-600°C to prepare high crystallinity, fine-grained cubic phase spinel type magnesium gallate (MgGa2O4) as magnesium Battery cathode material.
It has achieved a high specific capacity of 210mAh g-1 and good cycle stability of magnesium gallate at a current density of 50mA g-1. It can maintain stable cycle performance for more than 70 cycles, which is better than similar spinel-type magnesium oxide cathode materials. .
Smart Images

Figure CN118724049A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of battery materials, and in particular relates to a cubic spinel-type magnesium gallate having good electrochemical performance obtained by a low-temperature combustion method and its application in the field of battery materials. Background Art
[0002] Magnesium battery is a new type of battery with great potential that has been developed in recent years. Compared with lithium, magnesium resources are extremely abundant. According to statistics, the world's magnesite resources are about 12 billion tons, and the magnesium content in seawater is estimated to be 6×10 16 Tons, in addition to a large amount of dolomite and salt lake magnesium resources. The rich reserves of magnesium give it a competitive advantage in terms of cost, and its high energy density (3833mAh cm -3 Compared with lithium metal 2046mAh cm -3 ) also makes magnesium batteries an ideal choice to replace lithium-ion batteries. In addition, magnesium ions are not easy to produce dendrites when deposited on the negative electrode, and are safer than lithium batteries. In-depth research on magnesium-ion battery technology will not only help promote the development of the energy field, but also is expected to make important contributions to solving global challenges such as environmental and energy security.
[0003] At present, the main research direction of positive electrode materials for magnesium-ion batteries is to explore materials that can reversibly insert and deintercalate magnesium ions and can stably exist in the electrolyte. Common positive electrode material choices include inorganic transition metal oxides, sulfides, borides, phosphates and other compounds. The spinel structure composite oxides (chemical formula: AB2O4) in metal oxides have the advantages of high working voltage and stable three-dimensional ion migration skeleton, which is conducive to the reversible deintercalation of magnesium ions. Studies have shown that MgCo2O4, MgMn2O4, MgFe2O4 and MgCr2O4 can all be used as positive electrode materials for magnesium batteries. "Gu, S., Hsieh, CT., Huq, MMet al. Preparation of MgCo2O4 / graphite composites as cathode materialsfor magnesium-ion batteries. J Solid State Electrochem 23, 1399–1407 (2019)" mentions a magnesium-ion battery with MgCo2O4 as the positive electrode material, which has 180mAh g -1 The initial capacity can be maintained at about 85% after 30 charge and discharge cycles.
[0004] Due to its solid-liquid dual-phase properties at room temperature, Ga metal can achieve high current cycles and high-rate charge and discharge as a negative electrode. Although magnesium-ion battery positive electrode materials have been widely studied, most of them are based on magnesium manganese oxide spinel positive electrode materials, which are lithium battery positive electrode materials. Magnesium gallium oxide is rarely used in lithium batteries, so there is almost no in-depth discussion on Ga composite oxides in lithium batteries and even magnesium batteries. Ga oxide Ga2O3 is a wide bandgap semiconductor material with unique conductive properties. Therefore, the research on Mg and Ga composite oxide positive electrode materials for magnesium-ion batteries has great theoretical and practical significance and is expected to fill the gap in research in this field. At present, the magnesium-manganese oxide positive electrode material MgMn2O4 for magnesium-ion batteries shows 150mAh g after 100 cycles. -1 The experimental specific capacity is about 200 μm. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the main purpose of the present invention is to provide a magnesium gallate positive electrode material for a rechargeable magnesium battery and a preparation method thereof, aiming to solve the problems of low specific capacity and poor cycle performance of the current magnesium battery positive electrode material and rapid specific capacity decay of the magnesium battery during the cycle. The present invention also provides the application of the magnesium gallate positive electrode material for a rechargeable magnesium battery in the field of battery materials.
[0006] The objective of the present invention is achieved through the following technical solutions:
[0007] In a first aspect, a method for preparing magnesium gallate as a positive electrode material for a rechargeable magnesium battery comprises the following steps:
[0008] 1) grinding magnesium nitrate hexahydrate, hydrated gallium nitrate and urea to obtain a white paste-like mixed raw material;
[0009] 2) Mix the white paste into raw materials at 3-5℃min -1 The temperature is raised to 400-600° C. and calcined for 10-30 min to obtain the final product, magnesium gallate, which is a positive electrode material for a rechargeable magnesium battery.
[0010] In certain specific embodiments, the molar ratio of magnesium nitrate hexahydrate, gallium nitrate hydrate and urea is (0.5-1.5):(1-3):(5-10).
