Ternary precursor with primary particles in coarse-fine interwoven state and preparation method thereof
By optimizing the XRD half-maximum width, specific surface area and tap density of the lithium-ion battery cathode material precursor through three coprecipitation methods, the problem of insufficient performance in the existing technology was solved and the preparation of high-performance precursor was achieved.
Patent Information
- Application Number
- CN202410782920.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-18
AI Technical Summary
It is difficult to achieve comprehensive optimization of XRD half-peak width, specific surface area and tap density in lithium-ion battery cathode material precursors with existing technology, resulting in insufficient performance.
A third co-precipitation method is used to nucleate at a higher reaction pH value, and the particle size of the agglomerates is monitored online, and an oxidant is further injected in parallel flow for the second co-precipitation to form spherical particles, and then the third step is performed under the condition of lowering the reaction pH value. Co-precipitation achieves the interlaced state of particles, controls oxidation, reaction pH, ammonia concentration and reaction time, and optimizes the physical and chemical indicators of the precursor.
The comprehensive optimization of the XRD half-peak width, specific surface area and tap density of the ternary precursor was achieved, and a precursor with a larger half-peak width, suitable specific surface area and high tap density was obtained, which is suitable for high-performance lithium-ion battery cathode materials.
Smart Images

Figure CN118724082A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion batteries, and in particular to a ternary precursor with primary particles in a coarse and fine intertwined state and a preparation method thereof. Background Art
[0002] Lithium-ion batteries are the most widely used secondary batteries in the world today. They have many advantages such as high energy density, high operating voltage, low self-discharge and long cycle life. The positive electrode materials of lithium-ion batteries mainly include lithium cobalt oxide, lithium iron phosphate, ternary materials (including lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide), lithium manganese oxide, etc. Among them, batteries with ternary material systems can provide higher energy density than other types of lithium-ion batteries, usually reaching more than 200Wh / kg, which makes the battery have higher endurance and power output capabilities.
[0003] Ternary precursors are important raw materials for the production of ternary cathode materials. They are usually made of nickel salts, cobalt salts and manganese salts. Nickel cobalt manganese hydroxides synthesized by coprecipitation or oxides obtained by further calcination are mixed and sintered with lithium salts to obtain ternary cathode materials. Ternary cathode materials have good inheritance of precursors. The physical and chemical indicators of the precursors (composition, morphology, structure, particle size, particle size distribution, specific surface area, impurity content, tap density, etc.) directly determine the physical and chemical properties of the final sintered product, and thus determine whether the cathode material can meet the terminal requirements of high specific capacity, high rate, long cycle life, high safety, etc.
[0004] With the continuous development of the industry and technology, the requirements for precursor indicators are also moving towards a more refined direction. For example, some cathode material manufacturers have put forward higher requirements for physical and chemical indicators such as the arrangement direction of primary particles of the precursor, internal structure, specific surface area and tap density. Some cathode material manufacturers also put forward higher requirements for the preferential growth of a certain crystal plane of the precursor, crystallinity, XRD half peak width, etc.
