High-temperature-resistant and high-stability gradient structure environmental barrier coating bonding layer and preparation method thereof

By preparing a lattice structure of Si bottom layer, HfSiO4-Si middle layer and HfSiO4 top layer on the ceramic matrix composite material, the problem of chemical instability caused by the low melting point of the bonding layer and oxide reaction of the ceramic matrix composite material in a high temperature environment is solved. , achieving high bonding strength and chemical stability at high temperatures, extending the service temperature and life of the coating.

CN118724601AActive Publication Date: 2024-10-01AVIC BEIJING INST OF AERONAUTICAL MATERIALS

Patent Information

Application Number
CN202410827268.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-01
Estimated Expiration
2044-06-25

AI Technical Summary

Technical Problem

The chemical instability of existing ceramic matrix composite materials due to the low melting point of the Si bonding layer and oxide reaction in high-temperature environments limits their application temperature and reliability in aeroengines.

Method used

Atmospheric plasma spraying technology is used to prepare a high-temperature-resistant, highly stable gradient structure environmental barrier coating, including a lattice structure of Si bottom layer, HfSiO4-Si middle layer and HfSiO4 top layer. By optimizing the composition and process parameters, the bonding of the bonding layer is improved. Strength and chemical stability.

Benefits of technology

It achieves high bonding strength and chemical stability of the bonding layer and the matrix of the ceramic matrix composite material at high temperatures, extends the service temperature and life of the coating, and breaks through the problems of low temperature bearing capacity and chemical instability in the existing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004910884650000011
    Figure HDA0004910884650000011
  • Figure HDA0004910884650000012
    Figure HDA0004910884650000012
  • Figure HDA0004910884650000021
    Figure HDA0004910884650000021
Patent Text Reader

Abstract

The invention provides a high-temperature-resistant and high-stability gradient structure environmental barrier coating bonding layer and a preparation method thereof. The high-temperature-resistant and high-stability gradient structure environmental barrier coating bonding layer comprises a Si bottom layer of a lattice structure, an HfSiO4-Si middle layer and an HfSiO4 top layer which are sequentially arranged. The bonding layer is prepared by adopting an atmospheric plasma spraying technology. The bonding layer with the gradient structure has the advantages of high temperature resistance, strong bonding and high-temperature phase stability, and is expected to break through the bottleneck of low temperature bearing capacity and high-temperature chemical instability of the existing environment barrier coating bonding layer system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of high-temperature protective coating materials, and in particular relates to a high-temperature resistant, high-stability gradient structure environmental barrier coating bonding layer and a preparation method thereof. Background Art

[0002] Ceramic matrix composites (CMCs) are expected to replace traditional high-temperature alloys and become the main candidate material for the hot end components of the new generation of high-performance aircraft engines due to their high temperature resistance, low density, excellent high-temperature mechanical properties and other performance advantages. However, in the engine gas environment, the service performance of CMCs components declines sharply due to water vapor-oxygen coupled corrosion, and ultra-high temperature and long-life environmental barrier coatings (EBCs) must be prepared on their surfaces to improve the service reliability and stability of the composite materials.

[0003] At present, the most widely used third-generation EBCs system consists of a Si bonding layer, a mullite intermediate layer, and a rare earth silicate environmental barrier layer. Among them, the Si bonding layer has the characteristics of high bonding strength with CMCs and close thermal expansion coefficient, and plays a vital role in the entire CMCs-EBCs system. However, the melting point of the Si bonding layer is only 1410℃, which will be greatly reduced in the presence of impurities. In addition, SiO2 formed by Si oxidation undergoes an α-β phase transition during the hot and cold alternation process, and the resulting tensile stress is the main cause of Si / SiO2 interface cracking. More seriously, at high temperatures, SiO2 reacts with the oxide in the environmental barrier layer to form a glassy phase, causing coating damage and failure. The above reasons limit the long-term use temperature of the EBCs system with Si as the bonding layer to below 1350℃. As aircraft engines develop towards a higher thrust-to-weight ratio, it is urgent to modify the material and structure of the Si bonding layer.

[0004] As a silicate material, HfSiO4 not only has a higher melting point (~2758℃), but also has a thermal expansion coefficient similar to that of CMCs matrix (3.11-5.97×10 -6 K -1 ), is a new type of high temperature resistant bonding layer material with great application potential. However, HfSiO4 itself has a low bonding strength with the substrate, and in the preparation process, due to the evaporation of SiO2, it is easy to cause unfavorable phenomena such as component segregation and loose structure, which limits its further application. Summary of the invention

[0005] In view of this, the object of the present invention is to provide a high-temperature resistant, high-stability gradient structure environmental barrier coating bonding layer and a preparation method thereof. The bonding layer has high bonding strength with the substrate and can withstand temperatures up to 1450°C. At this temperature, the heterogeneous interfaces in the EBCs system remain chemically stable, which can effectively improve the service temperature and performance of the CMCs hot end components.

