Method for preparing rock wool from blast furnace slag, prepared rock wool and application
By melting blast furnace slag and other raw materials in an electric furnace to prepare rock wool, the problem of low utilization rate of blast furnace slag and environmental pollution is solved, the goals of efficient utilization and circular economy are achieved, and the added value of rock wool products is increased.
Patent Information
- Application Number
- CN202410749895.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-01
AI Technical Summary
The comprehensive utilization rate of blast furnace slag is low, and the proportion of blast furnace slag in existing rock wool production is too low, leading to resource waste and environmental pollution, and traditional raw material mining causes environmental damage.
By mixing blast furnace slag, silica sand, iron tailings, bauxite and other raw materials, and heating and melting them in an electric furnace, rock wool with a high acidity coefficient that meets national standards is prepared, and the proportion of blast furnace slag in the rock wool raw materials is increased to More than 50%, replacing traditional basalt and dolomite.
It achieves efficient utilization of blast furnace slag, increases the added value of rock wool products, promotes circular economy, reduces carbon emissions, and reduces the exploitation of natural resources and environmental damage.
Smart Images

Figure CN118724470A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of comprehensive utilization of smelting solid waste, and more specifically, to a method for preparing rock wool using blast furnace slag, the prepared rock wool and applications. Background Art
[0002] Blast furnace slag is the waste slag produced when smelting pig iron. When smelting iron in a blast furnace, raw materials such as sintered ore, pelletized ore, lump ore, coke and coal powder are added. As the charge descends, iron oxides such as sintered ore, pelletized ore and lump ore are gradually reduced and reduced to molten iron at 1400-1500℃, while impurities such as gangue and ash that cannot enter pig iron form slag mainly composed of aluminosilicates. The chemical composition of blast furnace slag is mainly composed of CaO, SiO2, MgO and Al2O3, and these four components account for about 90% of the blast furnace slag components.
[0003] Blast furnace slag is the main byproduct of pig iron smelting and the largest solid waste slag produced in the metallurgical industry. Every ton of pig iron produced produces about 300 kg of blast furnace slag. At present, the comprehensive utilization rate of blast furnace slag in my country is about 90%, and the utilization rate in the northern region is lower, while the utilization rate of blast furnace slag abroad is basically 100%. It can be seen that further research is needed on the comprehensive utilization of blast furnace slag, to expand the application of blast furnace slag, to improve the resource utilization rate, and to reduce the accumulation of blast furnace slag, which occupies a large amount of land and causes pollution to the surrounding environment.
[0004] At present, the comprehensive utilization of blast furnace slag is mainly in the field of building materials, and the added value of the products is low, such as: blast furnace slag is used as a raw material for cement to produce slag silicate cement; blast furnace slag is ground into slag powder and used as an admixture for concrete; blast furnace slag is used as a raw material, and auxiliary raw materials are added to mix to prepare new road construction materials; blast furnace slag has potential hydration activity, and the activity can be stimulated through a series of treatments to prepare wall bricks. In terms of high added value applications of blast furnace slag, such as the preparation of microcrystalline glass, new ceramic materials, agricultural fertilizers, and adsorbents for treating industrial wastewater, it is still in the laboratory research stage and has no specific practical application.
[0005] In the metallurgical industry, the slag produced by the blast furnace is condensed without any treatment to form a slag block called dry slag. Taking advantage of its alkalinity, it can be used to prepare the raw materials for rock wool insulation materials. In the current industry's rock wool production and manufacturing process, the main raw materials for preparing rock wool products are basalt (accounting for about 65%), with some dolomite (accounting for 15%), and a small amount of dry slag (accounting for 20%). Among the raw materials of rock wool products, solid waste blast furnace slag is only added in a small amount, and the main raw materials are basalt and dolomite, both of which are natural mineral resources. During the mining process, it is easy to cause damage to the environment. Summary of the invention
[0006] In view of the defects existing in the prior art, the purpose of the present invention is to provide a method for preparing rock wool using blast furnace slag, the prepared rock wool and its application, which can increase the proportion of smelting solid waste blast furnace slag (dry slag) in the rock wool raw materials, so that blast furnace slag is used as the main raw material, and the proportion is increased to more than 50%, and the quality of the rock wool product is not affected, and the requirements of the national rock wool product standard GB / T 25975-2018 are also met.