[0005] However, the various physical and chemical indicators of the precursor sometimes restrict each other. For example, when a higher specific surface area is obtained, the precursor is often loose and porous, and the tap density is easy to reduce; on the contrary, when the tap density of the precursor is high, the primary particles are often densely stacked, and the specific surface area is difficult to increase. For example, the half-peak width of the XRD spectrum is often related to the crystallinity and grain size of the precursor, and this indicator will affect the specific surface area and tap density. In the production and preparation of positive electrode materials, sometimes higher requirements are placed on the XRD half-peak width, specific surface area and tap density of the precursor. In addition to being related to the elemental composition ratio of the precursor, the XRD half-peak width of the precursor is also related to factors such as the crystallinity of the precursor. Generally speaking, the better the crystal development and the larger the grain size, the narrower the half-peak width. If conventional preparation methods are used to obtain products with a wide half-peak width, the tap density of the precursor will often be low and the specific surface area will be too large. Therefore, in order to achieve comprehensive optimization among various physical and chemical indicators and obtain high-performance precursor materials, it is necessary to improve the precursor preparation technology and process control level. Summary of the invention
[0006] In view of the problems existing in the prior art, the present invention provides a ternary precursor in which primary particles are in a coarse and fine interwoven state and a preparation method thereof. The preparation method comprises three coprecipitations, wherein a first coprecipitation is performed to form nuclei at a higher reaction pH value, and online monitoring is performed until the particle size of agglomerates generated by the first coprecipitation is reduced to a minimum value, and an oxidant is further injected in parallel, and a second coprecipitation is performed under the condition of four parallel injections, so that the primary particles in a single type of spherical particles undergo crystal growth to form flaky coarse primary particles, the reaction pH value is lowered to cause secondary nucleation, and flaky fine primary particles are grown in situ on the flaky coarse primary particles, thereby obtaining a ternary precursor in which primary particles are in a coarse and fine interwoven state; the preparation method of the present invention can obtain a ternary precursor with comprehensively optimized XRD half-peak width, specific surface area and tap density by controlling the process of oxidation, reaction pH value, ammonia concentration and reaction time during the coprecipitation process.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] One of the purposes of the present invention is to provide a method for preparing a ternary precursor in which primary particles are in a coarse and fine intertwined state, the preparation method comprising the following steps:
[0009] Injecting a nickel-cobalt-manganese mixed salt solution, a precipitant solution and a complexing agent solution into a reaction bottom solution in parallel to perform a first coprecipitation, and controlling the reaction pH value of the first coprecipitation to be N1;
[0010] Online monitoring shows that the particle size of the agglomerates generated by the first coprecipitation is reduced to a minimum value, and an oxidant is further injected in parallel to perform a second coprecipitation, and the reaction pH value of the second coprecipitation is controlled to remain at N1;
[0011] The particle size of the particles in the second co-precipitation is monitored online to 2.5-4.5 μm, four parallel flows are maintained for injection and a third co-precipitation is performed, and the reaction pH value of the third co-precipitation is controlled to be N2. After reaching the target particle size, solid-liquid separation is performed to obtain a ternary precursor in which the primary particles are in a coarse and fine interwoven state;
[0012] Among them, 1.5≤N1-N2≤2.5.
[0013] The preparation method of the present invention comprises three co-precipitations, wherein the first co-precipitation is firstly carried out to form nuclei at a relatively high reaction pH value, and the generated primary particles are first agglomerated into quasi-spherical shapes, and the quasi-spherical particles are then agglomerated into irregular large particles. As the first co-precipitation proceeds, the irregular large particles are gradually dispersed into quasi-spherical particles, so that the particle size of the agglomerates generated by the first co-precipitation decreases. It is monitored online that the particle size of the agglomerates generated by the first co-precipitation decreases to a minimum value, and an oxidant is further injected in parallel. A second co-precipitation is carried out under the condition of four parallel injections, so that the primary particles in the single quasi-spherical particles undergo crystal growth to form flaky coarse primary particles. The particle size of the particles in the second co-precipitation is monitored online to be 2.5-4.5 μm, and the four parallel injections are maintained and a third co-precipitation is carried out, the reaction pH value is lowered to cause secondary nucleation, and flaky fine primary particles are grown in situ on the flaky coarse primary particles, thereby obtaining a ternary precursor in which the primary particles are in a coarse and fine interwoven state.
[0014] The control of the coprecipitation reaction conditions includes the reaction atmosphere, pH, ammonia concentration and reaction time. The reaction atmosphere will affect the oxidation degree of the precursor, the pH and ammonia concentration will affect the supersaturation of the reaction system, and the reaction time will affect the particle size and crystal development degree of the precursor. These factors in turn affect and restrict the sphericity, primary particle morphology, specific surface area, tap density and crystallinity of the precursor. The preparation method of the present invention can obtain a ternary precursor with comprehensively optimized XRD half-peak width, specific surface area and tap density by controlling the process of oxidation, reaction pH value, ammonia concentration and reaction time during the coprecipitation process, and the specific surface area is 10-15m 2 / g, tap density is 1.5-1.7g / cm 3 , (001) half-peak width is 0.50-0.60.
[0015] As a preferred technical solution of the present invention, the nickel-cobalt-manganese mixed salt solution includes a soluble nickel salt, a soluble cobalt salt and a soluble manganese salt, and the molar ratio of the three is a:b:(1-ab); wherein 0.6≤a≤0.7, 0<b<0.2.
