Micron copper powder and its preparation method and application

By controlling the copper ion reduction process through multiple inorganic reduction reactions, spherical or quasi-spherical micron copper powder with high purity and uniform particle size is prepared, which solves the problem of uneven purity and particle size of copper powder in the existing technology and improves its performance in Application performance in the electronics industry.

CN116213747BActive Publication Date: 2024-10-29GUANGZHOU KECHENG ENVIRONMENTAL PROTECTION TECH

Patent Information

Application Number
CN202310173936.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-28
Publication Date
2024-10-29
Estimated Expiration
2043-02-28

AI Technical Summary

Technical Problem

The copper powder in the existing technology has low purity, uneven particle size, and unclear morphology, resulting in poor application results in the fields of multilayer ceramic capacitors, solar photovoltaic industries, and conductive adhesives.

Method used

By mixing the copper source, complexing agent, precipitant and solvent, adding the inorganic reducing agent in batches for multiple reduction reactions, the copper ion reduction process is controlled to form spherical or quasi-spherical micron copper powder to ensure uniform and uniform particle size. High purity.

Benefits of technology

The preparation of micron copper powder with high purity, high tap density and uniform particle size is achieved, which reduces production costs, simplifies wastewater treatment, and improves conductivity and application performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116213747B_ABST
    Figure CN116213747B_ABST
Patent Text Reader

Abstract

The present application relates to a micron copper powder and a preparation method thereof, wherein the preparation method of the micron copper powder comprises the following steps: mixing a copper source, a ligand, a precipitant and a solvent to obtain a copper-based mixed solution; adding a reducing agent to the copper-based mixed solution in batches for multiple times to perform a slow-release reduction reaction; and performing solid-liquid separation, washing and drying of the reaction product after the reaction to obtain a micron copper powder; wherein the number of the multiple reduction reactions is 3 times or more. The copper powder prepared by the preparation method of the micron copper powder provided in the present application has a spherical or quasi-spherical morphology, a uniform particle size and an average particle size of 1-5 μm, good dispersibility, high tap density and purity, and good conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of conductive material preparation, and in particular to a micron copper powder and a preparation method and application thereof. Background Art

[0002] With the development of the electronics industry, it has become a trend to replace precious metals such as silver and palladium with base metals represented by copper. The main reason is that copper not only has excellent conductivity, but also has a relatively low price. In multilayer ceramic capacitors (MLCCs), copper has replaced silver as the mainstream terminal electrode, and the core material for manufacturing copper terminal electrodes is copper powder. In addition, in the solar photovoltaic industry, heterojunction (HJT) cells are considered to be a new generation of photovoltaic cell technology. Due to its advantages such as high conversion efficiency, low attenuation rate, fewer process steps and clear cost reduction routes, it is expected to become the next generation of mainstream photovoltaic cells. HJT cells are low-temperature manufacturing processes. Silver-coated copper powder can be used instead of silver powder to prepare conductive slurry and then make metal electrodes, thereby greatly reducing the manufacturing cost of the battery. Among them, spherical micron copper powder is the basic raw material of silver-coated copper powder. In addition, in the conductive adhesive industry, there is also the potential and trend of copper powder replacing silver powder. The copper powder used in these related fields needs to meet the following characteristics: spherical or spherical morphology, high purity, uniform particle size, high tap density, etc. As for the particle size of copper powder, although small-sized ultrafine copper powder has obvious advantages, the smaller the size of copper powder, the easier it is to oxidize, and the effect is not good in actual application. Therefore, on the whole, spherical micron copper powder with a size of 1-5μm is the preferred raw material in the current electronic industry.

[0003] In the current technology for preparing spherical micron copper powder, on the one hand, the purity of copper powder is low, and the use of organic reducing agents increases the preparation cost and waste liquid treatment cost. On the other hand, the quality of copper powder does not meet the use requirements, mainly manifested in the small size (non-micron level), uneven particle size, unclear morphology, etc. Summary of the invention

[0004] Based on this, the purpose of the present application is to provide a spherical or quasi-spherical micron copper powder with high purity, high tap density and uniform particle size, and a preparation method and application thereof.

[0005] In one aspect of the present application, a method for preparing micron copper powder is provided, comprising the following steps:

[0006] Mixing a copper source, a complexing agent, a precipitant and a solvent to obtain a copper-based mixed solution;

[0007] Adding a reducing agent to the copper-based mixed solution in batches for multiple times to perform multiple reduction reactions; and

[0008] The reaction products after multiple reduction reactions are subjected to solid-liquid separation, washing and drying to obtain micron copper powder;

[0009] The number of the multiple reduction reactions is 3 or more, and the time of each reduction reaction is ≥ 30 min.

[0010] The first reduction reaction in the multiple reduction reactions is the first reduction reaction stage, the reducing agent added in the first reduction reaction stage is the first reducing agent, the last reduction reaction is the last reduction reaction stage, the reducing agent added in the last reduction reaction stage is the last reducing agent, the remaining reduction reactions are the intermediate reduction reaction stages, and the reducing agent added in the intermediate reduction reaction stages is the intermediate reducing agent:

[0011] The temperature of the first reduction reaction stage is 30°C to 85°C, and the amount of the first reducing agent is 30% to 50% of the total weight of the reducing agent added.

[0012] The temperature of the intermediate reduction reaction stage is 40°C to 105°C, and the amount of the intermediate reducing agent is 20% to 60% of the total weight of the added reducing agent.

[0013] The temperature of the last reduction reaction stage is 80° C. to 105° C., and the amount of the last reducing agent used is 5% to 40% of the total weight of the added reducing agent.

[0014] In some embodiments, the multiple reduction reactions are performed 3 to 5 times.

