Preparation method of porous ceramic and porous ceramic

By employing a multi-step approach involving electric field treatment, silver plating, and atmosphere control, the problems of low porosity and compressive strength in porous ceramics were solved, resulting in the preparation of porous ceramics with high porosity and high compressive strength.

CN118724571BActive Publication Date: 2024-11-29成都达奇科技股份有限公司

Patent Information

Application Number
CN202411214942.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-29
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

Existing porous ceramics have low porosity and compressive strength, making it difficult to simultaneously meet the requirements of high porosity and high compressive strength.

Method used

A multi-step approach involving electric field treatment, silver plating, anionic surfactant treatment, and atmosphere control, including argon and oxygen treatment, alkaline immersion, silver plating, and sintering under different atmospheres, is employed to improve the surface cleanliness, porosity, and compressive strength of porous ceramics.

Benefits of technology

It significantly improves the porosity and compressive strength of porous ceramics, forming a dense, high-strength three-dimensional network structure, which is suitable for the efficient preparation of porous ceramics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724571B_ABST
    Figure CN118724571B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of porous ceramics and porous ceramics, and belongs to the technical field of porous ceramics. The preparation method comprises the following steps: step 100, placing an organic porous matrix into a cavity to which an electric field is applied, and treating it in argon atmosphere and oxygen atmosphere in turn to obtain a first modified matrix; step 200, soaking the first modified matrix in alkali solution to obtain a second modified matrix; step 300, plating a silver layer on the pore surface of the second modified matrix to obtain a third modified matrix; step 400, soaking the third modified matrix in an anionic surfactant solution to obtain a fourth modified matrix; step 500, attaching a slurry containing ceramic powder to the pore surface of the fourth modified matrix to obtain a pre-fired body; step 600, sintering the pre-fired body in air atmosphere and nitrogen atmosphere in turn to obtain porous ceramics. The process of the invention is simple, easy to operate and control, and the obtained porous ceramics have both high porosity and high compressive strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of porous ceramics, and in particular to a preparation method of porous ceramics and porous ceramics. Background Art

[0002] Porous ceramics can have the characteristics of both porous materials and ceramic materials. As a porous material, it has uniformly distributed voids, high porosity and high specific surface area. As a ceramic material, it can be used in wear resistance, high temperature resistance and corrosion resistance. Due to the various excellent physical properties of porous ceramics, it has important applications in many fields, such as filter materials, thermal insulation materials, sound absorption materials and biomedicine.

[0003] There are many methods for preparing porous materials at present, and the porous materials prepared by different methods have great differences in structure and performance. Common preparation methods include gel casting, foaming, and sacrificial template method.

[0004] The gel casting method uses the sol gelation process to form a three-dimensional network structure by stacking and cross-linking colloidal particles, so that the ceramic powder is solidified in situ to obtain a green body, and then the colloid is removed by demoulding drying and debinding sintering to achieve the purpose of pore formation. This method has a simple process, is easy to operate and apply on a large scale, but the organic monomers introduced in the process are prone to produce polluting gases, which have an impact on the environment.

[0005] The foaming method introduces bubbles into the slurry by mechanical stirring or adding a foaming agent, and then sintering the formed slurry after drying. The space left by the bubbles will form fine gaps to achieve the purpose of pore formation. This method is simple and easy to control the size and shape of the pores, but the stability of the foam slurry is easily affected by the system components, and the pore size is small.

[0006] The sacrificial template method is to squeeze and absorb the template material, such as polyurethane foam, into the ceramic powder slurry. During the molding process, the template material will occupy a certain space in the green body. During the calcination process, the template material will sinter or evaporate, leaving pores inside the material. This preparation method has low cost and simple process, but it is easy to cause uneven slurry, and the slurry is easy to fall off during the sintering process, which in turn affects the porosity and compressive strength of the ceramic material. Summary of the invention

[0007] The main purpose of the present invention is to provide a method for preparing porous ceramics and porous ceramics, so as to solve the technical problems of low porosity and compressive strength of porous ceramics in the prior art.