[0006] The present invention provides a high-temperature resistant and highly stable gradient structure environmental barrier coating bonding layer, which is characterized by comprising a Si bottom layer, a HfSiO4-Si middle layer and a HfSiO4 top layer arranged in sequence.

[0007] Preferably, in the HfSiO4-Si intermediate layer, Si is uniformly distributed in the HfSiO4 in the form of dots;

[0008] The mass content of HfSiO4 is between 70% and 90%.

[0009] Preferably, the mass content of HfSiO4 in the HfSiO4 top layer is greater than 90%.

[0010] Preferably, the thickness of the Si bottom layer of the lattice structure is 10 to 40 μm;

[0011] The thickness of the HfSiO4-Si intermediate layer is 10 to 50 μm;

[0012] The thickness of the HfSiO4 top layer is 20-50 μm.

[0013] The present invention provides a method for preparing a high temperature resistant, high stability gradient structure environmental barrier coating bonding layer as described in the above technical solution, comprising the following steps:

[0014] A) pretreating the ceramic matrix composite material matrix;

[0015] B) using atmospheric plasma spraying technology to sequentially prepare a Si bottom layer, a HfSiO4-Si middle layer and a HfSiO4 top layer of a lattice structure on the surface of the pretreated ceramic matrix composite material substrate;

[0016] C) heat treating the coating to obtain a high temperature resistant, highly stable gradient structure environmental barrier coating bonding layer.

[0017] Preferably, the matrix material is a ceramic-based composite material;

[0018] The pretreatment includes cleaning, sandblasting and plasma jet heating of the base material in sequence.

[0019] Preferably, in the process of forming the Si bottom layer with a lattice structure by atmospheric plasma spraying, the base material is shielded by a porous mesh tooling, argon and hydrogen are used as plasma, the argon flow rate is 40-60L / min, the hydrogen flow rate is 5-15L / min, the spraying distance is 80-150mm, the spraying current is 300-600A, the powder feeding rate is 10-30%, and the particle size of the Si powder is 15-60μm.

[0020] Preferably, in the process of forming the HfSiO4-Si intermediate layer by atmospheric plasma spraying, argon and hydrogen are used as plasma, the flow rate of argon is 40-80L / min, the flow rate of hydrogen is 5-15L / min, the spraying distance is 100-200mm, the spraying current is 500-800A, the powder feeding rate is 10-30%, the particle size of Si powder is 15-60μm, and the particle size of HfSiO4 powder is 15-45μm.

[0021] Preferably, in the process of forming the HfSiO4 top layer by atmospheric plasma spraying, HfO2 and SiO2 with a molar ratio of 1: (1.2-1.8) are used as raw materials, argon and hydrogen are used as plasma, the argon flow rate is 40-80 L / min, the hydrogen flow rate is 5-15 L / min, the spraying distance is 100-200 mm, the spraying current is 400-600 A, the powder feeding rate is 10-30%, the particle size of the HfO2 powder is 15-45 μm, and the particle size of the SiO2 powder is 15-60 μm.

[0022] Preferably, in step C), the heat treatment temperature is 1400-1600° C., and the heat treatment time is 10-30 hours.

[0023] The present invention provides a high temperature resistant, highly stable gradient structure environmental barrier coating bonding layer, comprising a Si bottom layer, a HfSiO4-Si middle layer and a HfSiO4 top layer arranged in sequence in a lattice structure. The present invention adopts atmospheric plasma spraying technology to prepare the above bonding layer. The gradient structure bonding layer described in the present invention has the advantages of high temperature resistance, strong bonding, and high temperature phase stability, and is expected to break through the bottleneck of low temperature bearing capacity and high temperature chemical instability of the existing environmental barrier coating bonding layer system. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Schematic diagram of the cross-sectional structure of a high-temperature resistant, high-stability gradient structure environmental barrier coating bonding layer prepared on the surface of a ceramic-based composite material in one embodiment of the present invention, wherein 1 is a ceramic-based composite material substrate, 2 is a Si bottom layer of a "lattice structure", 3 is a HfSiO4-Si middle layer, and 4 is a HfSiO4 top layer;

[0025] Figure 2 This is a flow chart of a method for preparing a high temperature resistant, highly stable gradient structure environmental barrier coating bonding layer prepared on the surface of a ceramic matrix composite material in one embodiment of the present invention;

[0026] Figure 3 This is a surface morphology of the bonding layer of the gradient structure environmental barrier coating in Example 1 of the present invention. DETAILED DESCRIPTION

[0027] The present invention provides a high-temperature resistant and highly stable gradient structure environmental barrier coating bonding layer, which is characterized by comprising a Si bottom layer, a HfSiO4-Si middle layer and a HfSiO4 top layer arranged in sequence.

[0028] The bonding layer provided by the present invention is bonded to the substrate and has high bonding strength; the substrate material is a ceramic composite material substrate, namely a CMCs substrate. The present invention has no special restrictions on the specific composition of the substrate material, and any ceramic composite material substrate conventionally used in the art can be used.