[0015] In some embodiments, the preparation method satisfies at least one of the following conditions:

[0016] (1) The time of the first reduction reaction stage is 30 min to 180 min;

[0017] (2) The duration of the intermediate reduction reaction stage is 30 min to 260 min;

[0018] (3) The duration of the final reduction reaction stage is 30 min to 240 min.

[0019] In some embodiments, the preparation method satisfies at least one of the following conditions:

[0020] (1) The ratio of the total molar amount of the reducing agent added to the molar amount of the copper element in the copper source is (0.4-4):1;

[0021] (2) The ratio of the molar amount of the complexing agent added to the molar amount of the copper element in the copper source can be (0.01-1):1;

[0022] (3) The ratio of the molar amount of the added precipitant to the molar amount of the copper element in the copper source can be (1-4):1.

[0023] In some embodiments, the reducing agent is an inorganic reducing agent.

[0024] In some embodiments, the inorganic reducing agent includes one or more of hydrazine hydrate, hydrazine hydrochloride, sodium hypophosphite, sodium phosphite, sodium sulfite, sodium dithionite, sodium borohydride and potassium borohydride.

[0025] In some embodiments, the copper source includes one or more of copper sulfate, basic copper sulfate, copper acetate, copper nitrate, copper chloride and basic copper chloride.

[0026] In some embodiments, the complexing agent includes one or more of ammonia, acetic acid, sodium acetate, ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate, tetrasodium ethylenediaminetetraacetate, triethanolamine, citric acid, sodium citrate, tartaric acid, sodium tartrate, salicylic acid, sodium salicylate, metaphosphoric acid, sodium metaphosphate, trimetaphosphoric acid, sodium trimetaphosphate, hexametaphosphoric acid, sodium hexametaphosphate, pyrophosphoric acid, sodium pyrophosphate, benzoic acid, sodium benzoate, glycine, lysine, aspartic acid and glutamic acid.

[0027] In some embodiments, the precipitant includes one or more of ammonia water, sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, ammonium carbonate, ammonium bicarbonate, potassium carbonate, oxalic acid, sodium oxalate and potassium oxalate.

[0028] In another aspect of the present application, copper powder prepared by the method for preparing micron copper powder is also provided.

[0029] In some of the embodiments, the copper particles in the copper powder are spherical or quasi-spherical, with an average particle size of 1 μm to 5 μm, a particle size distribution span of ≤1.5, and a copper content of ≥99%.

[0030] In some embodiments, the copper powder has a carbon content of ≤0.3wt% and a tap density of ≥3.5g / cm 3 .

[0031] In some embodiments, the carbon content of the copper powder is ≤0.02 wt %.

[0032] In another aspect, the present application further provides the use of the copper powder as a conductive material in electronic devices.

[0033] Compared with the prior art, this application has at least the following beneficial effects:

[0034] The preparation method of micron copper powder provided in the present application controls the process of reducing copper ions to elemental copper slowly through multiple reduction reactions, and the synergistic effect between the multiple reduction reactions jointly controls the formation process of elemental copper particles, so that the finally formed copper powder has a spherical or quasi-spherical morphology, uniform particle size with an average particle size of 1μm-5μm, good dispersibility, high tap density and purity, and good conductivity.

[0035] The preparation method of micron copper powder provided in the present application can use pure inorganic reducing agent in the aqueous system, effectively reducing the production cost. The prepared copper powder has high purity and low impurity content. At the same time, the organic matter content in the generated mother liquor is low. The process is environmentally friendly and the wastewater treatment is simple. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0037] Figure 1 This is a scanning electron microscope image of the copper powder prepared in Example 1;

[0038] Figure 2 This is a scanning electron microscope image of the copper powder prepared in Comparative Example 1;

[0039] Figure 3 This is a particle size distribution diagram of the copper powder prepared in Example 1;

[0040] Figure 4 This is the particle size distribution diagram of the copper powder prepared in Comparative Example 1. DETAILED DESCRIPTION

[0041] For ease of understanding of the application, reference to the embodiments of the application will now be provided in detail, one or more examples of which are described below. Each example is provided as an explanation rather than a limitation of the application. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the application more thorough and comprehensive. In fact, it is obvious to those skilled in the art that various modifications and changes can be made to the application without departing from the scope or spirit of the application. For example, the features described or described as part of an embodiment can be used in another embodiment to produce a further embodiment.

[0042] Therefore, it is intended that the present application covers such modifications and variations that fall within the scope of the appended claims and their equivalents. Other objects, features and aspects of the present application are disclosed in or are apparent from the following detailed description. It will be appreciated by those of ordinary skill in the art that this discussion is merely a description of exemplary embodiments and is not intended to limit the broader aspects of the present application.

[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0044] In this article, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions of the listed features.

[0045] Herein, when it comes to numerical ranges, unless otherwise specified, the numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0046] Only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an undefined range; and any lower limit can be combined with other lower limits to form an undefined range, and any upper limit can be combined with any other upper limit to form an undefined range. In addition, each separately disclosed point or single value itself can be combined with any other point or single value as a lower limit or upper limit or with other lower limits or upper limits to form an undefined range. The use of numerical ranges represented by endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4 and 5, etc.

[0047] Except as shown in the operating examples or otherwise indicated, all numbers used in the specification and claims to indicate the amounts of ingredients, physicochemical properties, etc. are understood to be adjusted in all cases by the term "about". For example, unless otherwise indicated, the numerical parameters listed in the above specification and the appended claims are approximate values, and those skilled in the art will be able to appropriately change these approximate values ​​to obtain the desired properties sought using the teachings disclosed herein.