[0016] Preferably, the total metal concentration of the nickel-cobalt-manganese mixed salt solution is 90-120 g / L, for example 90 g / L, 95 g / L, 100 g / L, 105 g / L, 110 g / L, 115 g / L or 120 g / L, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0017] It should be noted that the total metal concentration of the nickel-cobalt-manganese mixed salt solution of the present invention refers to the total concentration of nickel-cobalt-manganese metal ions.
[0018] Preferably, the soluble nickel salt includes at least one of nickel sulfate, nickel chloride or nickel nitrate.
[0019] Preferably, the soluble cobalt salt comprises at least one of cobalt sulfate, cobalt chloride or cobalt nitrate.
[0020] Preferably, the soluble manganese salt comprises at least one of manganese sulfate, manganese chloride or manganese nitrate.
[0021] As a preferred technical solution of the present invention, the precipitant solution is a sodium hydroxide solution or a potassium hydroxide solution.
[0022] Preferably, the concentration of the precipitant solution is 25-35wt%, for example, 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, 33wt%, 34wt% or 35wt%, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0023] Preferably, the complexing agent solution is aqueous ammonia.
[0024] Preferably, the concentration of the complexing agent solution is 14-18wt%, such as 14wt%, 15wt%, 16wt%, 17wt% or 18wt%, etc., but is not limited to the listed values, and other values not listed within the above range are also applicable.
[0025] It should be noted that the reaction base liquid of the present invention is prepared from pure water, a precipitant solution and a complexing agent solution, and is used to maintain the stability of the reaction system; the reaction base liquid is prepared in a reactor, stirring is started, the temperature is raised to the target temperature, nitrogen is passed to replace the air in the reactor, and nitrogen is continuously passed during the co-precipitation process.
[0026] As a preferred technical solution of the present invention, the oxidant includes hydrogen peroxide solution and / or air.
[0027] Preferably, the oxidant is a hydrogen peroxide solution with a concentration of 1.5 to 2.5 wt%, and the injection flow rate is 0.5 to 5 L / h, for example, 0.5 L / h, 1 L / h, 1.5 L / h, 2 L / h, 2.5 L / h, 3 L / h, 3.5 L / h, 4 L / h, 4.5 L / h or 5 L / h, but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0028] As a preferred technical solution of the present invention, the reaction temperature of the first coprecipitation is 50-70°C, for example, 50°C, 53°C, 55°C, 57°C, 60°C, 62°C, 65°C, 68°C or 70°C, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0029] Preferably, the concentration of the complexing agent of the first co-precipitation is 5-7 g / L, for example 5 g / L, 5.5 g / L, 6 g / L, 6.5 g / L or 7 g / L, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0030] Preferably, the reaction pH value N1 of the first coprecipitation is 11.3-11.8, such as 11.3, 11.4, 11.5, 11.6, 11.7 or 11.8, but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0031] As a preferred technical solution of the present invention, the reaction temperature of the second co-precipitation is 50-70°C, for example, 50°C, 53°C, 55°C, 57°C, 60°C, 62°C, 65°C, 68°C or 70°C, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0032] Preferably, the concentration of the complexing agent of the second co-precipitation is 5-7 g / L, for example 5 g / L, 5.5 g / L, 6 g / L, 6.5 g / L or 7 g / L, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0033] Preferably, the reaction pH value N1 of the second coprecipitation is 11.3-11.8, such as 11.3, 11.4, 11.5, 11.6, 11.7 or 11.8, but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0034] As a preferred technical solution of the present invention, the reaction temperature of the third coprecipitation is 50-70°C, for example, 50°C, 53°C, 55°C, 57°C, 60°C, 62°C, 65°C, 68°C or 70°C, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0035] Preferably, the concentration of the complexing agent of the third co-precipitation is 2-3 g / L, for example 2 g / L, 2.1 g / L, 2.2 g / L, 2.3 g / L, 2.4 g / L, 2.5 g / L, 2.6 g / L, 2.7 g / L, 2.8 g / L, 2.9 g / L or 3 g / L, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0036] Preferably, the reaction pH value of the third coprecipitation is 9.2-9.7, such as 9.2, 9.3, 9.4, 9.5, 9.6 or 9.7, but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0037] As a preferred technical solution of the present invention, the target particle size is 3 to 5 μm, for example 3 μm, 3.3 μm, 3.5 μm, 3.7 μm, 4 μm, 4.2 μm, 4.5 μm, 4.7 μm or 5 μm, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0038] As a preferred technical solution of the present invention, the preparation method comprises the following steps:
[0039] Injecting a nickel-cobalt-manganese mixed salt solution, a precipitant solution and a complexing agent solution into a reaction bottom solution in parallel, performing a first coprecipitation at 50-70° C., controlling the reaction pH value N1 of the first coprecipitation to be 11.3-11.8, and the complexing agent concentration to be 5-7 g / L;