[0008] In order to achieve the above object, the present invention first provides a method for preparing porous ceramics, and the technical scheme is as follows:

[0009] The method for preparing porous ceramics comprises the following steps:

[0010] Step 100, placing an organic porous substrate into a cavity to which an electric field is applied, and treating the surface of the organic porous substrate in an argon atmosphere and an oxygen atmosphere in sequence to obtain a first modified substrate;

[0011] Step 200, soaking the first modified substrate in an alkaline solution, washing and drying after soaking, to obtain a second modified substrate;

[0012] Step 300, plating a silver layer on the pore surface of the second modified substrate to obtain a third modified substrate;

[0013] Step 400, soaking the third modified substrate in an anionic surfactant solution, washing and drying after soaking, to obtain a fourth modified substrate;

[0014] Step 500, attaching a slurry containing ceramic powder to the pore surface of the fourth modified substrate, and drying to obtain a pre-fired green body;

[0015] Step 600, placing the pre-fired green body into a sintering furnace, and sintering the pre-fired green body in an air atmosphere and a nitrogen atmosphere in turn to obtain a porous ceramic.

[0016] As a further improvement of the above-mentioned method for preparing porous ceramics: the organic porous matrix is ​​a polyurethane sponge with a ppi of 30 to 70.

[0017] As a further improvement of the above-mentioned method for preparing porous ceramics: in step 100, based on the cavity volume of 1L, the volume of the organic porous matrix is ​​0.05 to 0.2 times the cavity volume, the pressure in the cavity is 100 to 500 mTorr, the power is 50 to 300 W, and it is first treated in an argon atmosphere of 10 to 50 sccm for 6 to 10 minutes, and then treated in an oxygen atmosphere of 5 to 30 sccm for 6 to 10 minutes.

[0018] As a further improvement of the above-mentioned method for preparing porous ceramics: in step 200, the alkali solution is a NaOH solution with a mass fraction of 20-30%, the soaking time is 2-6 hours, and the soaking temperature is room temperature.

[0019] As a further improvement of the above-mentioned method for preparing porous ceramics: in step 300, plating a silver layer on the pore surface of the second modified substrate includes the following steps:

[0020] soaking the second modified substrate in a silver nitrate solution for sensitization;

[0021] After sensitization is completed, the plating solution is transferred into the plating solution, which includes silver nitrate, ammonia water and sodium hydroxide;

[0022] Glucose solution is added to the plating solution, and after the reaction is completed, washing and drying are performed to obtain the third modified matrix.

[0023] As a further improvement of the above-mentioned method for preparing porous ceramics: in step 400, the anionic surfactant solution is an SDS solution with a mass fraction of 2-4%, the soaking time is 1-3 hours, and the soaking temperature is 70-80°C.

[0024] As a further improvement of the above-mentioned method for preparing porous ceramics: in step 500, the preparation of the slurry comprises the steps of: firstly, wet-grinding and mixing the ceramic powder and the sodium carboxymethyl cellulose solution, and then adding the polyvinyl alcohol solution and wet-grinding and mixing, so as to obtain the slurry;

[0025] The solid content of the slurry is 40-50%, the ceramic powder includes diatomaceous earth, alumina, magnesium oxide and kaolin in a mass ratio of (8-10):(4-6):(2-4):(2-4), the mass fraction of sodium carboxymethyl cellulose solution is 0.3-0.5%, and the mass fraction of polyvinyl alcohol solution is 2-4%.

[0026] As a further improvement of the above-mentioned method for preparing porous ceramics: in step 500, the drying is firstly standing and drying at room temperature for 24 to 48 hours, and then drying at 50 to 70°C for 12 to 24 hours.

[0027] As a further improvement of the above-mentioned method for preparing porous ceramics: in step 600, the sintering process includes the following stages:

[0028] Raise the temperature from room temperature to 400-500°C in an air atmosphere and keep it warm for 1-2 hours;

[0029] Switch the atmosphere to nitrogen atmosphere, continue to raise the temperature to 600-650°C, and keep it for 1-2 hours;

[0030] Maintaining nitrogen atmosphere, continue to raise the temperature to 750-800°C and keep it for 1-2 hours;

[0031] Maintaining nitrogen atmosphere, continue to raise the temperature to 900-950°C and keep it for 1-2 hours;

[0032] Maintaining the nitrogen atmosphere, continue to raise the temperature to 1050-1200°C, keep it at that temperature for 2-4 hours, and then cool the furnace to obtain porous ceramics.

[0033] In order to achieve the above object, the present invention secondly provides a porous ceramic, and the technical solution is as follows:

[0034] The porous ceramic is prepared by the above-mentioned method for preparing the porous ceramic.