[0048] On the one hand, the present application provides a method for preparing micron copper powder, comprising the following steps:

[0049] (a) mixing a copper source, a coordination agent, a precipitant and a solvent to obtain a copper-based mixed solution;

[0050] (b) adding a reducing agent to the copper-based mixed solution in batches for multiple times to perform multiple reduction reactions; and

[0051] (c) subjecting the reaction product to solid-liquid separation, washing and drying to obtain micron copper powder.

[0052] The copper source is not particularly limited, and may include, but is not limited to, copper sulfate, basic copper sulfate, copper acetate, copper nitrate, copper chloride, basic copper chloride, and combinations thereof.

[0053] The ligand is not particularly limited and may include, but is not limited to, aqueous ammonia, acetic acid, sodium acetate, ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate, tetrasodium ethylenediaminetetraacetate, triethanolamine, citric acid, sodium citrate, tartaric acid, sodium tartrate, salicylic acid, sodium salicylate, metaphosphoric acid, sodium metaphosphate, trimetaphosphoric acid, sodium trimetaphosphate, hexametaphosphoric acid, sodium hexametaphosphate, pyrophosphoric acid, sodium pyrophosphate, benzoic acid, sodium benzoate, glycine, lysine, aspartic acid, glutamic acid and combinations thereof.

[0054] The precipitant is not particularly limited and may include, but is not limited to, aqueous ammonia, sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, ammonium carbonate, ammonium bicarbonate, potassium carbonate, oxalic acid, sodium oxalate, potassium oxalate and combinations thereof.

[0055] The solvent is typically water.

[0056] The reducing agent is preferably an inorganic reducing agent. The inorganic reducing agent may include, but is not limited to, hydrazine hydrate, hydrazine hydrochloride, sodium hypophosphite, sodium phosphite, sodium sulfite, sodium dithionite, sodium borohydride, potassium borohydride, and combinations thereof.

[0057] The number of multiple reduction reactions may be 3 or more times, preferably 3 to 5 times.

[0058] The time of each reduction reaction shall not be less than 30 minutes.

[0059] The process of multiple reduction reactions is divided into the first reduction reaction, the last reduction reaction and the remaining reduction reactions. It can be understood that the remaining reduction reactions are reduction reactions other than the first reduction reaction and the last reduction reaction. It should be noted that each reduction reaction in the multiple reduction reactions refers to the start from the addition of the reducing agent. The time of adding the reducing agent is not counted in the time of the reduction reaction. The method of adding the reducing agent is not limited.

[0060] The first reduction reaction is the first reduction reaction stage, the last reduction reaction is the last reduction reaction stage, and the remaining reduction reactions are intermediate reduction reaction stages. The reducing agent added in the first reduction reaction stage is the first reducing agent. The reducing agent added in the last reduction reaction stage is the last reducing agent, and the reducing agent added in the intermediate reduction reaction stage is the intermediate reducing agent.

[0061] The temperature of the first reduction reaction stage is 30° C. to 85° C. The amount of the first reducing agent is 30% to 50% of the total amount of the added reducing agent. In some preferred embodiments, the time of the first reduction reaction stage is 30 min to 180 min.

[0062] In the above "30℃~85℃", the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: 35℃, 40℃, 45℃, 50℃, 55℃, 60℃, 65℃, 70℃, 75℃, 80℃; or a range consisting of any two numerical values, for example, it can be 35℃~85℃, 50℃~85℃, 65℃~85℃, 35℃~80℃, 50℃~80℃, 65℃~80℃, 35℃~70℃, 50℃~70℃, 60℃~70℃, 65℃~75℃.

[0063] In the above-mentioned "30%~50%", the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiment and the following point values: 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%; or a range consisting of any two numerical values, for example, it can be 35%~50%, 40%~50%, 45%~50%, 35%~45%, 35%~40%.

[0064] In the above "30min~180min", the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiment and the following point values: 40min, 50min, 60min, 70min, 80min, 90min, 100min, 110min, 120min, 130min, 140min, 150min, 160min, 170min; or a range consisting of any two numerical values, for example, it can be 40min~180min, 80min~180min, 120min~180min, 160min~180min, 40min~160min, 80min~160min, 120min~160min, 40min~140min, 80min~140min, 120min~140min, 40min~100min, 80min~100min, 80min~120min.

[0065] The temperature of the intermediate reduction reaction stage is 40° C. to 105° C. The amount of the intermediate reducing agent is 20% to 60% of the total amount of the added reducing agent. In some preferred embodiments, the time of the intermediate reduction reaction stage is 30 min to 260 min.

[0066] In the above-mentioned "40℃~105℃", the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: 45℃, 50℃, 55℃, 60℃, 65℃, 70℃, 75℃, 80℃, 85℃, 90℃, 95℃, 100℃; or a range consisting of any two numerical values, for example, it can be 45℃~105℃, 65℃~105℃, 85℃~105℃, 45℃~80℃, 60℃~80℃, 65℃~80℃, 45℃~70℃, 50℃~70℃, 60℃~70℃, 65℃~75℃.

[0067] In the above-mentioned "20%~60%", the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiment and the following point values: 25%, 30%, 35%, 40%, 45%, 50%, 55%; or a range consisting of any two numerical values, for example, it can be 25%~60%, 35%~60%, 45%~60%, 55%~60%, 25%~50%, 35%~50%, 45%~50%, 55%~50%, 25%~40%, 35%~40%.

[0068] In the above "30min~260min", the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiment and the following point values: 50min, 70min, 90min, 110min, 130min, 150min, 170min, 190min, 210min, 230min, 250min; or a range consisting of any two numerical values, for example, it can be 50min~260min, 110min~260min, 170min~260min, 230min~260min, 50min~210min, 110min~210min, 170min~210min, 50min~150min, 110min~150min.

[0069] The temperature of the last reduction reaction stage is 80° C. to 105° C. The amount of the last reducing agent used is 5% to 40% of the total amount of the added reducing agent. In some preferred embodiments, the time of the last reduction reaction stage is 30 min to 240 min.

