A special admixture for gypsum board and its preparation process

By combining modifiers and additives, the mechanical properties and high temperature and humidity resistance of gypsum board are improved, solving the problems of insufficient mechanical properties and processing performance of gypsum board, and extending its service life.

CN118724499BActive Publication Date: 2024-11-26ZHEJIANG WULONG CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411231030.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-26
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

Existing gypsum boards have insufficient mechanical properties and resistance to high temperature and humidity, and high water content affects processing performance and molding time.

Method used

A special admixture for gypsum board is prepared by using a combination of modifiers and additives, including sodium gluconate, potassium tartrate, nitric acid triacetic acid, modified short-cut composite fibers, water-reducing agent, silica fume, polyvinyl alcohol, and sodium carboxymethyl cellulose, to improve the strength of gypsum and the dispersibility of fibers through modification treatment.

Benefits of technology

It significantly improves the mechanical properties and high temperature and humidity resistance of gypsum board, while ensuring the processing performance of gypsum and extending its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention provides a special admixture for gypsum board and a preparation process thereof, and relates to the technical field of gypsum board preparation. The special admixture for gypsum board is mainly divided into a modifier and an auxiliary agent, wherein the modifier is composed of sodium gluconate, potassium tartrate, and nitrilotriacetic acid; the auxiliary agent is composed of modified short-cut composite fiber, water reducer, silica fume, polyvinyl alcohol, and sodium carboxymethyl cellulose, and the modified short-cut composite fiber is obtained by modifying and compounding short-cut carbon fibers and plant fibers of different lengths. The present invention overcomes the shortcomings of the prior art, and effectively improves the mechanical properties of gypsum after the addition of modifiers and auxiliary agents to modify the gypsum itself, and further improves the high temperature and high humidity resistance of the gypsum board, ensuring the processing performance of the gypsum while extending its service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of gypsum board preparation, and in particular to a special admixture for gypsum board and a preparation process thereof. Background Art

[0002] Gypsum board has the advantages of light weight, fire resistance, heat insulation, adjustable indoor humidity, and quick construction, and has been widely used in partition walls and ceilings in industrial and civil buildings. Existing gypsum boards are mostly prepared by mixing gypsum raw materials with admixtures and water. The admixtures added are different according to the requirements of the gypsum board.

[0003] Natural gypsum itself is very brittle. When used as a building material, it needs to use admixtures to improve its mechanical properties. In the existing technology, other auxiliary materials or additives are mostly added to improve the mechanical properties of gypsum. At the same time, in order to ensure the processing performance of gypsum, it is generally necessary to add 60%-80% of water to ensure fluidity. However, high water content will prolong the molding time of gypsum. Therefore, at this stage, water reducers are mostly used to reduce the moisture content of gypsum processing. On this basis, the development and improvement of gypsum admixtures to comprehensively improve the mechanical properties of gypsum and ensure the processability of gypsum is a major focus of research. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention provides a special admixture for gypsum board and a preparation process thereof, which effectively modifies the gypsum itself by adding a modifier and an auxiliary agent, thereby comprehensively improving the mechanical properties of the gypsum, and further improving the high temperature and high humidity resistance of the gypsum board, thereby ensuring the processing performance of the gypsum while extending its service life.

[0005] To achieve the above objectives, the technical solution of the present invention is implemented through the following technical solutions:

[0006] A special admixture for gypsum board, the admixture comprises a modifier and an auxiliary agent, the modifier is composed of the following materials in parts by weight: 10-14 parts of sodium gluconate, 2-6 parts of potassium tartrate, and 10-15 parts of nitrilotriacetic acid; the auxiliary agent is composed of the following materials in parts by weight: 2-6 parts of modified short-cut composite fibers, 0.4-0.6 parts of water reducer, 10-12 parts of silica fume, 0.1-0.4 parts of polyvinyl alcohol, and 1-3 parts of sodium carboxymethyl cellulose; wherein the modified short-cut composite fibers are prepared by mixing carbon fibers with lengths of 3 mm and 8 mm in a ratio of 2:3, then oxidizing, and then mixing the carbon fibers and short-cut 12 mm plant fibers in a mass ratio of 5:2, acid washing, and high-pressure modification.