[0007] To achieve the above object, the present invention adopts the following technical solution:
[0008] A first aspect of the present invention provides a method for preparing rock wool using blast furnace slag, comprising the following steps:
[0009] S1, uniformly mixing blast furnace slag, silica sand, iron tailings, bauxite and serpentine to prepare a mixture;
[0010] S2, putting the mixed material into an electric furnace, heating and melting the mixed material in the electric furnace to obtain rock wool.
[0011] Preferably, the blast furnace slag is the main raw material, accounting for 50-60% by mass of the total raw materials in the proportion;
[0012] The silica sand, the iron tailings, the bauxite and the serpentine are respectively measured and distributed, and in the proportion, they account for 10-16%, 10-18%, 7-12% and 5-10% of the mass percentage of the total raw materials respectively.
[0013] Preferably, the blast furnace slag, the silica sand, the iron tailings, the bauxite, and the serpentine are accurately measured, unloaded layer by layer on a belt conveyor, and transported to a loading bin to become the mixed material.
[0014] Preferably, the mixed material is uniformly added into the electric furnace according to the hourly production requirement, 40% is added into the central feeding point of the electric furnace, and 10% is added into each of the other 6 feeding points.
[0015] Preferably, the heating temperature of the electric furnace is ≥1500°C.
[0016] Preferably, the rock wool comprises the following components by mass percentage:
[0017] SiO2: 43-48%;
[0018] Al2O3: 12-15%;
[0019] MgO: 6-9%;
[0020] CaO: 18-24%;
[0021] FeO: 3-5%;
[0022] Fe2O3: 3-5%;
[0023] Na2O+K2O≤4%.
[0024] Preferably, the acidity coefficient of the rock wool is ≥1.8.
[0025] Preferably, the melting temperature of the rock wool is ≤1500°C, and the viscosity at 1400-1480°C is 1.0-3.0 Pa.S.
[0026] The second aspect of the present invention provides a rock wool, which is prepared by the method for preparing rock wool using blast furnace slag provided by the first aspect of the present invention.
[0027] The third aspect of the present invention provides an application of rock wool, wherein the rock wool provided by the second aspect of the present invention is used for external thermal insulation of the exterior wall of a building.
[0028] The method for preparing rock wool using blast furnace slag, the prepared rock wool and its application provided by the present invention have the following beneficial effects:
[0029] 1) Using blast furnace slag (dry slag) as the main raw material and adding some other raw materials to adjust the composition, it can be made into rock wool board for external insulation of building exterior walls, which is an excellent and high-end rock wool product on the market;
[0030] 2) The raw material ratio technology is not only applicable to the production of rock wool from cold charge electric furnaces, but also to the production of rock wool with high acidity coefficient from hot molten slag;
[0031] 3) Blast furnace slag replaces basalt and dolomite in traditional rock wool raw materials, and with the addition of iron tailings solid waste, the proportion of solid waste in rock wool raw materials reaches more than 70%, turning waste into treasure, promoting the circular economy, and reducing carbon emissions from the rock wool manufacturing industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a schematic diagram of the on-site process of the method for preparing rock wool using blast furnace slag of the present invention;
[0033] Figure 2 This is a schematic diagram of the relationship between the viscosity and temperature of rock wool in Example 1 of the method for preparing rock wool using blast furnace slag of the present invention. DETAILED DESCRIPTION
[0034] In order to better understand the above technical solution of the present invention, the technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0035] The key core technology for high value-added utilization of blast furnace slag lies in the chemical composition of the blast furnace slag selected for application, and the targeted selection of other raw materials to supplement its SiO2, Al2O3, MgO, FeO and Fe2O3. The goal of formulation is first to adjust the acidity coefficient of the mixture to above 1.8, and secondly to focus on the balance of the chemical composition of the mixture, such as SiO2, Al2O3, MgO, CaO, etc. Various components meet the composition of the rock wool melt for external insulation of building exterior walls, and the high-temperature viscosity test is used to judge the length of the material properties. Only materials with long properties are suitable for the preparation of rock wool fibers. Only when the above conditions are met can the mixed raw materials prepare external wall insulation rock wool products with high acidity coefficients.