[0040] The particle size of the agglomerates generated by the first coprecipitation is monitored online to be reduced to a minimum value, and an oxidant is further injected in parallel to perform a second coprecipitation at 50 to 70° C. The reaction pH value of the second coprecipitation is controlled to be still N1, still 11.3 to 11.8, and the concentration of the complexing agent is 5 to 7 g / L;
[0041] The particle size of the particles in the second coprecipitation is monitored online to 2.5-4.5 μm, four parallel streams are injected and the third coprecipitation is performed at 50-70° C. The reaction pH value N2 of the third coprecipitation is controlled to be 9.2-9.7, and the concentration of the complexing agent is 2-3 g / L. After reaching the target particle size of 3-5 μm, the reaction is stopped, and aging, washing, and drying are performed in sequence to obtain a ternary precursor in which the primary particles are in a coarse and fine interwoven state;
[0042] Among them, 1.5≤N1-N2≤2.5;
[0043] The nickel-cobalt-manganese mixed salt solution comprises a soluble nickel salt, a soluble cobalt salt and a soluble manganese salt, and the molar ratio of the three is a:b:(1-ab); wherein 0.6≤a≤0.7, 0<b<0.2; the total metal concentration of the nickel-cobalt-manganese mixed salt solution is 90-120 g / L; the precipitant solution is a sodium hydroxide solution or a potassium hydroxide solution; the concentration of the precipitant solution is 25-35 wt%; the complexing agent solution is ammonia water; the concentration of the complexing agent solution is 14-18 wt%; the oxidant is a hydrogen peroxide solution with a concentration of 1.5-2.5 wt%, and the injection flow rate is 0.5-5 L / h.
[0044] The second object of the present invention is to provide a ternary precursor in which primary particles are in a coarse and fine intertwined state. The ternary precursor in which primary particles are in a coarse and fine intertwined state is prepared according to the preparation method described in one of the objects. The ternary precursor in which primary particles are in a coarse and fine intertwined state is formed by stacking coarse primary particles in a flaky state, and fine primary particles in a flaky state grow in situ on the coarse primary particles.
[0045] The ternary precursor in which the primary particles of the present invention are in a coarse and fine interlaced state can not only reduce the crystallinity and the average grain size, thereby obtaining a ternary precursor with a larger XRD half-peak width, but also, because the primary particles are in a coarse and fine interlaced state and are staggered and filled, the porosity of the ternary precursor particles is guaranteed and the density is improved, so that the ternary precursor has both a higher tap density and a suitable specific surface area.
[0046] Compared with the prior art solutions, the present invention has at least the following beneficial effects:
[0047] (1) The preparation method of the present invention comprises three co-precipitations, wherein the first co-precipitation is performed to form nuclei at a relatively high reaction pH value, and the particle size of the agglomerates generated by the first co-precipitation is monitored online to be reduced to a minimum value, and an oxidant is further injected in parallel, and a second co-precipitation is performed under the condition of four parallel injections, so that the primary particles in the single spherical particles undergo crystal growth to form flaky coarse primary particles, the reaction pH value is lowered to cause secondary nucleation, and flaky fine primary particles are in situ grown on the flaky coarse primary particles, thereby obtaining a ternary precursor in which the primary particles are in a coarse and fine interwoven state;
[0048] (2) The ternary precursor in which the primary particles are in a coarse and fine interlaced state according to the present invention can not only reduce the crystallinity and the average grain size, thereby obtaining a ternary precursor with a larger XRD half-peak width, but also, because the primary particles are in a coarse and fine interlaced state and staggered filling, the porosity of the ternary precursor particles is guaranteed and the density is improved, so that the ternary precursor has both a higher tap density and a suitable specific surface area;
[0049] (3) The preparation method of the present invention can obtain a ternary precursor with comprehensive optimization of XRD half-peak width, specific surface area and tap density by controlling the process of oxidation, reaction pH value, ammonia concentration and reaction time during the coprecipitation process, and the specific surface area is 10-15m 2 / g, tap density is 1.5-1.7g / cm 3 , (001) half-peak width is 0.50-0.60, which has strong operability and is easy for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 This is a SEM image of a ternary precursor in which primary particles prepared in Example 1 of the present invention are in a coarse and fine intertwined state;
[0051] Figure 2 This is a cross-sectional SEM image of a ternary precursor in which primary particles prepared in Example 1 of the present invention are in a coarse and fine intertwined state. DETAILED DESCRIPTION
[0052] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.
