Medium-entropy pyrophosphate ceramic material with low thermal conductivity as well as preparation method and application of medium-entropy pyrophosphate ceramic material

By doping zirconium pyrophosphate with yttrium and niobium ions, and using magnesium oxide and polyethylene glycol solutions as sintering aids, medium-entropy pyrophosphate ceramic materials were prepared, which solved the structural phase change of zirconium pyrophosphate materials at high temperatures. problem, achieving low thermal conductivity and stable thermal expansion properties of the material, simplifying the process and reducing environmental impact.

CN118724583APending Publication Date: 2024-10-01ZHENGZHOU UNIVERSITY OF AERONAUTICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410765733.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing zirconium pyrophosphate materials have structural phase changes at high temperatures, resulting in large differences in thermal expansion coefficients. Repeated thermal cycles induce thermal stress, leading to material cracking and shortened service life. In addition, traditional preparation methods are complex, pollute the environment, have low yields, and are difficult to mass-produce. Scale application.

Method used

By mixing ammonium dihydrogen phosphate, zirconium oxide, yttrium oxide and niobium oxide at a molar ratio of 15:3:1, grinding, drying, heat treatment, adding magnesium oxide and polyethylene glycol solution as sintering aids, and pressing and forming and sintering to prepare medium-entropy pyrophosphate ceramic materials to avoid structural phase changes and reduce thermal conductivity and thermal expansion coefficient.

Benefits of technology

It achieves the stability of low thermal conductivity, low dielectric constant, low dielectric loss and thermal expansion coefficient of the material, simplifies the process flow, lowers the sintering temperature, reduces environmental pollution, extends the service life of the material, and reduces production costs. cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004892397290000011
    Figure HDA0004892397290000011
  • Figure HDA0004892397290000012
    Figure HDA0004892397290000012
  • Figure HDA0004892397290000021
    Figure HDA0004892397290000021
Patent Text Reader

Abstract

The invention provides a medium-entropy pyrophosphate ceramic material with low thermal conductivity and a preparation method and application thereof, and belongs to the technical field of ceramic materials. The preparation method comprises the following steps: mixing ammonium dihydrogen phosphate, zirconium oxide, yttrium oxide and niobium oxide, grinding, drying and carrying out heat treatment to obtain a powder raw material; mixing the powder raw material with a sintering aid, grinding and drying to obtain a ceramic raw material; carrying out compression molding on the ceramic raw material, and sintering to obtain the medium-entropy pyrophosphate ceramic material. The preparation method provided by the invention has the characteristics of simple process, short production period and environmental friendliness; and the prepared medium-entropy pyrophosphate ceramic material has the characteristics of low dielectric constant, low dielectric loss, low thermal conductivity, stable thermal expansion coefficient and no structural phase change.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ceramic materials, and in particular to a medium-entropy pyrophosphate ceramic material with low thermal conductivity, and a preparation method and application thereof. Background Art

[0002] The thermal insulation performance of materials mainly depends on thermal conductivity. In recent years, ceramic materials with low thermal conductivity have attracted people's attention. Zirconium pyrophosphate is a new type of low thermal conductivity material with the advantages of low thermal conductivity, small thermal expansion coefficient, and high temperature resistance. Zirconium pyrophosphate is doped with heterovalent elements to further reduce the thermal conductivity and medium and low temperature thermal expansion coefficient of zirconium phosphate. At the same time, it has the advantage of low dielectric constant, making it a new type of ceramic material with broader application prospects. It can be widely used in communications, electronics, military and other fields.

[0003] Existing technical research shows that zirconium pyrophosphate has low dielectric constant and dielectric loss, strong corrosion resistance, low thermal conductivity, low thermal expansion and other properties. However, zirconium pyrophosphate material undergoes a structural phase transition at around 290°C, and the thermal expansion coefficient before and after the phase transition is quite different. Repeated thermal cycles will introduce large thermal stress, causing the material to crack and even shorten the service life of the material. This performance defect limits the application prospects of the material.