[0011] Furthermore, the molar ratio of the magnesium nitrate hexahydrate, the hydrated gallium nitrate and the urea is 1:2:7.
[0012] In some specific embodiments, in step 2), the calcination temperature is 400° C. and the calcination time is 20 min.
[0013] In some specific embodiments, in step 2), the calcination heating rate is 4°C min -1 .
[0014] In a second aspect, a magnesium gallate positive electrode material for a rechargeable magnesium battery is prepared according to the aforementioned preparation method.
[0015] Furthermore, the purity of the magnesium gallate as the positive electrode material of the rechargeable magnesium battery is not less than 99%, the particle size is 0.5-1.5 μm, and the crystal form is cubic spinel type.
[0016] In a third aspect, a use of the aforementioned magnesium gallate positive electrode material for a rechargeable magnesium battery in a rechargeable magnesium battery.
[0017] Compared with the prior art, the present invention has at least the following advantages:
[0018] 1) The present invention uses hydrated magnesium nitrate, hydrated gallium nitrate and urea as raw materials, and obtains cubic phase spinel structure magnesium gallate (MgGa2O4) powder with high crystallinity, fine grains and uniform composition through low temperature combustion method under specific process parameters, and uses the magnesium gallate powder material as a positive electrode material for magnesium ion secondary batteries for electrochemical testing to characterize the specific capacity and cycle performance during the charge and discharge cycle. The electrochemical performance test results show that the magnesium gallate positive electrode material for the rechargeable magnesium battery in the present invention has good rate performance and cycle stability; its specific capacity and cycle performance are good at 50mA g -1 At a current density of 210 mAh g -1 Although it takes a certain amount of time for the activation process, MgGa2O4 can maintain a stable cycle of more than 70 cycles, and has a higher charge-discharge specific capacity and stability compared with similar spinel magnesium-manganese composite oxide positive electrode materials.
[0019] 2) The preparation method of magnesium gallate, a positive electrode material for a rechargeable magnesium battery, provided by the present invention has a simple preparation process and strong replicability, and provides a new method for spinel magnesium ion battery positive electrode materials, which is of great significance. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the specific embodiments of the present invention, the drawings required for use in the specific embodiments or the description of the prior art will be briefly introduced below.
[0021] Figure 1 The original XRD patterns of the magnesium ion battery positive electrode material MgGa2O4 obtained in Example 2 and Comparative Examples 1-3 of the present invention;
[0022] Figure 2 This is a high-resolution TEM image of the magnesium ion battery positive electrode material MgGa2O4 obtained in Example 2 of the present invention;
[0023] Figure 3 The SEM image and EDS spectrum of the positive electrode material MgGa2O4 of the magnesium ion battery in Example 2 of the present invention;
[0024] Figure 4 The cycle specific capacity curve of the positive electrode material MgGa2O4 of the magnesium ion battery in Example 2 of the present invention; DETAILED DESCRIPTION
[0025] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. The following embodiments are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.
[0026] When a certain amount, concentration or other value or parameter is expressed in the form of a range, a preferred range, or a preferred upper and lower numerical limit, it should be understood that it is equivalent to specifically revealing any range by combining any pair of upper range limits or preferred numerical values with any lower range limit or preferred numerical value, regardless of whether the range is specifically disclosed. Unless otherwise indicated, the numerical range values listed herein include the endpoints of the range, and all integers and fractions within the range.
[0027] Unless otherwise indicated, all percentages, parts, ratios, etc. herein are by weight.
[0028] The materials, methods, and examples herein are illustrative and are not to be construed as limiting unless specifically stated.
[0029] In the following examples, the urea raw material had a purity of 99%, specifically purchased from McLean; the gallium (III) nitrate hydrate raw material had a purity of 99.9%, specifically purchased from McLean; the magnesium nitrate hexahydrate raw material had an analytical purity, specifically purchased from Chengdu Kelong;
[0030] The test methods used in the following embodiments include:
[0031] The crystal phase of each test sample was tested by XRD phase analysis; the surface morphology and element distribution were analyzed by scanning electron microscopy; the crystal information was analyzed by transmission electron microscopy; the electrochemical performance was tested by the Xinwei test platform;
[0032] Example 1
[0033] The present embodiment provides a method for preparing magnesium gallate, a positive electrode material for a rechargeable magnesium battery, comprising the following steps:
[0034] 1) grinding magnesium nitrate hexahydrate, gallium nitrate hydrate and urea in a molar ratio of 0.5:1:5 to obtain a white paste-like mixed raw material;
[0035] 2) Mix the white paste into raw materials at 5℃min-1 The temperature was raised to 600°C and calcined for 10 min to obtain the final product, magnesium gallate, which is a positive electrode material for a rechargeable magnesium battery.