[0053] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0054] Example 1
[0055] This embodiment provides a method for preparing a ternary precursor in which primary particles are in a coarse and fine interlaced state, and the preparation method comprises the following steps:
[0056] A nickel-cobalt-manganese mixed salt solution is prepared by using nickel sulfate, cobalt sulfate and manganese sulfate in a molar ratio of 0.6:0.1:0.3, wherein the total metal concentration of the nickel-cobalt-manganese mixed salt solution is 90 g / L; a sodium hydroxide solution with a concentration of 30 wt% is used as a precipitant solution; and an ammonia solution with a concentration of 15 wt% is used as a complexing agent solution;
[0057] Add pure water, precipitant solution and complexing agent solution into the reactor to prepare the reaction base solution, start stirring, raise the temperature to 50°C, and replace the air in the reactor with nitrogen;
[0058] The nickel-cobalt-manganese mixed salt solution, the precipitant solution and the complexing agent solution are injected into the reaction bottom solution in parallel, and nitrogen is continuously introduced to perform the first coprecipitation at 50° C., and the reaction pH value N1 of the first coprecipitation is controlled to be 11.6, and the complexing agent concentration is 5.0 g / L;
[0059] The particle size of the agglomerates generated by the first coprecipitation was monitored online to be reduced to a minimum value, and a hydrogen peroxide solution with a concentration of 2 wt % was further injected in parallel as an oxidant at an injection flow rate of 0.5 L / h, and a second coprecipitation was performed at 50° C. The reaction pH value of the second coprecipitation was controlled to be still N1, still 11.6, and the complexing agent concentration was 5.0 g / L;
[0060] The reaction was continued for 30 hours until the particle size grew to 3.0 μm, and then four parallel streams were injected and the third co-precipitation was carried out at 50°C. The reaction pH value N2 of the third co-precipitation was controlled to be 9.2, and the concentration of the complexing agent was 2.0 g / L. After the third co-precipitation was carried out for 30 hours, the target particle size of 3.5 μm was reached, and the reaction was stopped. The particles were aged, washed, and dried in sequence to obtain a ternary precursor with primary particles in a coarse and fine interwoven state.
[0061] Figure 1 The SEM image of the ternary precursor obtained in this embodiment shows that the primary particles are in a coarse and fine intertwined state. Figure 2 The cross-sectional SEM image of the ternary precursor obtained in this embodiment shows that the primary particles are in a coarse and fine intertwined state. Figure 1 and Figure 2 It can be seen that the primary particles are in a coarse and fine intertwined state. The ternary precursor is formed by the accumulation of flaky coarse primary particles, while flaky fine primary particles grow in situ on the coarse primary particles.
[0062] Example 2
[0063] This embodiment provides a method for preparing a ternary precursor in which primary particles are in a coarse and fine interlaced state, and the preparation method comprises the following steps:
[0064] A nickel-cobalt-manganese mixed salt solution is prepared by using nickel sulfate, cobalt sulfate and manganese sulfate in a molar ratio of 0.7:0.1:0.2, wherein the total metal concentration of the nickel-cobalt-manganese mixed salt solution is 110 g / L; a sodium hydroxide solution with a concentration of 35 wt% is used as a precipitant solution; and an ammonia solution with a concentration of 18 wt% is used as a complexing agent solution;
[0065] Add pure water, precipitant solution and complexing agent solution into the reactor to prepare the reaction base solution, start stirring, raise the temperature to 60°C, and replace the air in the reactor with nitrogen;
[0066] The nickel-cobalt-manganese mixed salt solution, the precipitant solution and the complexing agent solution are injected into the reaction bottom solution in parallel, and nitrogen is continuously introduced to perform the first coprecipitation at 60° C. The reaction pH value N1 of the first coprecipitation is controlled to be 11.8, and the complexing agent concentration is 6.0 g / L;
[0067] The particle size of the agglomerates generated by the first coprecipitation was monitored online to be reduced to a minimum value, and a hydrogen peroxide solution with a concentration of 2 wt % was further injected in parallel as an oxidant at an injection flow rate of 2 L / h, and a second coprecipitation was performed at 60° C. The reaction pH value of the second coprecipitation was controlled to be still N1, still 11.8, and the complexing agent concentration was 6.0 g / L;
[0068] The reaction was continued for 40 hours until the particle size grew to 3.8 μm, and then four parallel streams were injected and the third co-precipitation was carried out at 60°C. The reaction pH value N2 of the third co-precipitation was controlled to be 9.5, and the concentration of the complexing agent was 2.5 g / L. After the third co-precipitation was carried out for 40 hours, the target particle size of 5.0 μm was reached, and the reaction was stopped. The particles were aged, washed, and dried in sequence to obtain a ternary precursor with primary particles in a coarse and fine interwoven state.