[0070] In the above-mentioned "80℃~105℃", the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiment and the following point values: 81℃, 83℃, 85℃, 87℃, 90℃, 93℃, 95℃, 97℃, 100℃, 102℃; or a range consisting of any two numerical values, for example, it can be 85℃~105℃, 90℃~105℃, 95℃~105℃, 100℃~105℃, 85℃~100℃, 90℃~100℃, 95℃~100℃, 85℃~95℃, 85℃~90℃.

[0071] In the above-mentioned "5%~40%", the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiment and the following point values: 10%, 15%, 20%, 25%, 30%, 35%; or a range consisting of any two numerical values, for example, it can be 10%~40%, 15%~40%, 20%~40%, 25%~40%, 30%~40%, 35%~40%, 10%~35%, 15%~35%, 20%~35%, 20%~30%.

[0072] In the above "30min~240min", the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiment and the following point values: 50min, 70min, 90min, 110min, 130min, 150min, 170min, 190min, 210min, 230min; or a range consisting of any two numerical values, for example, it can be 50min~240min, 110min~240min, 170min~240min, 230min~240min, 50min~210min, 110min~210min, 170min~210min, 50min~150min, 110min~150min.

[0073] The ratio of the total molar amount of the added reducing agent to the molar amount of the copper element in the copper source can be any value between (0.4 and 4): 1. Understandably, the ratio of the total molar amount of the added reducing agent to the molar amount of the copper element in the copper source can include, but is not limited to, 0.4: 1, 0.8: 1, 1: 1, 1.5: 1, 2: 1, 2.5: 1, 3: 1, 3.5: 1, 4: 1.

[0074] The ratio of the molar amount of the added complexing agent to the molar amount of the copper element in the copper source can be any value between (0.01-1): 1. Understandably, the ratio of the molar amount of the added complexing agent to the molar amount of the copper element in the copper source can include, but is not limited to, 0.02: 1, 0.03: 1, 0.04: 1, 0.05: 1, 0.06: 1, 0.07: 1, 0.08: 1, 0.09: 1.

[0075] The ratio of the molar amount of the added precipitant to the molar amount of the copper element in the copper source can be any value between (1 to 4): 1. Understandably, the ratio of the molar amount of the added precipitant to the molar amount of the copper element in the copper source can include, but is not limited to, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1.

[0076] In another aspect, the present application provides copper powder prepared by the method for preparing micron copper powder described in any one of the above embodiments.

[0077] The copper particles in the copper powder can be spherical or quasi-spherical. The spherical or quasi-spherical copper particles can improve the flatness and density of the copper powder used as a conductive material to prepare a copper electrode.

[0078] The average particle size of the copper particles in the copper powder is 1 μm to 5 μm, and the particle size distribution span is ≤1.5.

[0079] The carbon content of the copper powder is ≤0.3wt%. The lower the carbon content, the better the conductivity of the copper powder. Too high a carbon content will reduce the conductivity of the copper powder. In some more preferred embodiments, the carbon content of the copper powder is ≤0.02wt%.

[0080] The tap density of copper powder is ≥3.5g / cm 3 If the tap density is too small, the porosity inside the electronic device (such as electrode) made of copper powder as a conductive material will increase, and the performance will deteriorate.

[0081] In another aspect, the present application further provides the use of the copper powder of any of the above embodiments as a conductive material in electronic devices. The electronic devices may include microelectronic devices, multilayer ceramic capacitors, solar cells, and the like.

[0082] The following are specific embodiments. The purpose is to further explain the present application in detail to help the technical personnel and researchers in the field to further understand the present application. The relevant technical conditions do not constitute any limitation to the present application. Any form of modification made within the scope of the claims of the present application is within the scope of protection of the claims of the present application.

[0083] Unless otherwise specified, the raw materials and reagents used in the following examples are all commercially available or can be prepared by known methods. The instruments are all conventionally selected in the art. The experimental methods without specific conditions in the examples are carried out according to conventional conditions, such as the conditions described in the literature, books or the methods recommended by the manufacturer.

[0084] Example 1

[0085] (1) Preparation of copper-based mixed solution

[0086] Add 200 mL of water to the reactor, start stirring, weigh 15 g of copper sulfate, 10 g of 20% ammonia water, and 6 g of sodium hydroxide and add them to the water. After adding, continue stirring until the mixed solution is evenly mixed.

[0087] (2) Slow-release reduction reaction

[0088] First reduction reaction: 3.94 g of hydrazine hydrate with a concentration of 80% was added to the mixed solution of step (1) for the first time, and the mixture was reacted at 50° C. for 30 min.

[0089] Second reduction reaction: add 1.576 g of hydrazine hydrate with a concentration of 80% for the second time and react at 105° C. for 145 min.

[0090] The third reduction reaction: 2.364 g of hydrazine hydrate with a concentration of 80% was added thereto for the third time, and the reaction was carried out at 105° C. for 135 min.

[0091] (3) Collecting copper powder

[0092] After the slow-release reduction reaction in step (2) is completed, the solid phase product is obtained by centrifugation, and washed with pure water. After washing, the product is placed in a vacuum drying oven and vacuum dried at 80° C. for 12 h to obtain spherical micron copper powder.

[0093] Example 2

[0094] (1) Preparation of copper-based mixed solution

[0095] Add 500 mL of water to the reactor, start stirring, weigh 111 g of basic copper carbonate, 54 g of sodium hydroxide, and 15 g of acetic acid and add them to the water. After adding, continue stirring until the mixed solution is mixed evenly.

[0096] (2) Slow-release reduction reaction

[0097] First reduction reaction: 26.4 g of sodium hypophosphite was added to the mixed solution of step (1) for the first time and reacted at 58° C. for 60 min.