[0035] The preparation method of the porous ceramic and the porous ceramic of the present invention have the following advantages:

[0036] First, high-energy argon ions formed by ionization of argon gas under the action of an electric field physically collide and bombard the pore surface of the organic porous matrix, thereby significantly increasing the specific surface area of ​​the organic porous matrix, which in turn helps to increase the adhesion surface of the ceramic slurry and the porosity and specific surface area of ​​the porous ceramic.

[0037] Second, oxygen is ionized under the action of the electric field to form high-energy oxygen atoms (O) and active oxygen (O3, O2 + ), these high-energy particles can not only destroy the chemical bonds of organic matter on the pore surface of the organic porous matrix, effectively remove organic pollutants, grease, oxide layers, etc., thereby efficiently cleaning the surface, but also introduce oxygen groups on the pore surface of the organic porous matrix to improve surface activity, increase the hydrophilicity and chemical reactivity of the surface, and ultimately achieve the effects of surface cleaning, activation and oxidation, which is conducive to the adhesion of ceramic slurry. Using oxygen treatment after argon treatment can remove impurities exposed after high-energy argon ions collide and bombard the pore surface of the organic porous matrix, and achieve deep removal of impurities.

[0038] Third, before attaching the ceramic slurry, a layer of silver is first plated on the pore surface of the organic porous matrix, which has the following effects: (1) Silver has unique properties such as excellent conductivity, antibacterial properties, and reflectivity, which is very useful in subsequent electronic components, antibacterial coatings, sensors, optical applications, electromagnetic shielding, fuel cells, etc. (2) The silver layer provides a metal base, which can increase the adhesion of the ceramic slurry to the polyurethane sponge, thereby promoting the uniform distribution of the ceramic slurry and reducing the formation of pores and defects. (3) At a certain sintering temperature, the silver layer will partially melt and diffuse in the ceramic slurry, which can help fill the pores and enhance the density of the ceramic structure, thereby increasing the compressive strength.

[0039] Fourth, after the silver layer is plated, it is further immersed in an anionic surfactant solution to form an adsorption layer on the surface of the silver layer through electrostatic adsorption or hydrophobic interaction, which has the following effects: (1) Increasing surface wettability: Anionic surfactants can increase the hydrophilicity of the silver layer surface and enhance the wettability of the silver layer in the subsequent aqueous ceramic slurry system, which is very beneficial for the uniform coating of the aqueous ceramic slurry and can reduce the formation of defects. (2) Regulating surface charge: Anionic surfactants can form a negatively charged adsorption layer on the surface of the silver layer, which helps to regulate the electrostatic repulsion between ceramic powder particles and prevent the particles from agglomerating during subsequent processing.

[0040] Fifth, the sintering process of first using a low-temperature air atmosphere and then a high-temperature nitrogen atmosphere has the following effects: (1) Switching the atmosphere in different temperature ranges can control the redox reaction and thus adjust the microstructure and chemical composition of the material. For example, a nitrogen atmosphere can inhibit the reduction of certain metal oxides, allowing the ceramic to maintain a higher oxidation state, or promote the formation of specific phases and enhance the performance of the material. (2) Treatment under different atmospheres, especially a nitrogen atmosphere, helps control the porosity and pore size distribution, thereby achieving precise control of the pore structure of porous ceramics. (3) Using a nitrogen atmosphere at a high temperature stage can reduce the loss of certain volatile oxides, maintain the chemical stability of porous ceramics, and avoid component segregation or inhomogeneity. (4) A nitrogen atmosphere can introduce nitrogen elements to form a nitride layer on the pore surface of porous ceramics, thereby enhancing the wear resistance and corrosion resistance of porous ceramics.

[0041] In summary, the preparation method of the porous ceramic and the process of the porous ceramic of the present invention are simple, easy to operate and control. It has been verified that the obtained porous ceramic has both high porosity and high compressive strength and has excellent application prospects.