[0029] The bonding layer provided by the present invention comprises a Si bottom layer with a lattice structure, the Si bottom layer with a lattice structure is in contact with the substrate material, and the thickness of the Si bottom layer is preferably 10 to 40 μm, more preferably 20 to 30 μm. According to the research of the present invention, the Si bonding layer with the above structure and thickness can retain the bonding force with the substrate to the maximum extent.

[0030] The bonding layer provided by the present invention includes a HfSiO4-Si intermediate layer in contact with the Si bottom layer; in the HfSiO4-Si intermediate layer, the preferred content of the HfSiO4 phase is between 70% and 90%, more preferably between 80% and 90%, such as 80%, 85%, 90%, preferably with any of the above values ​​as the upper or lower limit of the range value; the thickness of the HfSiO4-Si intermediate layer is preferably 10 to 50 μm, more preferably 30 to 50 μm. According to the research of the present invention, the HfSiO4-Si intermediate layer with the above composition and thickness range can fully consume the HfO2 phase formed by the volatilization of SiO2, and at the same time exert the high-temperature self-healing function.

[0031] The bonding layer provided by the present invention includes a HfSiO4 top layer in contact with the HfSiO4-Si intermediate layer; in the HfSiO4 top layer, the preferred content of the HfSiO4 phase is greater than 90%, more preferably greater than 95%, such as 96%, 97%, 98%, 99%, 100%, preferably a range value with any of the above values ​​as the upper or lower limit; the thickness of the HfSiO4 top layer is preferably 20 to 50 μm, more preferably 20 to 40 μm. This study found that the HfSiO4 top layer with the above composition and thickness range has excellent oxygen barrier effect, and maintains high temperature chemical stability with surface BSAS, mullite or rare earth silicate and other environmental barrier materials.

[0032] The "lattice structure" Si bottom layer adopted in the present invention can not only ensure the bonding strength between the adhesive layer and the CMCs matrix, but also inhibit the peeling of the coating caused by the softening and melting of Si at high temperature. In the HfSiO4-Si intermediate layer, no chemical reaction occurs between HfSiO4 and Si, and the main phase HfSiO4 has an extremely low oxygen permeability, which effectively avoids the disadvantage of rapid oxidation of Si. The second phase Si is distributed in the HfSiO4 matrix in a dotted form, and can react quickly with the HfO2 phase precipitated in the HfSiO4, while softening and melting at high temperature to fill the internal cracks of the coating. In the HfSiO4 top layer, HfSiO4 has excellent chemical stability and will not chemically react with environmental barrier materials such as BSAS, mullite or rare earth silicates on its surface.

[0033] The present invention provides a method for preparing a high temperature resistant, high stability gradient structure environmental barrier coating bonding layer as described in the above technical solution, comprising the following steps:

[0034] A) pretreating the ceramic matrix composite material matrix;

[0035] B) using atmospheric plasma spraying technology to sequentially prepare a Si bottom layer, a HfSiO4-Si middle layer and a HfSiO4 top layer of a lattice structure on the surface of the pretreated ceramic matrix composite material substrate;

[0036] C) heat treating the coating to obtain a high temperature resistant, highly stable gradient structure environmental barrier coating bonding layer.

[0037] See also Figure 2 , Figure 2 The present invention is a flow chart of a method for preparing a high temperature resistant, highly stable gradient structure environmental barrier coating bonding layer prepared on the surface of a ceramic-based composite material in one embodiment of the present invention.

[0038] The present invention pre-treats the ceramic-based composite material matrix. The pre-treatment in the present invention preferably includes the following steps:

[0039] 1) Clean and dry the base material;

[0040] 2) Sandblasting after drying;

[0041] 3) Plasma jet heating after sandblasting.

[0042] The present invention uses acetone to perform ultrasonic cleaning on the base material, and the ultrasonic cleaning time is 10 to 30 minutes, preferably 15 to 20 minutes; the drying is performed in an oven; the drying temperature is 100 to 120° C., preferably 110 to 115° C.; the drying time is 15 to 30 minutes, preferably 20 to 25 minutes.

[0043] In the present invention, in order to increase the surface roughness of the ceramic matrix composite material and thus improve the bonding force between the bonding layer and the substrate, the cleaned substrate is sandblasted. The present invention preferably uses 100-300 mesh quartz sand to sandblast the cleaned substrate, preferably 150-200 mesh; the sandblasting pressure is 0.1-0.3 MPa, more preferably 0.2-0.3 MPa, and the sandblasting time is preferably 10-30 seconds, more preferably 15-25 seconds.

[0044] The present invention performs plasma jet heating on the sandblasted ceramic-based composite material substrate to make its surface temperature reach 400-600°C, preferably 500-600°C.

[0045] After obtaining the pretreated substrate material, the present invention uses atmospheric plasma spraying technology to sequentially prepare a "lattice structure" Si bottom layer, a HfSiO4-Si middle layer and a HfSiO4 top layer on its surface to obtain a gradient structure bonding layer.