[0007] Preferably, the method for preparing the modified chopped composite fiber comprises the following steps:

[0008] S1. Prepare materials according to the following mass ratio: chopped 3mm carbon fiber: chopped 8mm carbon fiber: chopped 12mm plant fiber = 2:3:2;

[0009] S2, taking short chopped carbon fibers of 3 mm and 8 mm and mixing them to obtain mixed short chopped carbon fibers for later use;

[0010] S3, soaking the mixed short carbon fibers in a hydrogen peroxide aqueous solution for oxidation treatment, then taking them out for rinsing with clean water and drying them to obtain the oxidized carbon fibers for later use;

[0011] S4, mixing the oxidized carbon fiber with the chopped 12 mm plant fiber, and then soaking it in a hydrochloric acid solution with a pH of 4-4.5 for 20-40 minutes, and then taking it out and rinsing it with clean water to obtain the acid-washed composite fiber for use;

[0012] S5. Treat the acid-washed composite fiber with 110-120° C. hot steam at a pressure of 1.2-1.4 MPa for 1-3 min to obtain modified short-cut composite fiber.

[0013] Preferably, the concentration of hydrogen peroxide in the aqueous hydrogen peroxide solution used in step S3 is 4%-6%, and the material-liquid ratio for soaking is 1:80-100, and the soaking time is 20-30 minutes.

[0014] Preferably, the drying method in step S3 is to treat in an oven at 120° C. for 1-2 hours.

[0015] Preferably, the water reducer is a polycarboxylate water reducer.

[0016] The preparation method of the special admixture for gypsum board comprises the following steps:

[0017] (1) Preparation of the modifier: Mix sodium gluconate, potassium tartrate and nitrilotriacetic acid evenly to obtain the modifier;

[0018] (2) Preparation of auxiliary agent: Add the modified short-cut composite fiber into clean water to disperse it, then add silica fume, polyvinyl alcohol and sodium carboxymethyl cellulose, stir well and dry, and then mix with water reducer to obtain auxiliary agent.

[0019] Preferably, the rotation speed for fully stirring in step (2) is 800-1200 r / min, the stirring time is 20-40 min, and the drying temperature is 50-60° C., and the moisture content after drying is controlled to be ≤10%.

[0020] The method of using special admixtures for gypsum board includes the following steps:

[0021] (1) Mix the modifier and gypsum raw material in a mass ratio of 0.1-0.3:100, then add clean water and stir thoroughly to obtain a mixed slurry for use;

[0022] (2) The mixed slurry is pressurized to 0.6-1.2 MPa and treated at 100-105°C for 30-60 min, then filtered, dried and ground to obtain modified gypsum for later use;

[0023] (3) The modified gypsum material, auxiliary agent and water are mixed and stirred in a mass ratio of 40-45:4-8:50-55 to prepare a gypsum board.

[0024] Preferably, the solid content of the mixed slurry in step (1) is controlled at 30%-40%.

[0025] Preferably, the mixing and stirring in step (3) is carried out by stirring at a speed of 120-200 r / min for 60-80 min.

[0026] The present invention provides a special admixture for gypsum board, which has the following advantages compared with the prior art:

[0027] The admixture of the present invention is divided into a modifier and an auxiliary agent, wherein the modifier is prepared by mixing sodium gluconate, potassium tartrate and nitrilotriacetic acid, and the gypsum raw material is mixed and high-temperature modified, so as to effectively improve the strength of the gypsum, further enhance the high temperature resistance and aging resistance of the subsequent gypsum board, and at the same time effectively enhance the mechanical properties of the subsequent gypsum board by compounding modified short-cut composite fibers, water reducers, silica fume, polyvinyl alcohol and sodium carboxymethyl cellulose, wherein modified carbon fibers and plant fibers with different short-cut lengths are adopted to ensure the dispersion of the fibers and enhance the compressive strength at the same time, so as to comprehensively enhance the use effect of the gypsum board. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] The carbon fibers used below have a carbon content of ≥95%, a fiber diameter of 7 μm, a tensile modulus of 220 GPa, a tensile strength of 3800 Mpa, and short chopped lengths of 3 mm and 8 mm respectively;