[0004] At present, the commonly used methods for preparing zirconium pyrophosphate powder are coprecipitation, hydrothermal and solid phase methods. Among them, coprecipitation and hydrothermal methods have the disadvantages of complex process, environmental pollution, low yield and high production cost, which are difficult to be applied on a large scale. For example, the patented technology of "A preparation method of zirconium phosphate ceramic material" (CN1844042A) discloses a preparation method using zirconium oxide and 85% phosphoric acid as raw materials. In the preparation process, corrosive liquid is used, which endangers human health. In contrast, the solid phase method has a simple production process, short preparation cycle, short production cycle, high purity, and a relatively environmentally friendly production process, which has strong practical significance. Summary of the invention

[0005] Based on the above content, the purpose of the present invention is to provide a preparation method and application of a medium-entropy pyrophosphate ceramic material with low thermal conductivity. The preparation method provided by the present invention has the characteristics of simple process, short production cycle and environmental friendliness. The prepared medium-entropy pyrophosphate ceramic material has the characteristics of low dielectric constant, low dielectric loss, low thermal conductivity, stable thermal expansion coefficient and no structural phase change.

[0006] In order to achieve the above object, the present invention provides the following technical solution: a method for preparing a medium-entropy pyrophosphate ceramic material with low thermal conductivity, comprising the following steps:

[0007] The ammonium dihydrogen phosphate, zirconium oxide, yttrium oxide and niobium oxide are mixed, ground, dried and heat treated to obtain a powder raw material;

[0008] The powder raw material is mixed with a sintering aid, and then ground and dried to obtain a ceramic raw material;

[0009] The ceramic raw material is pressed into shape and then sintered to obtain the medium-entropy pyrophosphate ceramic material.

[0010] Preferably, the molar ratio of diammonium phosphate, zirconium oxide, yttrium oxide and niobium oxide is 15:3:1:1.

[0011] Preferably, the purity of the ammonium dihydrogen phosphate is greater than 99.0%; the purity of the zirconium oxide is greater than 99.99%; the purity of the yttrium oxide is greater than 99.5%; and the purity of the niobium oxide is greater than 99.5%.

[0012] Preferably, the heat treatment is: keeping warm at 1000° C. for 1 hour.

[0013] Preferably, the sintering aid is magnesium oxide and polyethylene glycol solution.

[0014] Preferably, the amount of the magnesium oxide is 1wt% of the powder raw material; the amount of the polyethylene glycol solution is 8-10wt% of the powder raw material.

[0015] Preferably, the concentration of the polyethylene glycol solution is 8-10 wt %.

[0016] Preferably, the sintering is carried out by keeping the temperature at 1000-1100° C. for 1-2 hours in an air atmosphere and normal pressure.

[0017] The present invention also provides a medium-entropy pyrophosphate ceramic material with low thermal conductivity prepared by the preparation method described in the above technical solution.

[0018] The present invention also provides the application of the medium-entropy pyrophosphate ceramic material with low thermal conductivity in the fields of communication, electronics and military.

[0019] Beneficial technical effects:

[0020] 1. The manufacturing process of the present invention is simple, the manufacturing cycle is short, and compared with zirconium pyrophosphate ceramics, the sintering temperature is significantly reduced, which is helpful for energy conservation and emission reduction.

[0021] 2. The present invention prepares a new type of medium-entropy pyrophosphate material by replacing part of the zirconium ions in zirconium pyrophosphate with yttrium and niobium ions, which not only reduces the thermal conductivity of the zirconium pyrophosphate ceramic and improves its thermal insulation performance, but also no structural phase change is found at the test temperature, and its thermal expansion performance is stable, which fully reduces the damage to the material caused by thermal shock.

[0022] 3. The present invention uses magnesium oxide and polyethylene glycol as sintering aids. Magnesium oxide reacts with the new phosphate to form a low melting point phase, which promotes the sintering densification of the medium-entropy zirconium pyrophosphate ceramic material and can reduce its sintering difficulty. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 is an X-ray diffraction pattern of the medium-entropy pyrophosphate ceramic material prepared in Example 2;

[0025] Figure 2 This is a SEM image of a cross section of a medium-entropy pyrophosphate ceramic material block prepared in Example 2;

[0026] Figure 3 The curve showing the change of the relative length of the low temperature section of the medium entropy pyrophosphate ceramic material block prepared in Example 2 with the temperature;

[0027] Figure 4 This is a curve showing the change in relative length of the high temperature section of the medium-entropy pyrophosphate ceramic material block prepared in Example 2 as a function of temperature. DETAILED DESCRIPTION

[0028] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0029] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0030] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0031] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0032] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0033] The present invention provides a method for preparing a medium-entropy pyrophosphate ceramic material with low thermal conductivity, comprising the following steps:

[0034] The ammonium dihydrogen phosphate, zirconium oxide, yttrium oxide and niobium oxide are mixed, ground, dried and heat treated to obtain a powder raw material;

[0035] The powder raw material is mixed with a sintering aid, and then ground and dried to obtain a ceramic raw material;

[0036] The ceramic raw material is pressed into shape and then sintered to obtain the medium-entropy pyrophosphate ceramic material.