[0046] In the process of preparing the "lattice structure" Si bottom layer by atmospheric plasma spraying, a customized porous mesh tooling is used to shield the base material, and the diameter of the circular hole is preferably 0.2-1 mm, more preferably 0.3-0.4 mm, such as 0.3, 0.35, 0.4 mm, preferably a range value with any of the above values ​​as the upper or lower limit; the hole spacing is preferably 0.3-0.8 mm, more preferably 0.4-0.5 mm, such as 0.4 mm, 0.45 mm, 0.5 mm, preferably a range value with any of the above values ​​as the upper or lower limit; argon and hydrogen are used as plasma, argon The flow rate of the gas is preferably 40 to 60 L / min, more preferably 40 to 50 L / min, such as 40 L / min, 45 L / min, 50 L / min, 55 L / min, 60 L / min, preferably a range value with the above arbitrary numerical value as the upper or lower limit; the flow rate of the hydrogen is preferably 5 to 15 L / min, more preferably 6 to 8 L / min, such as 5 L / min, 6 L / min, 7 L / min, 8 L / min, 9 L / min, 10 L / min, 11 L / min, 12 L / min, 13 L / min, 14 L / min, 15 L / min, 16 L / min, 17 L / min, 18 L / min, 19 L / min, 20 L / min, 21 L / min, 22 L / min, 23 L / min, 24 L / min, 25 L / min, 26 L / min, 27 L / min, 28 L / min, 29 L / min, 30 L / min, 31 L / min, 32 L / min, 33 L / min, 34 L / min, 35 L / min, 36 L / min, 37 L / min, 38 L / min, 39 L / min, 40 L / min, 41 L / min, 42 L / min, 43 L / min, 44 L / min, 45 L / min, 46 L / min, 47 L / min, 48 L / min, 49 L / min, 50 L / min, 51 L / min, 52 L / min, 53 L / min, 54 L / min, 56 L / min, 57 L / min, 58 L / min, 59 L / min 4L / min, 15L / min, preferably a range value with any of the above values ​​as the upper or lower limit; the spraying distance is preferably 80-150mm, more preferably 100-120mm, such as 80mm, 90mm, 100mm, 110mm, 120mm, 130mm, 140mm, 150mm, preferably a range value with any of the above values ​​as the upper or lower limit; the spraying current is preferably 300-600A, more preferably 400-550A, such as 300A, 350A, 400A, 450A, 500A, 550A, 6 00A, preferably a range value with any of the above values ​​as the upper or lower limit; the powder feeding rate is preferably 10-30%, more preferably 20-25%, such as 10%, 15%, 20%, 25%, 30%, preferably a range value with any of the above values ​​as the upper or lower limit; the powder particle size of Si is preferably 15-60μm, more preferably 15-45μm, specifically such as 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, preferably a range value with any of the above values ​​as the upper or lower limit.

[0047] In the process of preparing the HfSiO4-Si intermediate layer by atmospheric plasma spraying, Si powder and HfSiO4 powder are mechanically mixed in proportion, and the mass ratio of Si to HfSiO4 is preferably 1:(2-10), more preferably 1:(6-8), such as 1:6, 1:7, 1:8, preferably a range value with any of the above values ​​as the upper or lower limit; argon and hydrogen are used as plasma, and the flow rate of argon is preferably 40-80 L / min, more preferably 50-65 L / min, such as 40 L / min, 45 L / min, 50 L / min, 55 L / min, 60 L / min, 65 L / min, The flow rate of hydrogen is preferably 5-15L / min, more preferably 8-12L / min, such as 5L / min, 6L / min, 7L / min, 8L / min, 9L / min, 10L / min, 11L / min, 12L / min, 13L / min, 14L / min, 15L / min, preferably a range value with any of the above values ​​as the upper or lower limit; the spraying distance is preferably 100-200mm, more preferably 120-180mm, Such as 100mm, 110mm, 120mm, 130mm, 140mm, 150mm, 160mm, 170mm, 180mm, 190mm, 200mm, preferably a range value with any of the above values ​​as the upper or lower limit; the spraying current is preferably 500-800A, more preferably 550-650A, such as 500A, 550A, 600A, 650A, 700A, 800A, selected as a range value with any of the above values ​​as the upper or lower limit; the powder feeding rate is preferably 10-30%, more preferably 20-30%, such as 10%, 15%, 20%, 25%, 30%, Preferably, it is a range value with any of the above-mentioned numerical values ​​as the upper or lower limit. The powder particle size of HfSiO4 is preferably 15-45μm, more preferably 20-40μm, such as 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, preferably a range value with any of the above-mentioned numerical values ​​as the upper or lower limit; the powder particle size of Si is preferably 15-60μm, more preferably 15-45μm, such as 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, preferably a range value with any of the above-mentioned numerical values ​​as the upper or lower limit.