[0069] Example 3
[0070] This embodiment provides a method for preparing a ternary precursor in which primary particles are in a coarse and fine interlaced state, and the preparation method comprises the following steps:
[0071] A nickel-cobalt-manganese mixed salt solution is prepared by using nickel sulfate, cobalt sulfate and manganese sulfate in a molar ratio of 0.65:0.05:0.3, wherein the total metal concentration of the nickel-cobalt-manganese mixed salt solution is 120 g / L; a sodium hydroxide solution with a concentration of 35 wt% is used as a precipitant solution; and an ammonia solution with a concentration of 18 wt% is used as a complexing agent solution;
[0072] Add pure water, precipitant solution and complexing agent solution into the reactor to prepare the reaction base solution, start stirring, raise the temperature to 70°C, and replace the air in the reactor with nitrogen;
[0073] The nickel-cobalt-manganese mixed salt solution, the precipitant solution and the complexing agent solution are injected into the reaction bottom solution in parallel, and nitrogen is continuously introduced to perform the first coprecipitation at 70° C., and the reaction pH value N1 of the first coprecipitation is controlled to be 11.3, and the complexing agent concentration is 7.0 g / L;
[0074] The particle size of the agglomerates generated by the first coprecipitation was monitored online to be reduced to a minimum value, and a hydrogen peroxide solution with a concentration of 2 wt % was further injected in parallel as an oxidant at an injection flow rate of 5 L / h, and a second coprecipitation was performed at 70° C. The reaction pH value of the second coprecipitation was controlled to be still N1, still 11.3, and the complexing agent concentration was 7.0 g / L;
[0075] The reaction was continued for 25 hours. After the particle size grew to 2.5 μm, four parallel streams were injected and the third co-precipitation was carried out at 70°C. The reaction pH value N2 of the third co-precipitation was controlled to be 9.7, and the concentration of the complexing agent was 3.0 g / L. After the third co-precipitation was carried out for 25 hours, the target particle size of 3.0 μm was reached, and the reaction was stopped. The particles were aged, washed, and dried in sequence to obtain a ternary precursor with primary particles in a coarse and fine interwoven state.
[0076] Comparative Example 1
[0077] This comparative example provides a method for preparing a ternary precursor, and the preparation method comprises the following steps:
[0078] A nickel-cobalt-manganese mixed salt solution is prepared by using nickel sulfate, cobalt sulfate and manganese sulfate in a molar ratio of 0.6:0.1:0.3, wherein the total metal concentration of the nickel-cobalt-manganese mixed salt solution is 90 g / L; a sodium hydroxide solution with a concentration of 30 wt% is used as a precipitant solution; and an ammonia solution with a concentration of 15 wt% is used as a complexing agent solution;
[0079] Add pure water, precipitant solution and complexing agent solution into the reactor to prepare the reaction base solution, start stirring, raise the temperature to 50°C, and replace the air in the reactor with nitrogen;
[0080] A nickel-cobalt-manganese mixed salt solution, a precipitant solution and a complexing agent solution are injected into the reaction base liquid in parallel, and nitrogen is continuously introduced to carry out co-precipitation at 50°C. The reaction pH value of the co-precipitation is controlled to be 11.6, and the complexing agent concentration is 5.0 g / L. After the reaction is continued for 50 hours, the target particle size of 3.5 μm is reached, and the reaction is stopped. The ternary precursor is obtained by aging, washing and drying in sequence.