[0037] The present invention replaces part of the zirconium ions in the zirconium pyrophosphate with heterovalent ions (yttrium and niobium ions) whose average radius is close to that of the zirconium ions, regulates the phase change of the material (no phase change is found in the test temperature range), and prepares a new pyrophosphate, which is a one-step sintering method to obtain a new material (i.e., the powder raw material), reduces the thermal expansion coefficient of the new material in the low temperature section, and greatly reduces the damage of thermal shock to the ceramic material. The new material then promotes the sintering densification of the medium-entropy zirconium pyrophosphate ceramic material by adding a sintering aid, which can reduce its sintering difficulty.

[0038] In some embodiments, the molar ratio of diammonium phosphate, zirconium oxide, yttrium oxide and niobium oxide is 15:3:1:1.

[0039] In the present invention, when the amount of diammonium phosphate is excessive, the raw materials will be wasted, and the excess diammonium phosphate will release more ammonia; the molar ratio of zirconium oxide to yttrium oxide / niobium oxide will affect the degree of positive thermal expansion of the obtained new phosphate ceramic. If the doping degree is higher than 3:1, the positive thermal expansion coefficient of the material will increase, and there will be a structural phase change; if the doping ratio is lower than 3:1, the degree of positive thermal expansion of the material is roughly the same, but too little zirconium oxide will reduce the mechanical properties of the prepared new material. Therefore, in order to obtain a ceramic material with no structural phase change and a low expansion coefficient, the present invention is preferably within the above parameter range.

[0040] In some embodiments, the purity of the ammonium dihydrogen phosphate is greater than 99.0%; the purity of the zirconium oxide is greater than 99.99%; the purity of the yttrium oxide is greater than 99.5%; and the purity of the niobium oxide is greater than 99.5%.

[0041] In some embodiments, the powder raw material and the sintering aid are mixed and ground for 1 to 2 hours; the grinding medium used for the grinding is anhydrous ethanol; and the purity of the anhydrous ethanol is greater than 99%.

[0042] In some embodiments, the heat treatment is: keeping the temperature at 1000° C. in an air atmosphere for 1 hour.

[0043] In the present invention, if the heat treatment temperature is too low, the material will not be fully crystallized, and if the temperature is too high, the phosphorus source will be seriously lost, resulting in low material purity. Therefore, the present invention preferably uses the above heat treatment temperature.

[0044] In some embodiments, after the heat treatment is completed, the step of crushing the material obtained by the heat treatment is further included. The present invention has no special requirements on the crushing method, and a method well known to those skilled in the art can be selected, such as grinding.

[0045] In some embodiments, the sintering aid is magnesium oxide and polyethylene glycol solution.

[0046] In some embodiments, the amount of magnesium oxide used is 1 wt % of the powder raw material; the amount of polyethylene glycol solution used is 8-10 wt % of the powder raw material.

[0047] The present invention sets the amount of magnesium oxide and the amount of polyethylene glycol solution as the above parameters because: too much magnesium oxide will cause obvious impurities in the material, and less than 1wt% will cause the strength of the ceramic material to decrease. Too much polyethylene glycol will cause the ceramic material to appear agglomerated in the microstructure, and too little polyethylene glycol will cause interlayer cracks. By adjusting the amount of polyethylene glycol added, the density and thermal conductivity of the material can be adjusted.

[0048] In some embodiments, the purity of the magnesium oxide is greater than 99.99%.

[0049] In some embodiments, the concentration of the polyethylene glycol solution is 8-10 wt %.

[0050] In some embodiments, the powder raw material is mixed with magnesium oxide and polyethylene glycol solution and then ground for 1 to 2 hours; the grinding medium used for the grinding is anhydrous ethanol; and the purity of the anhydrous ethanol is greater than 99%.