[0030] The plant fiber is ramie fiber, and the short cut length is 12 mm;

[0031] The water reducer is CQJ-JSS02 polycarboxylate water reducer (Shanghai Chenqi Chemical Technology Co., Ltd.);

[0032] Silica ash is BK-96 raw ash with a bulk density of 200kg / m 3 , pH value is 6, silicon dioxide content> 96%;

[0033] The gypsum raw material is natural building gypsum, and its main chemical composition content is shown in Table 1 below:

[0034] Table 1

[0035]

[0036] The mechanical properties of the gypsum processing are shown in Table 2 below:

[0037] Table 2

[0038]

[0039] Example 1 Raw material preparation:

[0040] 1. Preparation of modified chopped composite fiber A:

[0041] (1) Prepare the materials according to the following mass ratio: chopped 3mm carbon fiber: chopped 8mm carbon fiber: chopped 12mm plant fiber = 2:3:2;

[0042] (2) Mix chopped 3 mm and 8 mm carbon fibers to obtain mixed chopped carbon fibers for later use;

[0043] (3) The mixed chopped carbon fibers were immersed in a 5% aqueous hydrogen peroxide solution at a material-liquid ratio of 1:90 for oxidation treatment for 25 minutes, then taken out for rinsing with clean water and baked in an oven at 120° C. for 1.5 hours to obtain the oxidized carbon fibers for use;

[0044] (4) The oxidized carbon fiber is mixed with the short-cut 12 mm plant fiber, and then immersed in a hydrochloric acid solution with a pH of 4 for 30 min, and then taken out and rinsed with clean water to obtain the acid-washed composite fiber for use;

[0045] (5) The acid-washed composite fiber was treated with 110° C. hot steam at a pressure of 1.4 MPa for 2 min to obtain modified short-cut composite fiber A.

[0046] 2. Preparation of modified chopped composite fiber B:

[0047] (1) Prepare the materials according to the following mass ratio: chopped 3mm carbon fiber: chopped 3mm plant fiber = 5:2;

[0048] (2) The chopped carbon fibers were immersed in a 5% aqueous hydrogen peroxide solution at a material-liquid ratio of 1:90 for oxidation treatment for 25 min, then taken out for rinsing with clean water and baked in an oven at 120° C. for 1.5 h to obtain the oxidized carbon fibers for use;

[0049] (3) Mixing the oxidized carbon fiber with the chopped 3 mm plant fiber, and then immersing it in a hydrochloric acid solution with a pH of 4 for 30 min, and then taking it out and rinsing it with clean water to obtain the acid-washed composite fiber for use;

[0050] (4) The acid-washed composite fiber was treated with 110° C. hot steam at a pressure of 1.4 MPa for 2 min to obtain modified short-cut composite fiber B.

[0051] 3. Preparation of modified chopped composite fiber C:

[0052] (1) Prepare the materials according to the following mass ratio: chopped 8mm carbon fiber: chopped 8mm plant fiber = 5:2;

[0053] (2) The chopped carbon fibers were immersed in a 5% aqueous hydrogen peroxide solution at a material-liquid ratio of 1:90 for oxidation treatment for 25 min, then taken out for rinsing with clean water and baked in an oven at 120° C. for 1.5 h to obtain the oxidized carbon fibers for use;

[0054] (3) The oxidized carbon fiber is mixed with the short-cut 8 mm plant fiber, and then immersed in a hydrochloric acid solution with a pH of 4 for 30 minutes, and then taken out and rinsed with clean water to obtain the acid-washed composite fiber for use;

[0055] (4) The acid-washed composite fiber was treated with 110° C. hot steam at a pressure of 1.4 MPa for 2 min to obtain modified short-cut composite fiber C.