[0048] In the process of preparing the HfSiO4 top layer by atmospheric plasma spraying, HfO2 powder and SiO2 powder are mechanically mixed in proportion, and the molar ratio of HfO2 to SiO2 is preferably 1:(1.2-1.8), and more preferably 1:(1.3-1.5), such as 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8; argon and hydrogen are used as plasma, and the flow rate of argon is preferably 40-80 L / min, and more preferably 45-55 L / min, such as 40 L / min, 45 L / min, 50 L / min, 55 L / min. in, 60L / min, 65L / min, 70L / min, 75L / min, 80L / min, preferably a range value with any of the above values ​​as the upper or lower limit; the flow rate of hydrogen is preferably 5-15L / min, more preferably 8-12L / min, such as 5L / min, 6L / min, 7L / min, 8L / min, 9L / min, 10L / min, 11L / min, 12L / min, 13L / min, 14L / min, 15L / min, preferably a range value with any of the above values ​​as the upper or lower limit; the spraying distance is preferably 100-200mm , more preferably 120-150mm, such as 100mm, 110mm, 120mm, 130mm, 140mm, 150mm, 160mm, 170mm, 180mm, 190mm, 200mm, preferably a range value with any of the above values ​​as the upper or lower limit; the spraying current is preferably 400-600A, more preferably 450-550A, such as 400A, 450A, 500A, 550A, 600A is preferably a range value with any of the above values ​​as the upper or lower limit; the powder feeding rate is preferably 10-30%, more preferably 20-30%, such as 10%, 15%, 20%, 25 %, 30%, preferably a range value with any of the above values ​​as the upper or lower limit, the powder particle size of HfO2 is 15-45μm, more preferably 20-40μm, such as 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, preferably a range value with any of the above values ​​as the upper or lower limit; the powder particle size of SiO2 is preferably 15-60μm, more preferably 15-45μm, such as 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, preferably a range value with any of the above values ​​as the upper or lower limit.

[0049] After the above-mentioned gradient structure is prepared by atmospheric plasma spraying, the coating is subjected to high-temperature heat treatment to obtain a high-temperature resistant and highly stable gradient structure environmental barrier coating bonding layer.

[0050] In the present invention, the temperature of the vacuum heat treatment is preferably 1400-1600°C, more preferably 1450-1550°C, such as 1400°C, 1450°C, 1500°C, 1550°C, 1600°C, preferably a range value with any of the above values ​​as the upper or lower limit; the time of the high temperature heat treatment is preferably 10-30h, more preferably 15-24 hours, preferably a range value with any of the above values ​​as the upper or lower limit.

[0051] The present invention modifies the composition and structure of the Si bonding layer in the third-generation environmental barrier coating system to obtain a high-temperature resistant and highly stable gradient structure bonding layer, which has the following advantages:

[0052] (1) The "lattice structure" Si bottom layer described in the present invention can maintain the bonding force between the coating and the substrate to the maximum extent, while avoiding interface stratification caused by Si softening and melting or high-temperature strength reduction.

[0053] (2) In the HfSiO4-Si intermediate layer of the present invention, the addition of Si can react with the HfO2 precipitated during the spraying process to generate HfSiO4 again, ensuring that the HfSiO4 phase content meets the design requirements. In addition, at high temperatures, the point-distributed Si softens and melts, which is conducive to filling the microcracks inside the coating, thereby increasing the service life of the coating.

[0054] (3) The HfSiO4 top layer of the present invention not only has an extremely low oxygen diffusion rate, but also maintains chemical stability with environmental barrier materials such as BSAS, mullite or rare earth silicate on its surface at high temperatures, and has excellent chemical stability.

[0055] (4) The preparation method described in the present invention uses a customized porous mesh tooling to shield the base material, and can quickly obtain a "lattice structure" with controllable size and spacing. The HfSiO4-Si middle layer uses HfSiO4 powder and Si powder as raw materials, and the HfSiO4 top layer uses HfO2 and SiO2 as raw materials to obtain a HfSiO4-HfO2-Si layer and a HfO2-SiO2 layer. In the subsequent high-temperature heat treatment process, HfO2 and Si in the HfSiO4-HfO2-Si layer react in situ to form a HfSiO4-Si middle layer, and HfO2 and SiO2 in the HfO2-SiO2 layer react in situ to form a HfSiO4 top layer. By adjusting the ratio of HfSiO4 and Si, HfO2 and SiO2 spraying powders, atmospheric plasma spraying process parameters and high-temperature heat treatment system, the precipitation of HfO2 phase with high thermal expansion coefficient and high oxygen permeability in the coating can be avoided.

[0056] In order to further illustrate the present invention, a high temperature resistant, high stability gradient structure environmental barrier coating bonding layer and a preparation method thereof provided by the present invention are described in detail below in combination with embodiments, but they should not be understood as limiting the scope of protection of the present invention.

[0057] The HfSiO4, Si, HfO2, SiO2 and other powders used in the following examples and comparative examples can be obtained from the market. For example, the HfO2, SiO2 and Si powders in this example were purchased from Beijing Jiawa New Material Technology Co., Ltd., and the HfSiO4 powder was commissioned by Changsha College to be prepared by ball milling mixing + high temperature solid phase sintering + spray granulation process, and these powder preparation processes are well known to those skilled in the art.