[0098] Second reduction reaction: add 13.2 g of sodium hypophosphite for the second time and react at 80°C for 30 min.

[0099] The third reduction reaction: add 26.4 g of sodium hypophosphite for the third time and react at 93° C. for 240 min.

[0100] (3) Collecting copper powder

[0101] After the slow-release reduction reaction in step (2) is completed, the solid phase product is filtered and washed with ethanol. After washing, the product is placed in a vacuum drying oven and vacuum dried at 60° C. for 8 h to obtain spherical micron copper powder.

[0102] Example 3

[0103] (1) Preparation of copper-based mixed solution

[0104] Add 800 mL of water to the reactor, start stirring, weigh 256.27 g of basic cupric chloride, 9.13 g of tetrasodium ethylenediaminetetraacetate, and 279.8 g of sodium carbonate and add them to the water. After adding, continue stirring until the mixture is evenly mixed.

[0105] (2) Slow-release reduction reaction

[0106] First reduction reaction: 13.62 g of sodium borohydride was added to the mixed solution of step (1) for the first time, and the mixture was reacted at 60° C. for 100 min.

[0107] Second reduction reaction: add 18.16 g of sodium borohydride for the second time and react at 90° C. for 90 min.

[0108] The third reduction reaction: 13.62 g of sodium borohydride was added for the third time and the reaction was carried out at 105° C. for 180 min.

[0109] (3) Collecting copper powder

[0110] After the reduction reaction in step (2) is completed, the solid phase product is filtered out and washed with pure water. After washing, the product is placed in a vacuum drying oven and vacuum dried at 60° C. for 10 h to obtain spherical micron copper powder.

[0111] Example 4

[0112] (1) Preparation of copper-based mixed solution

[0113] Add 1L of water to the reactor, start stirring, weigh 129g of sodium oxalate, 12g of tartaric acid, and 200g of copper sulfate and add them to the water. After adding, continue stirring until the mixture is evenly mixed.

[0114] (2) Slow-release reduction reaction

[0115] First reduction reaction: 5.53 g of potassium borohydride was added to the mixed solution of step (1) for the first time, and the reaction was carried out at 30° C. for 180 min.

[0116] Second reduction reaction: add 5.88 g of potassium borohydride for the second time and react at 40°C for 30 min.

[0117] The third reduction reaction: 1.04 g of potassium borohydride was added for the third time and reacted at 40° C. for 60 min.

[0118] Fourth reduction reaction: 4.84 g of potassium borohydride was added for the fourth time and reacted at 80° C. for 30 min.

[0119] (3) Collecting copper powder

[0120] After the slow-release reduction reaction in step (2) is completed, the solid phase product is filtered and washed with pure water. After washing, the product is placed in a vacuum freeze drying box and vacuum freeze-dried for 10 hours to obtain spherical micron copper powder.

[0121] Example 5

[0122] (1) Preparation of copper-based mixed solution

[0123] Add 2L of water to the reactor, start stirring, weigh 1200g of copper nitrate, 477.44g of triethanolamine, and 922.56g of ammonium carbonate and add them to the water. After adding, continue stirring until the mixed solution is mixed evenly.

[0124] (2) Slow-release reduction reaction

[0125] First reduction reaction: 525.63 g of hydrazine hydrate with a concentration of 80% was added to the mixed solution of step (1) for the first time, and the reaction was carried out at 85° C. for 105 min.

[0126] Second reduction reaction: add 150.18 g of hydrazine hydrate with a concentration of 80% for the second time and react at 73° C. for 80 min.

[0127] The third reduction reaction: 300.36 g of hydrazine hydrate with a concentration of 80% was added thereto for the third time, and the reaction was carried out at 73° C. for 80 min.

[0128] Fourth reduction reaction: 450.54 g of hydrazine hydrate with a concentration of 80% was added thereto for the fourth time, and the reaction was carried out at 73° C. for 100 min.

[0129] The fifth reduction reaction: 75.09 g of hydrazine hydrate with a concentration of 80% was added to the fourth reaction mixture, and the reaction was carried out at 100° C. for 75 min.

[0130] (3) Collecting copper powder

[0131] After the slow-release reduction reaction in step (2) is completed, the solid phase product is filtered and washed with ethanol. After washing, the product is placed in an oven filled with nitrogen and dried at 65° C. for 15 h to obtain spherical micron copper powder.

[0132] Comparative Example 1

[0133] (1) Preparation of copper-based mixed solution

[0134] Add 200 mL of water to the reactor, start stirring, weigh 15 g of copper sulfate and 6 g of sodium hydroxide and add them to the water. After adding, continue stirring until the mixed solution is mixed evenly.

[0135] (2) Slow-release reduction reaction

[0136] First reduction reaction: 3.94 g of hydrazine hydrate with a concentration of 80% was added to the mixed solution of step (1) for the first time, and the mixture was reacted at 50° C. for 30 min.

[0137] Second reduction reaction: add 1.576 g of hydrazine hydrate with a concentration of 80% for the second time and react at 105° C. for 145 min.

[0138] The third reduction reaction: 2.364 g of hydrazine hydrate with a concentration of 80% was added thereto for the third time, and the reaction was carried out at 105° C. for 135 min.

[0139] (3) Collecting copper powder

[0140] After the slow-release reduction reaction in step (2) is completed, the solid phase product is obtained by centrifugation, and washed with pure water. After washing, the product is placed in a vacuum drying oven and vacuum dried at 80° C. for 12 h to obtain copper powder.

[0141] Comparative Example 2

[0142] (1) Preparation of copper-based mixed solution

[0143] Add 200 mL of water to the reactor, start stirring, weigh 15 g of copper sulfate and 10 g of 20% ammonia water and add them to the water. After adding, continue stirring until the mixed solution is mixed evenly.