[0036] Example 2
[0037] The present embodiment provides a method for preparing magnesium gallate, a positive electrode material for a rechargeable magnesium battery, comprising the following steps:
[0038] 1) grinding magnesium nitrate hexahydrate, gallium nitrate hydrate and urea in a molar ratio of 1:2:7 to obtain a white paste-like mixed raw material;
[0039] 2) Mix the white paste into raw materials at 4℃min -1 The temperature was raised to 500°C and calcined for 20 minutes to obtain the final product, magnesium gallate, which is a positive electrode material for a rechargeable magnesium battery.
[0040] Example 3
[0041] The present embodiment provides a method for preparing magnesium gallate, a positive electrode material for a rechargeable magnesium battery, comprising the following steps:
[0042] 1) grinding magnesium nitrate hexahydrate, gallium nitrate hydrate and urea in a molar ratio of 1.5:2:10 to obtain a white paste-like mixed raw material;
[0043] 2) Mix the white paste into raw materials at 3℃min -1 The temperature was raised to 400°C and calcined for 30 minutes to obtain magnesium gallate, a positive electrode material for a rechargeable magnesium battery.
[0044] Comparative Example 1
[0045] This comparative example provides a method for preparing magnesium gallate, a positive electrode material for a rechargeable magnesium battery. The preparation method is basically the same as that of Example 2, except that the method is heated to 800° C. at the same heating rate and calcined for 20 minutes.
[0046] Although pure magnesium gallate powder was obtained in this comparative example, the obtained magnesium gallate had low crystallinity, large grains and a broad XRD peak.
[0047] Comparative Example 2
[0048] This comparative example provides a preparation method of magnesium gallate, a positive electrode material for a rechargeable magnesium battery. The preparation method is basically the same as that of Example 2, except that urea is replaced with citric acid, the raw materials are weighed in the same molar ratio, heated to 500° C. at the same heating rate, and calcined for 20 minutes.
[0049] This preparation scheme cannot obtain magnesium gallate because citric acid is not suitable as the combustion agent in the preparation method of this patent. The combustion agent (citric acid) used cannot obtain magnesium gallate crystals, so the XRD image shows that the sample of comparative example 2 is amorphous.
[0050] Comparative Example 3
[0051] This comparative example provides a method for preparing magnesium gallate, a positive electrode material for a rechargeable magnesium battery. The difference in the preparation method is that according to the raw material ratio of Example 2, the three chemicals are directly added to deionized water without grinding, stirred and heated until the water is evaporated, the raw materials are fully mixed and made into a gel, and then heated to 500°C at the same heating rate and calcined for 20 minutes.
[0052] Although magnesium gallate powder was obtained in this comparative example, the XRD peak was wider than that in comparative example 1, and the crystallinity of the obtained magnesium gallate was lower; and according to the XRD results showing large noise, it was judged that the magnesium gallate powder prepared by this scheme contained amorphous.
[0053] Performance Test:
[0054] This application takes Example 2 as an example, and performs a performance test on the magnesium gallate, a positive electrode material for a rechargeable magnesium battery prepared in Example 2 and Comparative Examples 1-3. Specifically:
[0055] 1) Morphology test
[0056] The present application conducted morphology test on the product prepared in Example 2, and its XRD test results are as follows: Figure 1 As shown in the figure, it can be seen that the 2θ angle of the diffraction peak of the magnesium gallate of the rechargeable magnesium battery positive electrode material is basically aligned with the angle in the standard card of MgGa2O4 (PDF#78-0551), and there is no impurity peak; in the XRD diffraction spectrum, obvious diffraction peaks can be observed at 2θ angles of 18.594°, 30.517°, 35.579°, 37.607°, 43.726°, 54.204°, 57.827°, and 53.422°, which are respectively consistent with the (111), (220), (311), (222), (400), (422), (511), and (440) crystal planes of the cubic phase magnesium gallate, and there are no other impurity peaks, and the calculated average lattice parameter is Compared with the standard cubic phase MgGa2O4 The results are basically consistent, which proves that the product is pure cubic spinel magnesium gallate; on the other hand, the high-angle annular dark field transmission electron microscopy (HAADF-TEM) images (such as Figure 2 Clear particle shapes and lattice fringes can also be observed in the HAADF image. By performing FFT and IFFT processing on the HAADF image, it is observed that the spacing between lattice fringes with different orientations is and They correspond to the crystal planes (111), (311), (200) and (511) (JCPDS No.78-0551), further proving that the product is pure cubic spinel magnesium gallate. Figure 3 ) shows that the particle size of the synthesized MgGa2O4 is about 1 μm; in the EDS spectrum ( Figure 3 ) shows that the distribution of C, O, Ga and Mg is relatively uniform.