[0058] Oxidation performance test:

[0059] The oxidation performance assessment method is as follows: statically oxidize the coated samples in an atmospheric environment at 1400°C for 10h, 50h and 100h, respectively, and observe the macroscopic morphology and cross-sectional microscopic morphology of the coating.

[0060] Thermal cycle performance test:

[0061] The thermal cycle performance assessment method is: using a flame thermal cycle tester, the temperature is set to 1400°C, each cycle includes "5 minutes of heating and 2 minutes of cooling", and the coating surface state is observed after every 50 cycles. When the coating peeling area reaches 10% of the total area, it is considered a failure.

[0062] Example 1

[0063] (1) Preparation of SiC f / SiC ceramic composite matrix test piece, size is The samples were ultrasonically cleaned with acetone for 15 min and then dried in an oven at 110 °C for 20 min.

[0064] (2) For SiC f The SiC substrate was sandblasted before spraying, with 220-mesh quartz sand, 0.3 MPa sandblasting pressure and 15 s sandblasting time.

[0065] (3) SiC f The SiC substrate is installed on the automatic working table of the atmospheric plasma spraying equipment and is heated by the plasma flame flow to a surface temperature of 600°C.

[0066] (4) The powder particle size of Si after spray granulation is selected to be 15-60 μm, the powder particle size of HfSiO4 is 15-45 μm, the powder particle size of HfO2 is 15-45 μm, and the powder particle size of SiO2 is 15-60 μm. The powder after granulation is porous spherical powder.

[0067] (5) Si and HfSiO4 powders were mixed in a mass ratio of 1:6, and HfO2 and SiO2 were mixed in a molar ratio of 1:1.3. Si, HfSiO4-Si, and HfO2-SiO2 powders were added to the powder feeder of the atmospheric plasma equipment in sequence.

[0068] (6) Using atmospheric plasma spraying method on SiC f / Prepare the "lattice structure" Si bottom layer on the surface of the SiC substrate, and use a customized porous mesh tooling to cover the substrate material, with a circular hole diameter of 0.3mm and a hole spacing of 0.4mm. Adjust the process parameters as follows: argon flow rate of 45L / min, hydrogen flow rate of 6L / min, spraying distance of 100mm, spraying current of 400A, powder feeding rate of 20%, and obtain a "lattice structure" Si bottom layer with a thickness of 25μm.

[0069] (7) An atmospheric plasma spraying method was used to prepare a HfSiO4-Si intermediate layer on the surface of the "lattice structure" Si bonding layer. The process parameters were adjusted as follows: the argon flow rate was 55 L / min, the hydrogen flow rate was 10 L / min, the spraying distance was 120 mm, the spraying current was 600 A, and the powder feeding rate was 25%. A HfSiO4-Si intermediate layer with a thickness of 40 μm was obtained.

[0070] (8) The HfSiO4 top layer was prepared on the surface of the HfSiO4-Si intermediate layer by atmospheric plasma spraying. The process parameters were adjusted as follows: the flow rate of argon was 50 L / min, the flow rate of hydrogen was 10 L / min, the spraying distance was 130 mm, the spraying current was 500 A, and the powder feeding rate was 25%. The HfSiO4 top layer with a thickness of 30 μm was obtained. Its surface morphology is shown in FIG. Figure 3 shown.

[0071] (9) The deposited coating is heat treated by adjusting the process parameters to: temperature of 1500°C and time of 24 h.

[0072] XRD was used to analyze the physical phase of the coating obtained in Example 1. The results showed that the HfSiO4 phase content in the HfSiO4-Si middle layer was about 82%, and the HfSiO4 phase content in the HfSiO4 top layer was about 95%. HfO2 phase was detected in both layers.

[0073] The microstructure of the coating obtained in Example 1 was detected using a scanning electron microscope. The results showed that the interfaces between the layers of the coating were tightly bonded, no obvious cracks and holes were observed at the interfaces, and the porosity inside the coating was less than 5%.

[0074] Example 2

[0075] A gradient structure bonding layer was prepared according to the method in Example 1, except that:

[0076] In (4), the thickness of the Si bottom layer of the “lattice structure” is 30 μm;

[0077] In (5), the thickness of the HfSiO4-Si intermediate layer is 50 μm;

[0078] In (6), the thickness of the HfSiO4 top layer is 40 μm.

[0079] The anti-oxidation performance test of the gradient structure bonding layer in Example 2 showed that after oxidation at 1400°C for 100 hours, the appearance of the coating did not change significantly compared with before oxidation, and no molten Si seepage was observed, indicating excellent anti-oxidation performance.

[0080] The thermal cycle performance test of the gradient structure bonding layer in Example 2 was carried out, and the results showed that the thermal cycle life of the gradient structure bonding layer in this example exceeded 1000 times.

[0081] Example 3

[0082] A gradient structure bonding layer was prepared according to the method in Example 2, and a Yb2Si2O7 coating with a thickness of 150 μm was prepared on the surface of the bonding layer by using atmospheric plasma spraying technology.