[0051] In some embodiments, the compression molding method is cold isostatic pressing at 400-600 MPa.

[0052] In some embodiments, the sintering is performed by keeping the temperature at 1000-1100° C. for 1-2 hours in an air atmosphere and normal pressure.

[0053] In the present invention, if the sintering temperature is too low, the grain growth will be poor and the finished product will still be in a powder state. If the sintering temperature is too high, the ceramic will bulge. Therefore, the present invention sets the sintering temperature to the above parameter range.

[0054] The present invention also provides a medium-entropy pyrophosphate ceramic material with low thermal conductivity prepared by the preparation method described in the above technical solution.

[0055] The present invention also provides the application of the medium-entropy pyrophosphate ceramic material with low thermal conductivity in the fields of communication, electronics and military.

[0056] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.

[0057] The purity of the ammonium dihydrogen phosphate used in the embodiment is greater than 99.0%; the purity of zirconium oxide is greater than 99.99%; the purity of yttrium oxide is greater than 99.5%; the purity of niobium oxide is greater than 99.5%; the purity of magnesium oxide is greater than 99.99%; and the purity of anhydrous ethanol is greater than 99%.

[0058] Example 1

[0059] Step 1. According to the molar ratio of ammonium dihydrogen phosphate: zirconium oxide: yttrium oxide: niobium oxide of 15:3:1:1, the ammonium dihydrogen phosphate, zirconium oxide, yttrium oxide and niobium oxide are mixed to obtain a mixture I; then the mixture I is ground in an agate mortar with anhydrous ethanol as a medium for 1 hour, and dried to obtain a grind; then the grind is kept warm at 1000° C. in an air atmosphere for 1 hour, and the powder raw material II is obtained by crushing.

[0060] Step 2: Add magnesium oxide and polyethylene glycol to the powder raw material II (the amount of magnesium oxide is 1wt% of the powder raw material II, the amount of polyethylene glycol solution is 10wt% of the powder raw material II, and the concentration of the polyethylene glycol solution is 8wt%) to obtain a mixture III, and then grind the mixture III in an agate mortar with anhydrous ethanol as the medium for 2 hours, and dry to obtain a ceramic raw material IV.

[0061] Step 3: cold isostatically press the ceramic raw material IV at 500 MPa to obtain a medium-entropy pyrophosphate ceramic body.

[0062] Step 4: In an air atmosphere and normal pressure, the pyrophosphate ceramic body is heated to 1000° C. and kept warm for 2 hours to obtain a medium-entropy pyrophosphate ceramic material.

[0063] The low thermal conductivity medium entropy pyrophosphate ceramic prepared in this embodiment is analyzed by X-ray diffraction, and the main crystal phase is cubic zirconium pyrophosphate phase, and the volume density is 1.805 g / cm 3 ; Dielectric constant at room temperature is 14.6 (frequency is 10MHz); Dielectric loss is 0.00313 (frequency is 10MHz); Thermal conductivity at room temperature is 0.4107W / (m·K); Thermal expansion coefficient is 7.11×10 -6 K -1 (Temperature range is -70~800℃).

[0064] Example 2

[0065] Step 1. According to the molar ratio of ammonium dihydrogen phosphate: zirconium oxide: yttrium oxide: niobium oxide of 15:3:1:1, the ammonium dihydrogen phosphate, zirconium oxide, yttrium oxide and niobium oxide are mixed to obtain a mixture I; then the mixture I is ground in an agate mortar with anhydrous ethanol as a medium for 2 hours, and dried to obtain a grind; then the grind is kept warm in an air atmosphere at 1100° C. for 1 hour, and the powder raw material II is obtained by crushing.

[0066] Step 2: Add magnesium oxide and polyethylene glycol to the powder raw material II (the amount of magnesium oxide is 1wt% of the powder raw material II, the amount of polyethylene glycol solution is 10wt% of the powder raw material II, and the concentration of the polyethylene glycol solution is 8wt%) to obtain a mixture III, and then grind the mixture III in an agate mortar with anhydrous ethanol as the medium for 2 hours, and dry to obtain a ceramic raw material IV.

[0067] Step 3: cold isostatically press the ceramic raw material IV at 600 MPa to obtain a medium-entropy pyrophosphate ceramic embryo.