[0057] 2) Electrical performance test
[0058] In this application, the prepared magnesium gallate as the positive electrode material of the rechargeable magnesium battery is used as the positive electrode material of the magnesium ion battery, graphite paper is used as the negative electrode material, glass fiber diaphragm (Whatman, GF / A) is used as the diaphragm of the magnesium ion battery, stainless steel is used as the current collector, 0.5M Mg(TFSI)2 / DME is used as the electrolyte, and CR2032 button cells are assembled in a glove box filled with high-purity argon. The assembled battery is tested for electrochemical performance on the Xinwei battery control test system; the specific test method is:
[0059] S1. The prepared magnesium gallate positive electrode material of the rechargeable magnesium battery is mixed with acetylene carbon black and a binder (PVDF) in a ratio of 6:3:1, and coated on a stainless steel current collector with a coating thickness of 100 μm.
[0060] S2. Dry the plate in a blast dryer at 60°C and then punch it into positive electrode sheets with a diameter of 12 mm.
[0061] S3. Graphite paper was used as the negative electrode and 0.5 M Mg(TFSI)2-DME was used as the electrolyte. The prepared positive electrode sheet was assembled into a CR2032 button cell in an argon glove box. The electrochemical performance of magnesium gallate as the positive electrode material was tested using a Xinwei electrochemical workstation. The test voltage window was -1.0 V to 1.2 V, and the current density was 50 mA g -1 .
[0062] The results are as follows Figure 4 As shown in the figure, it can be seen that the magnesium gallate positive electrode material for the rechargeable magnesium battery prepared in this application has a current density of 50mA g -1 MgGa2O4 exhibits 210 mAh g -1 The specific capacity is about 210 mAh g / cm2, and it can be stably cycled for about 70 cycles (70-150 cycles). The specific capacity reaches a maximum of 210 mAh g / cm2 around the 80th to 85th cycle. -1 Then, the specific capacity slowly decreased to 188 mAh g in the 85th to 120th cycle. -1 The specific capacity of the 120-150th cycle slowly rises to 210 mAh g-1 , its fluctuation amplitude is very small, showing good cycle stability; compared with similar spinel magnesium oxide positive electrode materials, it has high charge and discharge specific capacity and stability.
[0063] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention.
Claims
1. A method for preparing magnesium gallate as a positive electrode material for a rechargeable magnesium battery. It is characterized in that The steps include: 1) grinding magnesium nitrate hexahydrate, hydrated gallium nitrate and urea to obtain a white paste-like mixed raw material; 2) Mix the white paste into raw materials at 3-5℃min -1 The temperature is raised to 400-600° C. and calcined for 10-30 min to obtain the final product, magnesium gallate, which is a positive electrode material for a rechargeable magnesium battery.
2. The method for preparing magnesium gallate as a positive electrode material for a rechargeable magnesium battery according to claim 1, It is characterized in that The molar ratio of the magnesium nitrate hexahydrate, the gallium nitrate hydrate and the urea is (0.5-1.5):(1-3):(5-10).
3. The method for preparing magnesium gallate as a positive electrode material for a rechargeable magnesium battery according to claim 2, It is characterized in that The molar ratio of the magnesium nitrate hexahydrate, the hydrated gallium nitrate and the urea is 1:2:
7.
4. The method for preparing magnesium gallate as a positive electrode material for a rechargeable magnesium battery according to claim 1, It is characterized in that In step 2), the calcination temperature is 400° C. and the calcination time is 20 min.
5. The method for preparing magnesium gallate as a positive electrode material for a rechargeable magnesium battery according to claim 4, It is characterized in that In step 2), the calcination heating rate is 4°C min -1 .
6. A rechargeable magnesium battery positive electrode material magnesium gallate, It is characterized in that Prepared according to the preparation method according to any one of claims 1 to 5.
7. The magnesium gallate positive electrode material for a rechargeable magnesium battery according to claim 6, It is characterized in that The purity of magnesium gallate, the positive electrode material of the rechargeable magnesium battery, is not less than 99%, the particle size is 0.5-1.5 μm, and the crystal form is cubic phase spinel type.
8. Use of magnesium gallate, a positive electrode material for a rechargeable magnesium battery according to claim 6 or 7, in a rechargeable magnesium battery.