[0042] The following is a further description of the embodiments of the invention provided in this specification in conjunction with the accompanying drawings and specific implementation methods. Additional aspects and advantages of the embodiments of the invention provided in this specification will be partially given in the following description, and partially will become apparent from the following description, or will be understood through the practice of the embodiments of the invention provided in this specification. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] The drawings that constitute part of the embodiments of the inventions provided in this specification are used to assist in understanding the embodiments of the inventions provided in this specification. The contents provided in the drawings and the related descriptions in the embodiments of the inventions provided in this specification can be used to explain the embodiments of the inventions provided in this specification, but do not constitute improper limitations on the embodiments of the inventions provided in this specification. In the drawings:

[0044] Figure 1 This is an appearance diagram of a porous ceramic according to an embodiment of the present invention. DETAILED DESCRIPTION

[0045] The following is a clear and complete description of the embodiments of the inventions provided in this specification in conjunction with the accompanying drawings. A person of ordinary skill in the art will be able to implement the embodiments of the inventions provided in this specification based on these descriptions. Before describing the embodiments of the inventions provided in this specification in conjunction with the accompanying drawings, it should be particularly noted that:

[0046] The technical solutions and technical features provided in each part of the embodiments of the invention provided in this specification, including the following description, may be combined with each other if there is no conflict.

[0047] In addition, the embodiments of the embodiments of the inventions provided in this specification involved in the following description are generally only a partial embodiment of the embodiments of the inventions provided in this specification rather than all the embodiments. Therefore, based on the embodiments of the embodiments of the inventions provided in this specification, all other embodiments obtained by ordinary technicians in this field without making any creative work should fall within the scope of protection of the embodiments of the inventions provided in this specification.

[0048] Regarding the terms and units in the embodiments of the inventions provided in this specification: The terms "including", "comprising", "having" and any variations thereof in the descriptions and claims of the embodiments of the inventions provided in this specification and in the related parts are intended to cover non-exclusive inclusions. In addition, other relevant terms and units in the embodiments of the inventions provided in this specification can be reasonably interpreted based on the relevant contents of the embodiments of the inventions provided in this specification.

[0049] Embodiment: The method for preparing the porous ceramic of this embodiment comprises the following steps:

[0050] Step 100, placing an organic porous substrate into a cavity to which an electric field is applied, and treating the surface of the organic porous substrate in an argon atmosphere and an oxygen atmosphere in sequence to obtain a first modified substrate;

[0051] Among them, the organic porous matrix is ​​a polyurethane sponge with a 40ppi. Based on the cavity volume of 1L, the volume of the organic porous matrix is ​​0.1 times the cavity volume. The pressure in the cavity is 300 mTorr and the power is 200W. It is first treated in an argon atmosphere of 40sccm for 10 minutes and then in an oxygen atmosphere of 20sccm for 10 minutes.

[0052] Step 200, soaking the first modified substrate in a NaOH solution with a mass fraction of 25% for 4 hours at room temperature, washing and drying after soaking to obtain a second modified substrate.

[0053] Step 300, plating a silver layer on the pore surface of the second modified substrate to obtain a third modified substrate;

[0054] Plating a silver layer on the pore surface of the second modified substrate comprises the following steps:

[0055] Step 310, immersing the second modified substrate in a 5 g / L silver nitrate solution for sensitization treatment, the sensitization treatment time is 10 minutes;

[0056] Step 320, after sensitization is completed, the solution is transferred into a plating solution, wherein the plating solution includes silver nitrate, ammonia water and sodium hydroxide, the pH value is 10-11, the concentration of silver nitrate is 5 g / L, and the concentration of ammonia water is 20 mL / L;

[0057] Step 330, adding glucose solution to the plating solution, the final concentration of glucose after addition is 7.5 g / L, the reaction time is 45 minutes, and after the reaction is completed, washing and drying are performed to obtain the third modified matrix.

[0058] Step 400, immersing the third modified matrix in a 3% by mass SDS solution for 2 hours at a temperature of 75°C, and washing and drying the solution after immersion to obtain a fourth modified matrix.

[0059] Step 500, attaching a slurry containing ceramic powder to the pore surface of the fourth modified substrate, and drying to obtain a pre-fired green body;

[0060] The preparation of the slurry comprises the following steps: firstly, wet-grinding and mixing the ceramic powder and the sodium carboxymethyl cellulose solution, and then adding the polyvinyl alcohol solution and wet-grinding and mixing to obtain the slurry; wherein the solid content of the slurry is 45%, the ceramic powder comprises diatomaceous earth, alumina, magnesium oxide and kaolin in a mass ratio of 9:5:3:3, the mass fraction of the sodium carboxymethyl cellulose solution is 0.4%, and the mass fraction of the polyvinyl alcohol solution is 3%;

[0061] The drying step is to first stand and dry at room temperature for 24 hours, and then dry at 60° C. for 24 hours.