[0144] (2) Slow-release reduction reaction

[0145] First reduction reaction: 3.94 g of hydrazine hydrate with a concentration of 80% was added to the mixed solution of step (1) for the first time, and the mixture was reacted at 50° C. for 30 min.

[0146] Second reduction reaction: add 1.576 g of hydrazine hydrate with a concentration of 80% for the second time and react at 105° C. for 145 min.

[0147] The third reduction reaction: 2.364 g of hydrazine hydrate with a concentration of 80% was added thereto for the third time, and the reaction was carried out at 105° C. for 135 min.

[0148] (3) Collecting copper powder

[0149] After the slow-release reduction reaction in step (2) is completed, the solid phase product is obtained by centrifugation, and washed with pure water. After washing, the product is placed in a vacuum drying oven and vacuum dried at 80° C. for 12 h to obtain copper powder.

[0150] Comparative Example 3

[0151] (1) Preparation of copper-based mixed solution

[0152] Add 200 mL of water to the reactor, start stirring, weigh 15 g of copper sulfate, 10 g of 20% ammonia water, and 6 g of sodium hydroxide and add them to the water. After adding, continue stirring until the mixed solution is evenly mixed.

[0153] (2) Controlling the reduction reaction

[0154] First reduction reaction: 4.1 g of hydrazine hydrate with a concentration of 80% was added to the mixed solution of step (1) for the first time, and the mixture was reacted at 50° C. for 30 min.

[0155] Second reduction reaction: add 3.78 g of hydrazine hydrate with a concentration of 80% for the second time and react at 105° C. for 280 min.

[0156] (3) Collecting copper powder

[0157] After the reduction reaction in step (2) is completed, the solid phase product is obtained by centrifugation, and washed with pure water. After washing, the product is placed in a vacuum drying oven and vacuum dried at 80° C. for 12 h to obtain copper powder.

[0158] Comparative Example 4

[0159] (1) Preparation of copper-based mixed solution

[0160] Add 1L of water to the reactor, start stirring, weigh 125g of copper sulfate and 60g of sodium hydroxide and add them to the water. After adding, continue stirring until the mixed solution is mixed evenly.

[0161] (2) Reduction reaction

[0162] Add 265 g of ascorbic acid to the mixed solution of step (1) and react at 90° C. for 120 min.

[0163] (3) Collecting copper powder

[0164] After the reduction reaction in step (2) is completed, the solid phase product is obtained by centrifugation, and washed with pure water. After washing, the product is placed in a vacuum drying oven and vacuum dried at 80° C. for 12 h to obtain copper powder.

[0165] Comparative Example 5

[0166] (1) Preparation of copper-based mixed solution

[0167] Add 1L of water to the reactor, start stirring, weigh 125g of copper sulfate, 87.5g of 20% ammonia water, and 80g of sodium hydroxide and add them to the water. After adding, continue stirring until the mixed solution is mixed evenly.

[0168] (2) Reduction reaction

[0169] Add 360.32 g of glucose to the mixed solution of step (1) and react at 90° C. for 120 min.

[0170] (3) Collecting copper powder

[0171] After the reduction reaction in step (2) is completed, the solid phase product is obtained by centrifugation, and washed with pure water. After washing, the product is placed in a vacuum drying oven and vacuum dried at 80° C. for 12 h to obtain copper powder.

[0172] Comparative Example 6

[0173] (1) Preparation of copper-based mixed solution

[0174] Add 200 mL of water to the reactor, start stirring, weigh 15 g of copper sulfate, 10 g of 20% ammonia water, and 6 g of sodium hydroxide and add them to the water. After adding, continue stirring until the mixed solution is evenly mixed.

[0175] (2) Slow-release reduction reaction

[0176] First reduction reaction: 3.94 g of hydrazine hydrate with a concentration of 80% was added to the mixed solution of step (1) for the first time, and the mixture was reacted at 50° C. for 10 min.

[0177] Second reduction reaction: add 1.576 g of hydrazine hydrate with a concentration of 80% for the second time and react at 105° C. for 15 min.

[0178] The third reduction reaction: add 2.364 g of hydrazine hydrate with a concentration of 80% for the third time and react at 105° C. for 20 min.

[0179] (3) Collecting copper powder

[0180] After the reduction reaction in step (2) is completed, the solid phase product is obtained by centrifugation, and washed with pure water. After washing, the product is placed in a vacuum drying oven and vacuum dried at 80° C. for 12 h to obtain copper powder.

[0181] Comparative Example 7

[0182] (1) Preparation of copper-based mixed solution

[0183] Add 200 mL of water to the reactor, start stirring, weigh 15 g of copper sulfate, 10 g of 20% ammonia water, and 6 g of sodium hydroxide and add them to the water. After adding, continue stirring until the mixed solution is evenly mixed.

[0184] (2) Slow-release reduction reaction

[0185] First reduction reaction: 3.94 g of hydrazine hydrate with a concentration of 80% was added to the mixed solution of step (1) for the first time, and the mixture was reacted at 50° C. for 30 min.

[0186] Second reduction reaction: add 1.576 g of hydrazine hydrate with a concentration of 80% for the second time and react at 70° C. for 145 min.

[0187] The third reduction reaction: 2.364 g of hydrazine hydrate with a concentration of 80% was added for the third time and the reaction was carried out at 70° C. for 135 min.

[0188] (3) Collecting copper powder

[0189] After the reduction reaction in step (2) is completed, the solid phase product is obtained by centrifugation, and washed with pure water. After washing, the product is placed in a vacuum drying oven and vacuum dried at 80° C. for 12 h to obtain copper powder.