[0036] The present invention provides a method for preparing rock wool using blast furnace slag, comprising the following steps:
[0037] S1, blast furnace slag (dry slag) and other raw materials are mixed evenly in proportion and then set aside;
[0038] Specifically, blast furnace slag (dry slag) and other raw materials are crushed to less than 20 mm and stored in corresponding silos. Figure 1 As shown, in the specific process, blast furnace slag 1, silica sand 2, iron tailings 3, bauxite 4 and serpentine 5 are weighed and discharged on the same conveyor belt 6 according to the mass ratio. The corresponding raw material mass ratios are 50-60%, 10-16%, 10-18%, 7-12%, and 5-10%, respectively. The chemical composition of various raw materials is shown in Table 1 below. The acidity coefficient of the mixed raw material components after proportioning must be greater than 1.8, and they are transported together to the silo 7 for charging the electric furnace. According to the production organization plan of the electric furnace, a certain amount of mixed raw materials are evenly added to the electric furnace 8.
[0039] Table 1 Main components of blast furnace slag and other raw materials
[0040]
[0041] Blast furnace slag (dry slag) is used as the main raw material, and some other raw materials are added to prepare rock wool components. The design principle is as follows: According to the structural theory of silicate network, SiO2 is the main network former, and a stable covalent bond is formed between silicon atoms and oxygen atoms. One silicon atom combines with four oxygen atoms to form a stable silicon-oxygen tetrahedron structure, forming the skeleton of the fiber. In the combined design, a high SiO2 content is conducive to improving the fiber strength and length, but it will increase the melt viscosity; AL2O3 can improve the chemical stability of the fiber and also increase the viscosity of the melt. The alkaline oxide CaO has the opposite effect to the acidic oxide, which can depolymerize the complex network structure composed of SiO2 and AL2O3, reduce the viscosity of the melt, and increase the fluidity of the melt. MgO and CaO have similar effects. They can replace CaO to a certain extent in rock wool fibers, improve the chemical durability of fibers, and expand the viscosity range of melt fiberization, which is beneficial to the actual process operation of preparing rock wool fibers. However, when the MgO content is high, it is not conducive to melt fiberization and is easy to produce slag balls, which increases the slag ball content in the fiber and reduces the performance of the fiber. Iron in the fiber exists in the form of Fe2+ and Fe3+, and iron oxide affects the melt viscosity, color and fire resistance of rock wool products.
[0042] (2) According to the control requirements of the hourly output, the mixed raw materials are uniformly fed into the electric furnace, and the high-quality rock wool melt is obtained after the temperature is raised and melted in the electric furnace;
[0043] Specifically, an electric furnace melting process is adopted, and the materials are fed into the electric furnace at a uniform speed through the feeding bin of the electric furnace and weighed (output when the control console is turned on), wherein the materials are fed into the center of the electric furnace for 40% and the materials are fed into the periphery for 60%. The temperature in the electric furnace is heated to ≥1500°C. After melting, the electric furnace is slag-discharging to obtain a rock wool melt with an acidity coefficient ≥1.8. In a specific embodiment, the acidity coefficient of the rock wool melt is 1.8-2.0.
[0044] The composition of the rock wool melt obtained above is shown in Table 2 below, specifically including the following components by mass percentage:
[0045] Table 2 Composition of rock wool melt for external wall insulation (%)
[0046]
[0047] The rock wool melt obtained above is in liquid state at a temperature ≥1500°C; the viscosity of the rock wool melt at 1350-1490°C is 1.0-3.0 Pa.S, and the material properties are long. It can be seen that it has the conditions for fiberization in the subsequent process.
[0048] (3) The rock wool melt passes through a four-roller centrifuge and a whole board wool line equipment to prepare rock wool products for exterior wall insulation.