[0062] Step 600, placing the pre-fired green body into a sintering furnace, and sintering the pre-fired green body in an air atmosphere and a nitrogen atmosphere in sequence to obtain a porous ceramic;

[0063] The heating rate of the sintering process is 5°C / minute, which specifically includes the following stages:

[0064] In air atmosphere, the temperature was raised from room temperature to 400°C and kept at this temperature for 1 hour;

[0065] Switch the atmosphere to nitrogen atmosphere, continue to raise the temperature to 600°C, and keep it for 1 hour;

[0066] Maintaining nitrogen atmosphere, continue to raise the temperature to 750°C and keep it for 1 hour;

[0067] Maintaining nitrogen atmosphere, continue to raise the temperature to 900°C and keep it for 1 hour;

[0068] Maintaining the nitrogen atmosphere, the temperature was continued to rise to 1100°C and kept at that temperature for 4 hours, and porous ceramics were obtained by cooling the furnace.

[0069] Figure 1 FIG. 2 is an appearance diagram of the porous ceramic of this embodiment. Figure 1 As shown, the porous ceramic is off-white, and the surface of the material has a macroporous structure that is visible to the naked eye and evenly distributed. The pores are densely connected by sintered powders, with high permeability and no powder falling off.

[0070] Generally speaking, the higher the porosity, the lower the compressive strength. In the prior art, if the compressive strength of porous ceramics is to reach more than 10MPa, the porosity is generally not higher than 70%. However, in this embodiment, the porosity of the porous ceramics tested by the BET method is 85.3%, and the compressive strength of the porous ceramics tested by the "Test Method for Compression Properties of Rigid Foam Plastics" (GB / T5486-2008) is 15.55MPa. It can be seen that the matrix performance, slurry hanging process and sintering process of the porous ceramics are all excellent, so as to form a dense, high-strength three-dimensional network porous structure.

[0071] Comparative Example 1: Compared with the embodiment, the difference of this comparative example is that only oxygen is used for modification in step 100. After testing, the porosity of the obtained porous ceramic is 79.6%, and the compressive strength is 15.69 MPa.

[0072] Comparative Example 2: Compared with the embodiment, the difference of this comparative example is that only argon gas is used for modification treatment in step 100. After testing, the porosity of the obtained porous ceramic is 84.4% and the compressive strength is 14.82 MPa.

[0073] Comparative Example 3: Compared with the embodiment, the difference of this comparative example is that step 300 is not performed. After testing, the porosity of the obtained porous ceramic is 82.5%, and the compressive strength is 12.24 MPa.

[0074] Comparative Example 4: Compared with the embodiment, the difference of this comparative example is that step 400 is not performed. After testing, the porosity of the obtained porous ceramic is 82.6%, and the compressive strength is 12.26 MPa.

[0075] Comparative Example 5: Compared with the embodiment, the difference of this comparative example is that in step 600, the sintering process is performed in an air atmosphere. After testing, the porosity of the obtained porous ceramic is 81.5%, and the compressive strength is 13.58 MPa.

[0076] Comparative Example 6: Compared with the embodiment, the difference of this comparative example is that in step 600, the sintering process is: heating from room temperature to 400°C in air atmosphere, keeping warm for 1 hour; switching the atmosphere to nitrogen atmosphere, continuing to heat to 1100°C, keeping warm for 4 hours, and cooling with the furnace to obtain porous ceramics. After testing, the porosity of the obtained porous ceramics is 81.1% and the compressive strength is 13.76MPa.

[0077] Comparative Example 7: Compared with the embodiment, the difference of this comparative example is that steps 100, 300, and 400 are not performed, and the sintering process in step 600 is: heating from room temperature to 400°C in air atmosphere, keeping warm for 1 hour; switching the atmosphere to nitrogen atmosphere, continuing to heat to 1100°C, keeping warm for 4 hours, and cooling with the furnace to obtain porous ceramics. After testing, the porosity of the obtained porous ceramics is 74.8%, and the compressive strength is 9.48MPa.

[0078] The above is a description of the relevant contents of the embodiments of the inventions provided in this specification. Based on these descriptions, a person of ordinary skill in the art will be able to implement the embodiments of the inventions provided in this specification. Based on the above contents of the embodiments of the inventions provided in this specification, all other preferred implementations and embodiments obtained by a person of ordinary skill in the art without making any creative work shall fall within the scope of protection of the embodiments of the inventions provided in this specification.