[0068] Step 4: In an air atmosphere and normal pressure, the pyrophosphate ceramic body is heated to 1100° C. and kept warm for 2 hours to obtain a medium-entropy pyrophosphate ceramic material.

[0069] The X-ray diffraction pattern of the medium entropy pyrophosphate ceramic material prepared in this embodiment is as follows: Figure 1 As shown, the SEM image of the cross section of the medium entropy pyrophosphate ceramic material block is as follows Figure 2 As shown. Figure 1 It can be seen that after zirconium pyrophosphate is doped, the product is pure phase, indicating that Y and Nb elements replace Zr element in the unit cell. Y and Nb elements inhibit the large positive thermal expansion of zirconium phosphate at medium and low temperatures by changing the polyhedral bond angle. The doping of Y and Nb elements will also aggravate phonon scattering, thereby reducing the thermal conductivity of the material. Figure 2 It can be seen that the microstructure is porous and the grain growth is obvious.

[0070] The low thermal conductivity medium entropy pyrophosphate ceramic prepared in this embodiment is analyzed by X-ray diffraction, and the main crystal phase is cubic zirconium pyrophosphate phase, and the volume density is 2.01g / cm 3 ; The room temperature dielectric constant is 11.6 (frequency is 10MHz); the dielectric loss is 0.00253 (frequency is 10MHz); the room temperature thermal conductivity is 0.4474W / (m·K), and the thermal expansion coefficient is 7.18×10 -6 K -1 (Temperature range is -70~800℃).

[0071] Figure 3 , Figure 4 The relative lengths of the low-temperature section and the high-temperature section of the medium-entropy pyrophosphate ceramic material block prepared in this embodiment vary with temperature. It can be seen from the figure that no phase change is found in the measurement range of -70 to 800 ° C and it shows positive expansion, and the thermal expansion coefficient is 7.18×10 -6 K -1 . The doping of Y and Nb elements can cause changes in the polyhedral bond angles, promote the stretching vibration of the bridging oxygen atoms, and thus reduce the thermal expansion rate of the material. Compared with zirconium pyrophosphate, not only is there no phase change, but the thermal expansion is also greatly suppressed. The harmful effects of thermal shock on the material are greatly reduced, and the service life of the material is extended.

[0072] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a medium-entropy pyrophosphate ceramic material with low thermal conductivity, characterized in that: The following steps are involved: The ammonium dihydrogen phosphate, zirconium oxide, yttrium oxide and niobium oxide are mixed, ground, dried and heat treated to obtain a powder raw material; The powder raw material is mixed with a sintering aid, and then ground and dried to obtain a ceramic raw material; The ceramic raw material is pressed into shape and then sintered to obtain the medium-entropy pyrophosphate ceramic material.

2. The preparation method according to claim 1, characterized in that: The molar ratio of the ammonium dihydrogen phosphate, zirconium oxide, yttrium oxide and niobium oxide is 15:3:1:

1.

3. The preparation method according to claim 1 or 2, characterized in that: The purity of the ammonium dihydrogen phosphate is greater than 99.0%; the purity of the zirconium oxide is greater than 99.99%; the purity of the yttrium oxide is greater than 99.5%; and the purity of the niobium oxide is greater than 99.5%.

4. The preparation method according to claim 1, characterized in that: The heat treatment is: keeping the temperature at 1000° C. for 1 hour.

5. The preparation method according to claim 1, characterized in that: The sintering aids are magnesium oxide and polyethylene glycol solution.

6. The preparation method according to claim 5, characterized in that: The amount of magnesium oxide used is 1wt% of the powder raw material; the amount of polyethylene glycol solution used is 8-10wt% of the powder raw material.

7. The preparation method according to claim 5, characterized in that: The concentration of the polyethylene glycol solution is 8-10 wt %.

8. The preparation method according to claim 1, characterized in that: The sintering is carried out by keeping the temperature at 1000-1100° C. for 1-2 hours under air atmosphere and normal pressure.

9. A medium-entropy pyrophosphate ceramic material with low thermal conductivity prepared by the preparation method according to any one of claims 1 to 8.

10. Application of the medium-entropy pyrophosphate ceramic material with low thermal conductivity as claimed in claim 9 in the fields of communications, electronics and military.