[0190] Comparative Example 8

[0191] (1) Preparation of copper-based mixed solution

[0192] Add 200 mL of water to the reactor, start stirring, weigh 15 g of copper sulfate, 10 g of 20% ammonia water, and 6 g of sodium hydroxide and add them to the water. After adding, continue stirring until the mixed solution is evenly mixed.

[0193] (2) Slow-release reduction reaction

[0194] First reduction reaction: 2.364 g of hydrazine hydrate with a concentration of 80% was added to the mixed solution of step (1) for the first time, and the mixture was reacted at 50° C. for 30 min.

[0195] Second reduction reaction: add 1.576 g of hydrazine hydrate with a concentration of 80% for the second time and react at 105° C. for 145 min.

[0196] The third reduction reaction: 3.94 g of hydrazine hydrate with a concentration of 80% was added thereto for the third time, and the reaction was carried out at 105° C. for 135 min.

[0197] (3) Collecting copper powder

[0198] After the reduction reaction in step (2) is completed, the solid phase product is obtained by centrifugation, and washed with pure water. After washing, the product is placed in a vacuum drying oven and vacuum dried at 80° C. for 12 h to obtain copper powder.

[0199] Comparative Example 9

[0200] (1) Preparation of copper-based mixed solution

[0201] Add 200 mL of water to the reactor, start stirring, weigh 15 g of copper sulfate, 10 g of 20% ammonia water, and 6 g of sodium hydroxide and add them to the water. After adding, continue stirring until the mixed solution is evenly mixed.

[0202] (2) Slow-release reduction reaction

[0203] First reduction reaction: 4.728 g of hydrazine hydrate with a concentration of 80% was added to the mixed solution of step (1) for the first time, and the mixture was reacted at 50° C. for 30 min.

[0204] Second reduction reaction: add 1.576 g of hydrazine hydrate with a concentration of 80% for the second time and react at 105° C. for 145 min.

[0205] The third reduction reaction: 1.576 g of hydrazine hydrate with a concentration of 80% was added for the third time, and the reaction was carried out at 105° C. for 135 min.

[0206] (3) Collecting copper powder

[0207] After the reduction reaction in step (2) is completed, the solid phase product is obtained by centrifugation, and washed with pure water. After washing, the product is placed in a vacuum drying oven and vacuum dried at 80° C. for 12 h to obtain copper powder.

[0208] Comparative Example 10

[0209] (1) Preparation of copper-based mixed solution

[0210] Add 200 mL of water to the reactor, start stirring, weigh 15 g of copper sulfate, 10 g of 20% ammonia water, and 6 g of sodium hydroxide and add them to the water. After adding, continue stirring until the mixed solution is evenly mixed.

[0211] (2) Slow-release reduction reaction

[0212] First reduction reaction: 3.94 g of hydrazine hydrate with a concentration of 80% was added to the mixed solution of step (1) for the first time, and the mixture was reacted at 50° C. for 30 min.

[0213] Second reduction reaction: add 0.788 g of hydrazine hydrate with a concentration of 80% for the second time and react at 105° C. for 145 min.

[0214] The third reduction reaction: 3.152 g of hydrazine hydrate with a concentration of 80% was added thereto for the third time, and the reaction was carried out at 105° C. for 135 min.

[0215] (3) Collecting copper powder

[0216] After the reduction reaction in step (2) is completed, the solid phase product is obtained by centrifugation, and washed with pure water. After washing, the product is placed in a vacuum drying oven and vacuum dried at 80° C. for 12 h to obtain copper powder.

[0217] The raw materials, reactants and reaction conditions in Examples 1 to 5 and Comparative Examples 1 to 10 are listed in Table 1 below, and the performance indicators of the products are listed in Table 2 below:

[0218] Among them, the test methods or test standards for each product performance test item are:

[0219] (1) Morphology and average particle size: Observe and measure using a scanning electron microscope (SEM). Figure 1 The copper powder shown is a dense, discrete, independently formed particle with a relatively regular smooth surface. The structure similar to a sphere is called a quasi-spherical morphology. On the contrary, if there is no dense, discrete, independently formed structure (such as loose, agglomerated, etc.), a smooth surface, uneven surface shape, different lengths, eccentricity, etc., it is an irregular morphology.

[0220] (2) Particle size distribution span: (D90-D10) / D50, where D10, D50, and D90 are tested using a laser particle size analyzer (model: LS-800).

[0221] (3) Copper content: The detection method refers to the national standard "Chemical analysis methods for copper and copper alloys Part 1: Determination of copper content" (GB / T 5121.1-2008).

[0222] (4) Tap density: The detection method refers to the national standard "Determination of tap density of metal powders" (GB / T5162-2021).

[0223] (5) Carbon content: tested using a carbon-sulfur analyzer (model: CS844).

[0224] (6) Mother liquor TOC: Use a total organic carbon analyzer (model: TOC-L) for testing.

[0225] Table 1

[0226]

[0227]

[0228] Table 2

[0229]

[0230] It can be seen from the data in Table 1 and Table 2 that in the above embodiment, the copper-based mixed solution is prepared by using a complexing agent and a precipitating agent, and the reducing agent is added in batches for 3 times or more, and the interval between each batch is not less than 30 minutes. The morphology of the prepared copper powder is spherical, the D50 particle size is 1 to 5 μm, and the tap density is greater than 4 g / cm 3 , the particle size distribution span (SPAN) is not greater than 1.5, indicating that the copper powder particle size is relatively uniform. At the same time, the TOC content in the mother liquor of the above embodiment is low (≤2500 mg / L), the process is environmentally friendly, and the wastewater treatment cost is low.

[0231] In Comparative Examples 1 and 2, the absence of either a coordinating agent or a precipitating agent in the preparation of the copper-based mixed solution will result in irregular morphology, a large SPAN value, and non-uniform particle size of the prepared copper powder.