[0083] The anti-oxidation performance of the gradient structure bonding layer in Example 3 was tested. The results showed that after oxidation at 1400°C for 100 hours, the appearance of the coating had no significant change compared to before oxidation, and no c-phase HfO2 was observed at the HfSiO4 / Yb2Si2O7 interface, indicating that the coating has good high-temperature chemical compatibility.

[0084] The thermal cycle performance test of the gradient structure bonding layer in Example 3 was carried out, and the results showed that the thermal cycle life of the gradient structure bonding layer in this example exceeded 1000 times.

[0085] The coating prepared in Example 3 and the bonding strength of the Si / Yb2Si2O7 coating with the same thickness were tested according to GB / T 8642 2002 (three groups of parallel samples were tested), and the results are shown in Table 1. It can be seen that the average bonding strength of the coating prepared in Example 3 is 22.3 MPa, and the bonding strength of the Si / Yb2Si2O7 coating is 24.9 MPa. The bonding strengths of the two are both greater than 20 MPa and differ by only 2.6 MPa, indicating that the gradient structure bonding layer in the present invention has a strong bonding force with the substrate.

[0086] Table 1 Bonding strength of coating of Example 4, Si / Yb2Si2O7 coating and coating of Comparative Example 4

[0087]

[0088]

[0089] Comparative Example 1

[0090] Comparative Example 1 is the same as Example 1 except that:

[0091] In (6), a continuous Si bottom layer with a thickness of 25 μm was prepared on the surface of the CMCs substrate by atmospheric plasma spraying.

[0092] The present invention tests the antioxidant performance of the bonding layer in Comparative Example 1. The results show that after oxidation at 1400°C for 10 hours, obvious bubbling is observed on the coating surface. The Si layer softens and melts at high temperature and seeps out of the surface, resulting in the bonding layer not having antioxidant performance at 1400°C.

[0093] The present invention conducts a thermal cycle performance test on the bonding layer in Comparative Example 1, and the results show that the thermal cycle life of the gradient structure bonding layer in this embodiment is less than 200 times.

[0094] Comparative Example 2

[0095] Comparative Example 2 is the same as Example 1, except that:

[0096] In (5), Si and HfSiO4 powders are mixed in a mass ratio of 1:15, HfO2 and SiO2 are mixed in a molar ratio of 1:1, and Si, HfSiO4-Si, and HfO2-SiO2 powders are sequentially added to the powder feeder of the atmospheric plasma equipment.

[0097] XRD was used to analyze the physical phase of the coating obtained in Comparative Example 2, and the results showed that the HfSiO4 phase content in the HfSiO4-Si intermediate layer was approximately 64%, the HfO2 phase content was 36%, and the HfSiO4 phase content in the HfSiO4 top layer was approximately 73%, and the HfO2 phase content was 27%.

[0098] The microstructure of the coating obtained in Example 1 was detected using a scanning electron microscope. The results showed that a large number of holes existed inside the coating due to the volatilization of SiO2, and the porosity inside the coating was greater than 10%.

[0099] The present invention tested the antioxidant performance of the bonding layer in Comparative Example 2, and the results showed that after oxidation at 1400° C. for 50 hours, obvious cracks appeared on the surface and inside of the coating, resulting in insufficient antioxidant performance of the bonding layer.

[0100] The present invention conducts a thermal cycle performance test on the bonding layer in Comparative Example 2, and the results show that the thermal cycle life of the gradient structure bonding layer in this embodiment is less than 600 times.

[0101] Comparative Example 3

[0102] Comparative Example 3: Based on Comparative Example 2, a Yb2Si2O7 coating with a thickness of 150 μm was prepared on the surface of the bonding layer by using atmospheric plasma spraying technology.

[0103] The present invention tested the antioxidant performance of the bonding layer in Comparative Example 3. The results showed that after oxidation at 1400°C for 50 hours, c-phase HfO2 was observed at the HfSiO4 / Yb2Si2O7 interface inside the coating, and a certain number of cracks were associated with the c-phase HfO2, indicating that the antioxidant performance of the bonding layer was poor.

[0104] The present invention conducts a thermal cycle performance test on the bonding layer in Comparative Example 3. The results show that the thermal cycle life of the gradient structure bonding layer in this embodiment is less than 500 times. The reason for the reduced thermal cycle life is that the fracture toughness of the c-phase HfO2 is low, and the thermal expansion coefficient is significantly higher than that of HfSiO4 and Yb2Si2O7. The accumulation of thermal stress leads to crack initiation and expansion, causing premature failure of the coating.

[0105] Comparative Example 4

[0106] Comparative Example 4 is the same as Example 3, except that:

[0107] Step (6) is omitted, and the HfSiO4-Si intermediate layer, the HfSiO4 top layer and the Yb2Si2O7 environmental barrier layer are directly prepared on the surface of the CMCs substrate.

[0108] The bonding strength of the coating prepared in Comparative Example 4 was tested according to GB / T 8642 2002, and the results are shown in Table 1. It can be seen that the average bonding strength of the coating in Comparative Example 4 is 14.7 MPa, which is 34% lower than that of the coating in Example 4.