[0056] 4. Preparation of modified chopped composite fiber D:

[0057] (1) Prepare the materials according to the following mass ratio: chopped 12mm carbon fiber: chopped 12mm plant fiber = 5:2;

[0058] (2) The chopped carbon fibers were immersed in a 5% aqueous hydrogen peroxide solution at a material-liquid ratio of 1:90 for oxidation treatment for 25 min, then taken out for rinsing with clean water and baked in an oven at 120° C. for 1.5 h to obtain the oxidized carbon fibers for use;

[0059] (3) The oxidized carbon fiber is mixed with short-cut 12 mm plant fiber, and then immersed in a hydrochloric acid solution with a pH of 4 for 30 min, and then washed with clean water to obtain an acid-washed composite fiber for use;

[0060] (4) The acid-washed composite fiber was treated with 110°C hot steam at a pressure of 1.4 MPa for 2 min to obtain modified short-cut composite fiber D.

[0061] 5. Composite fiber material:

[0062] The materials are prepared according to the following mass ratio: chopped 3mm carbon fiber: chopped 8mm carbon fiber: chopped 12mm plant fiber = 2:3:2, and the fibers are evenly mixed to obtain a composite fiber material.

[0063] 6. Preparation of modifier:

[0064] The raw materials were mixed according to the following weight parts to obtain a modifier: 12 parts of sodium gluconate, 4 parts of potassium tartrate, and 13 parts of nitrilotriacetic acid.

[0065] 7. Preparation of auxiliary agents:

[0066] (1) Prepare the following materials by weight: 4 parts of fiber material, 0.5 parts of water reducing agent, 11 parts of silica fume, 0.3 parts of polyvinyl alcohol, and 2 parts of sodium carboxymethyl cellulose;

[0067] (2) Disperse the fiber material in 10 times the volume of clean water, then add silica fume, polyvinyl alcohol and sodium carboxymethyl cellulose, stir at a speed of 1000 r / min for 30 minutes, then dry at 60°C to a moisture content of ≤10%, and then mix with a water reducer to obtain an auxiliary agent.

[0068] According to the preparation method of the auxiliary agent, different fiber materials are selected for preparation according to the following Table 3:

[0069] Table 3

[0070]

[0071] Embodiment 2 Modification treatment of gypsum:

[0072] (1) Mix the modifier and gypsum raw material in a mass ratio of 0.2:100, then add clean water to adjust the solid content to 30%, stir well, and obtain a mixed slurry for use;

[0073] (2) The mixed slurry is pressurized to 1 MPa and treated at 100°C for 40 minutes, then filtered, dried and ground to obtain modified gypsum.

[0074] The setting time of the modified gypsum material was tested, and gypsum test blocks were prepared according to GB / T 17669.3 "Determination of Mechanical Properties of Building Gypsum". The test block size was 40 mm × 40 mm × 160 mm. The flexural and compressive strengths were tested under 2h and absolute dry conditions. The specific results are shown in Table 4 below:

[0075] Table 4

[0076]

[0077] Example 3 Preparation of gypsum board:

[0078] The modified gypsum prepared in Example 2 is used as a raw material, and the modified gypsum, auxiliary agent and water are mixed in a mass ratio of 42:6:53, and stirred at a speed of 1180 r / min for 70 min to obtain a mixed slurry;

[0079] The mixed slurry is made into a paper-faced gypsum board with a specification of 2440 mm×1220 mm×12.0 mm, and the auxiliary agents selected in the preparation of the specific straight-faced gypsum board are shown in Table 5 below

[0080] Table 5

[0081]

[0082] Samples were cut from each group at a distance of >100 mm from the edge of the gypsum board. The sample specifications for the breaking load test were 400 mm × 300 mm (divided into horizontal and vertical directions), and the sample specifications for the shear force test were 150 mm × 150 mm. The transverse breaking load, longitudinal breaking load and shear force of each group of gypsum boards were directly tested according to the method specified in GB / T 9775-2008 "Paper-faced gypsum board". The specific results are shown in Table 6 below:

[0083] Table 6

[0084]

[0085] The above groups of gypsum boards were dried in a 45°C oven to constant weight, and then placed in a constant temperature and humidity chamber at 40°C and 90% relative humidity for 30 days. The transverse breaking load, longitudinal breaking load and shear force are shown in Table 7 below:

[0086] Table 7

[0087]

[0088] From the above tests, it can be seen that the gypsum board prepared in Experimental Group 1 has higher mechanical properties and also has better resistance to high temperature and high humidity.