[0081] Comparative Example 2
[0082] This comparative example provides a method for preparing a ternary precursor, and the preparation method comprises the following steps:
[0083] A nickel-cobalt-manganese mixed salt solution is prepared by using nickel sulfate, cobalt sulfate and manganese sulfate in a molar ratio of 0.6:0.1:0.3, wherein the total metal concentration of the nickel-cobalt-manganese mixed salt solution is 90 g / L; a sodium hydroxide solution with a concentration of 30 wt% is used as a precipitant solution; and an ammonia solution with a concentration of 15 wt% is used as a complexing agent solution;
[0084] Add pure water, precipitant solution and complexing agent solution into the reactor to prepare the reaction base solution, start stirring, raise the temperature to 50°C, and replace the air in the reactor with nitrogen;
[0085] The nickel-cobalt-manganese mixed salt solution, the precipitant solution and the complexing agent solution are injected into the reaction bottom solution in parallel, and nitrogen is continuously introduced to perform the first coprecipitation at 50° C., and the reaction pH value of the first coprecipitation is controlled to be 11.6, and the complexing agent concentration is 5.0 g / L;
[0086] The particle size of the agglomerates generated by the first coprecipitation is monitored online to be reduced to a minimum value, and a hydrogen peroxide solution with a concentration of 2 wt % is further injected in parallel as an oxidant at an injection flow rate of 0.5 L / h, and a second coprecipitation is performed at 50° C. The reaction pH value of the second coprecipitation is controlled to be still 11.6, and the complexing agent concentration is 5.0 g / L;
[0087] After the reaction was continued for 40 hours, the target particle size of 3.5 μm was reached, and the reaction was stopped. The ternary precursor was obtained by aging, washing and drying in sequence.
[0088] The ternary precursors prepared in the above examples and comparative examples were tested for physical and chemical indicators, and the results are shown in Table 1.
[0089] Table 1
[0090]
[0091]
[0092] In summary, the ternary precursor in which the primary particles are in a coarse and fine interlaced state according to the present invention can not only reduce the crystallinity and the average grain size, thereby obtaining a ternary precursor with a larger XRD half-peak width, but also, because the primary particles are in a coarse and fine interlaced state and staggered filling, the porosity of the ternary precursor particles is guaranteed and the density is improved, so that the ternary precursor has both a higher tap density and a suitable specific surface area; the preparation method of the present invention can obtain a ternary precursor with comprehensively optimized XRD half-peak width, specific surface area and tap density by controlling the process of oxidation, reaction pH value, ammonia concentration and reaction time during the coprecipitation process, and the specific surface area is 10-15m 2 / g, tap density is 1.5-1.7g / cm 3 , (001) half-peak width is 0.50-0.60, which has strong operability and is easy for large-scale production.
[0093] The present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0094] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0095] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0096] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing a ternary precursor in which primary particles are in a coarse and fine intertwined state, characterized in that: The preparation method comprises the following steps: Injecting a nickel-cobalt-manganese mixed salt solution, a precipitant solution and a complexing agent solution into a reaction bottom solution in parallel to perform a first coprecipitation, and controlling the reaction pH value of the first coprecipitation to be N1; Online monitoring shows that the particle size of the agglomerates generated by the first coprecipitation is reduced to a minimum value, and an oxidant is further injected in parallel to perform a second coprecipitation, and the reaction pH value of the second coprecipitation is controlled to remain at N1; The particle size of the particles in the second co-precipitation is monitored online to 2.5-4.5 μm, four parallel flows are maintained for injection and a third co-precipitation is performed, and the reaction pH value of the third co-precipitation is controlled to be N2. After reaching the target particle size, solid-liquid separation is performed to obtain a ternary precursor in which the primary particles are in a coarse and fine interwoven state; Among them, 1.5≤N1-N2≤2.
5.
2. The preparation method according to claim 1, characterized in that: The nickel-cobalt-manganese mixed salt solution includes a soluble nickel salt, a soluble cobalt salt and a soluble manganese salt, and the molar ratio of the three is a:b:(1-ab); wherein 0.6≤a≤0.7, 0<b<0.2; Preferably, the total metal concentration of the nickel-cobalt-manganese mixed salt solution is 90-120 g / L.