[0049] The present invention also provides a rock wool, which is prepared by the method for preparing rock wool using blast furnace slag according to the present invention, and is prepared by using blast furnace slag as a main raw material, adding other raw materials, and melting in an electric furnace to form a rock wool melt; in a specific embodiment, the above-mentioned rock wool melt is discharged from a four-roll centrifuge at a temperature ≥1500°C, and rock wool fibers are obtained under the combined action of blowing air, four-roll high-speed rotation, etc., and then after the process of cotton collection, pendulum cotton stacking, high-temperature curing, cutting, etc., the rock wool with performance meeting the national standard is obtained; the acidity coefficient of the rock wool is between 1.8 and 2.0, the average fiber diameter is ≤6μm, the slag ball content is ≤7%, and the thermal conductivity is ≤0.040W / mK.
[0050] The present invention also provides an application of rock wool. The rock wool of the present invention is used for external wall insulation of buildings, which can replace basalt and dolomite in traditional rock wool raw materials, greatly improve the utilization value of slag, contribute to the country's circular economy, and reduce environmental damage caused by the exploitation of natural resources.
[0051] Example 1
[0052] Refer to Figure 1 As shown, this embodiment 1 provides a method for preparing rock wool using blast furnace slag, comprising the following steps:
[0053] (1) Taiyuan Iron and Steel Co., Ltd. blast furnace slag (dry slag) is used as the main raw material. The composition of the blast furnace slag is: SiO2: 35.98%, Al2O3: 11.45%, MgO: 6.31%, CaO: 43.07%, FeO: 0.23%, calculated by mass percentage. Other raw materials are silica sand, iron tailings, bauxite and serpentine as shown in Table 3 below. The proportions of various raw materials are according to the proportion A (shown in Table 4 below). Figure 1 The process shown is well proportioned and mixed evenly before use;
[0054] (2) Using an electric furnace melting process, the mixed raw materials are added into the electric furnace, heated to above 1500°C in the electric furnace, and after all are melted, a rock wool melt with an acidity of ≥1.8 is obtained, and then enters the subsequent rock wool preparation process. After testing, the acidity coefficient of the rock wool melt is specifically 1.91;
[0055] (3) Preparation of rock wool: The high-temperature rock wool melt passes through a four-roll centrifuge, a cotton collector, a pendulum, and finally becomes cotton fiber for pressing rock wool. After adding an adhesive to the cotton fiber, it goes through a process of pendulum cotton spreading, high-temperature drying, and cutting to obtain a finished rock wool product that meets the national standard requirements for external wall insulation rock wool. The relationship between the viscosity of rock wool and temperature is as follows: Figure 2 As shown;
[0056] The performance of the above-mentioned rock wool product prepared with blast furnace slag as the main raw material meets the requirements of the national standard GB / T 25975-2018 rock wool products for external insulation of building exterior walls; the acidity coefficient of the rock wool is 1.91, the average fiber diameter is 4.75μm, the slag ball content is 5.7%, and the thermal conductivity is 0.035W / mK.
[0057] Example 2
[0058] Refer to Figure 1 As shown, this embodiment 2 provides a method for preparing rock wool using blast furnace slag, comprising the following steps:
[0059] (1) The main raw material is blast furnace slag of Hubei Iron and Steel Co., Ltd., whose chemical composition is: SiO2: 32.31%, Al2O3: 16.14%, MgO: 7.88%, CaO: 38.2%, FeO: 0.15%, and other raw material components are silica sand, iron tailings, bauxite and serpentine as shown in Table 3 below; according to the formula B in Table 4 below, the proportions of blast furnace slag, silica sand, iron tailings, bauxite and serpentine are 55%, 13%, 14%, 8% and 10% respectively. Figure 1 The process shown is well proportioned and mixed evenly before use;
[0060] (2) Using an electric furnace melting process, the mixed raw materials are added into the electric furnace, heated to above 1500°C in the electric furnace, and after all are melted, a rock wool melt with an acidity of ≥1.8 is obtained, and then enters the subsequent rock wool preparation process. After testing, the acidity coefficient of the rock wool melt is specifically 1.95;
[0061] (3) Preparation of rock wool: The high-temperature rock wool melt passes through a four-roll centrifuge, a cotton collector, a pendulum, and finally becomes cotton fiber for pressing rock wool. After adding an adhesive to the cotton fiber, it goes through a process of pendulum cotton spreading, high-temperature drying, and cutting to obtain a finished rock wool product that meets the national standard requirements for external wall insulation rock wool.