[0232] In Comparative Example 3, when the reducing agent was added in batches twice, the morphology of the prepared copper powder was also irregular, the SPAN value was large, and the particle size was uneven.

[0233] In Comparative Examples 4 and 5, the copper powder prepared by a single reduction reaction using an organic reducing agent (ascorbic acid and glucose) has an irregular morphology, a large SPAN value, an uneven particle size, and a TOC content in its production mother liquor as high as 40,000 to 50,000 mg / L. The process is not environmentally friendly, and wastewater treatment is difficult and costly.

[0234] Comparing Comparative Examples 6 to 10 with Examples 1 to 5, factors such as the reduction reaction time after the reducing agent is added in batches, the reduction reaction temperature, and the amount of reducing agent added in batches will cause the reduction reaction to be unable to proceed in a sustained manner, affecting the reaction process, resulting in irregular morphology and uneven particle size of the final copper powder.

[0235] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0236] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.

Claims

1. A method for preparing micron copper powder, characterized in that: The following steps are involved: Mixing a copper source, a complexing agent, a precipitant and a solvent to obtain a copper-based mixed solution; Adding a reducing agent to the copper-based mixed solution in batches for multiple times to perform multiple reduction reactions; and The reaction products after multiple reduction reactions are subjected to solid-liquid separation, washing and drying to obtain micron copper powder; The number of the multiple reduction reactions is 3 or more, and the time of each reduction reaction is ≥ 30 min. In the multiple reduction reactions, the first reduction reaction is the first reduction reaction stage, the last reduction reaction is the last reduction reaction stage, and the remaining reduction reactions are intermediate reduction reaction stages. The reducing agent added in the first reduction reaction stage is the first reducing agent, the reducing agent added in the last reduction reaction stage is the last reducing agent, and the reducing agent added in the intermediate reduction reaction stage is the intermediate reducing agent: The temperature of the first reduction reaction stage is 30°C to 85°C, and the amount of the first reducing agent is 30% to 50% of the total weight of the reducing agent added. The temperature of the intermediate reduction reaction stage is 40°C to 105°C, and the amount of the intermediate reducing agent is 20% to 60% of the total weight of the added reducing agent. The temperature of the final reduction reaction stage is 80°C to 105°C, and the amount of the final reducing agent is 5% to 40% of the total weight of the added reducing agent; The reducing agent is an inorganic reducing agent, and the inorganic reducing agent includes one or more of hydrazine hydrate, hydrazine hydrochloride, sodium hypophosphite, sodium phosphite, sodium sulfite, sodium dithionite, sodium borohydride and potassium borohydride; The copper particles in the copper powder prepared by the preparation method are spherical or quasi-spherical, with an average particle size of 1 μm to 5 μm, a particle size distribution span of ≤1.5, and a copper content of ≥99%.

2. The method for preparing micron copper powder according to claim 1, characterized in that: The number of the multiple reduction reactions is 3 to 5 times.

3. The method for preparing micron copper powder according to claim 1, characterized in that: At least one of the following conditions is met: (1) The duration of the first reduction reaction stage is 30 min to 180 min; (2) The duration of the intermediate reduction reaction stage is 30 min to 260 min; (3) The duration of the final reduction reaction stage is 30 min to 240 min.

4. The method for preparing micron copper powder according to claim 1, characterized in that: At least one of the following conditions is met: (1) The ratio of the total molar amount of the added reducing agent to the molar amount of the copper element in the copper source is (0.4-4):1; (2) The ratio of the molar amount of the complexing agent added to the molar amount of the copper element in the copper source is (0.01-1):1; (3) The ratio of the molar amount of the added precipitant to the molar amount of the copper element in the copper source is (1-4):

1.

5. The method for preparing micron copper powder according to any one of claims 1 to 4, characterized in that: The copper source includes one or more of copper sulfate, basic copper sulfate, copper acetate, copper nitrate, copper chloride and basic copper chloride.

6. The method for preparing micron copper powder according to any one of claims 1 to 4, characterized in that: The complexing agent includes one or more of ammonia water, acetic acid, sodium acetate, ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate, tetrasodium ethylenediaminetetraacetate, triethanolamine, citric acid, sodium citrate, tartaric acid, sodium tartrate, salicylic acid, sodium salicylate, metaphosphoric acid, sodium metaphosphate, trimetaphosphoric acid, sodium trimetaphosphate, hexametaphosphoric acid, sodium hexametaphosphate, pyrophosphoric acid, sodium pyrophosphate, benzoic acid, sodium benzoate, glycine, lysine, aspartic acid and glutamic acid.

7. The method for preparing micron copper powder according to any one of claims 1 to 4, characterized in that: The precipitant includes one or more of ammonia water, sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, ammonium carbonate, ammonium bicarbonate, potassium carbonate, oxalic acid, sodium oxalate and potassium oxalate.

8. The copper powder prepared by the method for preparing micron copper powder according to any one of claims 1 to 7, characterized in that: The copper powder has a carbon content of ≤0.3wt% and a tap density of ≥3.5 g / cm 3 .

9. The copper powder according to claim 8, characterized in that The carbon content of the copper powder is ≤0.02wt%.

10. Use of the copper powder prepared by the preparation method according to any one of claims 1 to 7 or the copper powder according to any one of claims 8 to 9 as a conductive material in electronic devices.

Citation Information

Patent Citations

  • Method for preparing compact silver-coated copper powder by using one pot method

    CN103128308A

  • Spherical nanometer copper powder as well as preparation method and application thereof

    CN111957986A

  • Preparation method of silver-coated copper powder

    CN113020587A

  • Preparation method for electronic-grade high-purity low-apparent-density dendritic copper powder

    CN113832500A

  • Preparation method and application of micron copper powder

    CN114749677A