[0089] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A special admixture for gypsum board, characterized in that: The admixture includes a modifier and an auxiliary agent, wherein the modifier is composed of the following materials in parts by weight: 10-14 parts of sodium gluconate, 2-6 parts of potassium tartrate, and 10-15 parts of nitrilotriacetic acid; the auxiliary agent is composed of the following materials in parts by weight: 2-6 parts of modified short-cut composite fiber, 0.4-0.6 parts of water reducer, 10-12 parts of silica fume, 0.1-0.4 parts of polyvinyl alcohol, and 1-3 parts of sodium carboxymethyl cellulose; The modified short-cut composite fiber is prepared by mixing carbon fibers with lengths of 3 mm and 8 mm in a ratio of 2:3, followed by oxidation treatment, and then acid washing and high-pressure modification of the carbon fibers and short-cut 12 mm plant fibers in a mass ratio of 5:

2. The preparation method of the modified short-cut composite fiber comprises the following steps: S1. Prepare the materials according to the following mass ratio: chopped 3mm carbon fiber: chopped 8mm carbon fiber: chopped 12mm plant fiber = 2:3:2; S2, taking short-cut 3mm and 8mm carbon fibers and mixing them to obtain mixed short-cut carbon fibers for later use; S3, soaking the mixed chopped carbon fibers in a hydrogen peroxide aqueous solution for oxidation treatment, then taking them out, rinsing them with clean water, and drying them to obtain the oxidized carbon fibers for later use; S4, mixing the oxidized carbon fibers with chopped 12 mm plant fibers, and then immersing the mixed fibers in a hydrochloric acid solution with a pH of 4-4.5 for 20-40 minutes, and then rinsing with clean water to obtain an acid-washed composite fiber for later use; S5. Treat the acid-washed composite fiber with 110-120° C. hot steam at a pressure of 1.2-1.4 MPa for 1-3 min to obtain modified chopped composite fiber.

2. The special admixture for gypsum board according to claim 1, characterized in that: The concentration of hydrogen peroxide in the aqueous hydrogen peroxide solution used in step S3 is 4%-6%, the material-liquid ratio for soaking is 1:80-100, and the soaking time is 20-30 minutes.

3. The special admixture for gypsum board according to claim 1, characterized in that: The drying method in step S3 is to carry out drying in an oven at 120° C. for 1-2 hours.

4. The special admixture for gypsum board according to claim 1, characterized in that: The water reducer is a polycarboxylate water reducer.

5. A method for preparing the special admixture for gypsum board according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: (1) Preparation of modifier: Sodium gluconate, potassium tartrate and nitrilotriacetic acid are mixed evenly to obtain the modifier; (2) Preparation of auxiliary agent: Add the modified short-cut composite fiber into clean water and disperse it, then add silica fume, polyvinyl alcohol and sodium carboxymethyl cellulose, stir thoroughly and dry, and then mix with water reducer to obtain auxiliary agent.

6. The preparation method according to claim 5, characterized in that: The rotation speed for fully stirring in step (2) is 800-1200 r / min, the stirring time is 20-40 min, and the drying temperature is 50-60° C., and the moisture content after drying is controlled to be ≤10%.

7. A method for using the special admixture for gypsum board according to any one of claims 1 to 4, characterized in that: The method of use comprises the following steps: (1) Mix the modifier and gypsum raw materials in a mass ratio of 0.1-0.3:100, then add clean water and stir thoroughly to obtain a mixed slurry for use; (2) The mixed slurry is pressurized to 0.6-1.2 MPa and treated at 100-105°C for 30-60 min, then filtered, dried and ground to obtain the modified gypsum material for later use; (3) The modified gypsum material, auxiliary agent and water are mixed and stirred in a mass ratio of 40-45:4-8:50-55 to prepare a gypsum board.

8. The method of use according to claim 7, characterized in that: The solid content of the mixed slurry in step (1) is controlled at 30%-40%.

9. The method of use according to claim 7, characterized in that: The mixing and stirring in step (3) is carried out by stirring at a speed of 120-200 r / min for 60-80 min.