Claims

1. A method for preparing porous ceramics, characterized in that: The following steps are involved: Step 100: placing an organic porous substrate into a cavity to which an electric field is applied, and treating the surface of the organic porous substrate in an argon atmosphere and an oxygen atmosphere in sequence to obtain a first modified substrate; Step 200, soaking the first modified substrate in an alkaline solution, washing and drying the substrate after soaking to obtain a second modified substrate; Step 300, using a plating solution including silver nitrate, ammonia water and sodium hydroxide to plate a silver layer on the pore surface of the second modified substrate to obtain a third modified substrate; Step 400, immersing the third modified substrate in an anionic surfactant solution to form an adsorption layer on the surface of the silver layer through electrostatic adsorption or hydrophobic interaction, and washing and drying the substrate after immersion to obtain a fourth modified substrate; Step 500: attaching a slurry containing ceramic powder to the pore surfaces of the fourth modified substrate and drying the slurry to obtain a pre-fired green body; Step 600: placing the pre-fired green body into a sintering furnace, and sintering the pre-fired green body in an air atmosphere and a nitrogen atmosphere in sequence to obtain a porous ceramic; In step 100, based on a chamber volume of 1 L, the volume of the organic porous matrix is ​​0.05 to 0.2 times the volume of the chamber, the pressure in the chamber is 100 to 500 mTorr, the power is 50 to 300 W, and the process is first performed in an argon atmosphere of 10 to 50 sccm for 6 to 10 minutes, and then in an oxygen atmosphere of 5 to 30 sccm for 6 to 10 minutes. The organic porous matrix is ​​a sponge with a ppi of 30 to 70. In step 600, the sintering process includes the following stages: In an air atmosphere, heat from room temperature to 400-500°C and keep warm for 1-2 hours; Switch the atmosphere to nitrogen, continue heating to 600-650°C, and keep warm for 1-2 hours; Maintain nitrogen atmosphere, continue to raise the temperature to 750-800℃, and keep it at this temperature for 1-2 hours; Maintain nitrogen atmosphere, continue to raise the temperature to 900-950°C, and keep warm for 1-2 hours; Maintaining the nitrogen atmosphere, the temperature is continued to rise to 1050-1200°C, kept at this temperature for 2-4 hours, and then cooled in the furnace to obtain porous ceramics.

2. The method for preparing the porous ceramic according to claim 1, wherein: The organic porous matrix is ​​a polyurethane sponge.

3. The method for preparing the porous ceramic according to claim 1, wherein: In step 200, the alkali solution is a NaOH solution with a mass fraction of 20 to 30%, the soaking time is 2 to 6 hours, and the soaking temperature is room temperature.

4. The method for preparing the porous ceramic according to claim 1, wherein: In step 300, plating a silver layer on the pore surface of the second modified substrate includes the following steps: soaking the second modified substrate in a silver nitrate solution for sensitization; After sensitization is completed, move into the plating solution; Glucose solution is added to the plating solution, and after the reaction is completed, washing and drying are performed to obtain the third modified matrix.

5. The method for preparing the porous ceramic according to claim 1, wherein: In step 400, the anionic surfactant solution is an SDS solution with a mass fraction of 2-4%, the soaking time is 1-3 hours, and the soaking temperature is 70-80°C.

6. The method for preparing the porous ceramic according to claim 1, wherein: In step 500, the preparation of the slurry includes the following steps: firstly, wet-grinding and mixing the ceramic powder and the sodium carboxymethyl cellulose solution, and then adding the polyvinyl alcohol solution and wet-grinding and mixing to obtain the slurry; The solid content of the slurry is 40-50%, the ceramic powder includes diatomaceous earth, alumina, magnesium oxide and kaolin in a mass ratio of (8-10):(4-6):(2-4):(2-4), the mass fraction of sodium carboxymethyl cellulose solution is 0.3-0.5%, and the mass fraction of polyvinyl alcohol solution is 2-4%.

7. The method for preparing the porous ceramic according to claim 1, wherein: In step 500, the drying is performed by first standing and drying at room temperature for 24 to 48 hours, and then drying at 50 to 70°C for 12 to 24 hours.

8. A porous ceramic, characterized in that: The porous ceramic is prepared by the preparation method of any one of claims 1 to 7.

Citation Information

Patent Citations

  • Method for rapidly removing organic template from cellular material

    CN103351005A

  • Preparation method of antibacterial, anti-mould and temperature regulating high buffering slow rebound polyurethane soft foam

    CN108003324A

Cited By

  • Temperature fuse

    CN224123334U