[0109] It can be seen from the above embodiments that the present invention provides a high-temperature resistant, highly stable gradient structure environmental barrier coating bonding layer, comprising a Si bottom layer, a HfSiO4-Si middle layer and a HfSiO4 top layer arranged in sequence in a lattice structure. The present invention adopts atmospheric plasma spraying technology to prepare the above bonding layer. The gradient structure bonding layer described in the present invention has the advantages of high temperature resistance, strong bonding, and high-temperature phase stability, and is expected to break through the bottleneck of low temperature bearing capacity and high-temperature chemical instability of the existing environmental barrier coating bonding layer system. Experimental results show that: the bonding layer and SiC f The bonding strength of the SiC / SiC ceramic composite material matrix is ​​>20MPa. After oxidation at 1400℃ for 100h, the coating has no obvious change in appearance compared with before oxidation, and no molten Si seepage is observed, indicating excellent anti-oxidation performance. The thermal cycle life of the bonding layer exceeds 1000 times.

[0110] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A high temperature resistant, high stability gradient structure environmental barrier coating bonding layer, characterized in that: It includes a Si bottom layer, a HfSiO4-Si middle layer and a HfSiO4 top layer which are arranged in sequence.

2. The high temperature resistant, high stability gradient structure environmental barrier coating bonding layer according to claim 1, characterized in that: In the HfSiO4-Si intermediate layer, Si is evenly distributed in HfSiO4 in the form of dots; The mass content of HfSiO4 is between 70% and 90%.

3. The high temperature resistant, high stability gradient structure environmental barrier coating bonding layer according to claim 1, characterized in that: The mass content of HfSiO4 in the HfSiO4 top layer is greater than 90%.

4. The high temperature resistant, high stability gradient structure environmental barrier coating bonding layer according to claim 1, characterized in that: The thickness of the Si bottom layer of the lattice structure is 10 to 40 μm; The thickness of the HfSiO4-Si intermediate layer is 10 to 50 μm; The thickness of the HfSiO4 top layer is 20-50 μm.

5. A method for preparing a high temperature resistant, high stability gradient structure environmental barrier coating bonding layer according to claim 1, comprising the following steps: A) pretreating the ceramic matrix composite material matrix; B) using atmospheric plasma spraying technology to sequentially prepare a Si bottom layer, a HfSiO4-Si middle layer and a HfSiO4 top layer of a lattice structure on the surface of the pretreated ceramic matrix composite material substrate; C) heat treating the coating to obtain a high temperature resistant, highly stable gradient structure environmental barrier coating bonding layer.

6. The preparation method according to claim 5, characterized in that: The matrix material is a ceramic-based composite material; The pretreatment includes cleaning, sandblasting and plasma jet heating of the base material in sequence.

7. The preparation method according to claim 5, characterized in that: In the process of forming the Si bottom layer with a lattice structure by atmospheric plasma spraying, the base material is shielded by a porous mesh tooling, argon and hydrogen are used as plasma, the argon flow rate is 40-60L / min, the hydrogen flow rate is 5-15L / min, the spraying distance is 80-150mm, the spraying current is 300-600A, the powder feeding rate is 10-30%, and the particle size of the Si powder is 15-60μm.

8. The preparation method according to claim 5, characterized in that: In the process of forming the HfSiO4-Si intermediate layer by atmospheric plasma spraying, argon and hydrogen are used as plasma, the flow rate of argon is 40-80L / min, the flow rate of hydrogen is 5-15L / min, the spraying distance is 100-200mm, the spraying current is 500-800A, the powder feeding rate is 10-30%, the particle size of Si powder is 15-60μm, and the particle size of HfSiO4 powder is 15-45μm.

9. The preparation method according to claim 5, characterized in that: In the process of forming the HfSiO4 top layer by atmospheric plasma spraying, HfO2 and SiO2 with a molar ratio of 1: (1.2-1.8) are used as raw materials, argon and hydrogen are used as plasma, the argon flow rate is 40-80 L / min, the hydrogen flow rate is 5-15 L / min, the spraying distance is 100-200 mm, the spraying current is 400-600 A, the powder feeding rate is 10-30%, the particle size of the HfO2 powder is 15-45 μm, and the particle size of the SiO2 powder is 15-60 μm.

10. The preparation method according to claim 5, characterized in that: In the step C), the heat treatment temperature is 1400-1600° C. and the heat treatment time is 10-30 hours.

Citation Information

Patent Citations

  • Functional gradient thermal barrier coating and preparation method thereof

    CN110205626A

  • Hafnium silicate environment barrier coating for ceramic-based composite material matrix and preparation method thereof

    CN111233446A

  • Thermal barrier composite coating with gradient structure and preparation method thereof

    CN116219357A

  • Multiphase embedded gradient color thermal barrier coating, preparation method and preparation system

    CN117127137A

  • High-temperature-corrosion-resistant multi-element complex-phase environmental barrier coating as well as preparation method and application thereof

    CN117902921A

Cited By

  • Multi-gradient thermal environment barrier coating, preparation method thereof and high-temperature-resistant component