3. The preparation method according to claim 1 or 2, characterized in that: The precipitant solution is a sodium hydroxide solution or a potassium hydroxide solution; Preferably, the concentration of the precipitant solution is 25-35wt%; Preferably, the complexing agent solution is aqueous ammonia; Preferably, the concentration of the complexing agent solution is 14-18 wt %.
4. The preparation method according to any one of claims 1 to 3, characterized in that The oxidant includes hydrogen peroxide solution and / or air; Preferably, the oxidant is a hydrogen peroxide solution with a concentration of 1.5 to 2.5 wt %, and the injection flow rate is 0.5 to 5 L / h.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The reaction temperature of the first coprecipitation is 50-70°C; Preferably, the concentration of the complexing agent in the first coprecipitation is 5 to 7 g / L; Preferably, the reaction pH value N1 of the first coprecipitation is 11.3-11.
8.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The reaction temperature of the second coprecipitation is 50-70°C; Preferably, the concentration of the complexing agent in the second coprecipitation is 5 to 7 g / L; Preferably, the reaction pH value N1 of the second coprecipitation is 11.3-11.
8.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The reaction temperature of the third coprecipitation is 50-70°C; Preferably, the concentration of the complexing agent in the third coprecipitation is 2 to 3 g / L; Preferably, the reaction pH value of the third coprecipitation is 9.2-9.
7.
8. The preparation method according to any one of claims 1 to 7, characterized in that: The target particle size is 3 to 5 μm.
9. The preparation method according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: Injecting a nickel-cobalt-manganese mixed salt solution, a precipitant solution and a complexing agent solution into a reaction bottom solution in parallel, performing a first coprecipitation at 50-70° C., controlling the reaction pH value N1 of the first coprecipitation to be 11.3-11.8, and the complexing agent concentration to be 5-7 g / L; The particle size of the agglomerates generated by the first coprecipitation is monitored online to be reduced to a minimum value, and an oxidant is further injected in parallel to perform a second coprecipitation at 50 to 70° C. The reaction pH value of the second coprecipitation is controlled to be still N1, still 11.3 to 11.8, and the concentration of the complexing agent is 5 to 7 g / L; The particle size of the particles in the second coprecipitation is monitored online to 2.5-4.5 μm, four parallel streams are injected and the third coprecipitation is performed at 50-70° C. The reaction pH value N2 of the third coprecipitation is controlled to be 9.2-9.7, and the concentration of the complexing agent is 2-3 g / L. After reaching the target particle size of 3-5 μm, the reaction is stopped, and aging, washing, and drying are performed in sequence to obtain a ternary precursor in which the primary particles are in a coarse and fine interwoven state; Among them, 1.5≤N1-N2≤2.5; The nickel-cobalt-manganese mixed salt solution comprises a soluble nickel salt, a soluble cobalt salt and a soluble manganese salt, and the molar ratio of the three is a:b:(1-ab); wherein 0.6≤a≤0.7, 0<b<0.2; the total metal concentration of the nickel-cobalt-manganese mixed salt solution is 90-120 g / L; the precipitant solution is a sodium hydroxide solution or a potassium hydroxide solution; the concentration of the precipitant solution is 25-35 wt%; the complexing agent solution is ammonia water; the concentration of the complexing agent solution is 14-18 wt%; the oxidant is a hydrogen peroxide solution with a concentration of 1.5-2.5 wt%, and the injection flow rate is 0.5-5 L / h.
10. A ternary precursor in which primary particles are in a coarse and fine interlaced state, characterized in that: The primary particles are in a coarse and fine interweaving state. According to the preparation method according to any one of claims 1 to 9, the primary particles are in a coarse and fine intertwined state. The ternary precursor is formed by stacking flaky coarse primary particles, and flaky fine primary particles grow in situ on the coarse primary particles.
Citation Information
Patent Citations
Ternary precursor in multiple crystal forms and preparation method of ternary precursor
CN109354077A
Nickel-cobalt binary precursor and preparation method thereof
CN113526573A
Preparation method of high-nickel ternary precursor washed by alkaline water
CN114057239A
Doped ternary precursor and preparation method thereof, ternary positive electrode material and lithium ion battery
CN115092974A
Method for preparing single-crystal ternary precursor
CN116199272A