[0062] The performance of the rock wool product prepared above meets the requirements of the national standard GB / T 25975-2018 rock wool products for external insulation of building exterior walls; the acidity coefficient of the rock wool is 1.95, the average fiber diameter is 5.1 μm, the slag ball content is 5.2%, and the thermal conductivity is 0.036 W / mK.
[0063] Table 3 Main components of other raw materials
[0064]
[0065] Table 4 Raw material ratio (%)
[0066] Element Blast furnace slag Silica sand Iron tailings Bauxite Serpentine Recipe A 58 15 12 5 10 Recipe B 55 13 14 8 10
[0067] Those skilled in the art should recognize that the above embodiments are only used to illustrate the present invention, and are not intended to limit the present invention. As long as they are within the spirit of the present invention, any changes or modifications to the above embodiments will fall within the scope of the claims of the present invention.
Claims
1. A method for preparing rock wool using blast furnace slag, characterized in that: The following steps are involved: S1, uniformly mixing blast furnace slag, silica sand, iron tailings, bauxite and serpentine to prepare a mixture; S2, putting the mixed material into an electric furnace, heating and melting the mixed material in the electric furnace to obtain rock wool.
2. The method for preparing rock wool using blast furnace slag according to claim 1, characterized in that: The blast furnace slag is the main raw material, accounting for 50-60% of the total raw materials in the proportion; The silica sand, the iron tailings, the bauxite and the serpentine are respectively measured and distributed, and in the proportion, they account for 10-16%, 10-18%, 7-12% and 5-10% of the mass percentage of the total raw materials respectively.
3. The method for preparing rock wool using blast furnace slag according to claim 2, characterized in that: After the blast furnace slag, the silica sand, the iron tailings, the bauxite, and the serpentine are accurately measured, they are unloaded layer by layer on a belt conveyor and transported to a loading bin to become the mixed material.
4. The method for preparing rock wool using blast furnace slag according to claim 5, characterized in that: The mixed material is evenly added into the electric furnace according to the hourly production requirement, 40% is added into the central feeding point of the electric furnace, and 10% is added into the other 6 feeding points respectively.
5. The method for preparing rock wool using blast furnace slag according to claim 1, characterized in that: The heating temperature of the electric furnace is ≥1500°C.
6. The method for preparing rock wool using blast furnace slag according to claim 1, characterized in that: The rock wool comprises the following components by mass percentage: SiO2: 43-48%; Al2O3: 12-15%; MgO: 6-9%; CaO: 18-24%; FeO: 3-5%; Fe2O3: 3-5%; Na2O+K2O≤4%.
7. The method for preparing rock wool using blast furnace slag according to claim 6, characterized in that: The acidity coefficient of the rock wool is ≥1.
8.
8. The method for preparing rock wool using blast furnace slag according to claim 6, characterized in that: The melting temperature of the rock wool is ≤1500°C, and the viscosity at 1400-1480°C is 1.0-3.0 Pa.S.
9. A rock wool, characterized in that: The rock wool is prepared by the method for preparing rock wool using blast furnace slag as claimed in any one of claims 1 to 8.
10. An application of rock wool, characterized in that: The rock wool as claimed in claim 9 is used for external thermal insulation of the exterior walls of buildings.
Citation Information
Patent Citations
Preparation technology for melt for production of mineral wool, rock wool and cast stone products
CN103588393A
Mineral wool melt, mineral wool and preparation method
CN115849722A
Quenching and tempering method for preparing rock wool from thermal-state blast furnace slag and rock wool
CN117602841A
Glass raw material vertical composite crushing system
CN209188967U
Rock wool
JP1997202645A