Method for synthesizing and polymerizing four-membered ring lactone and recovering polymer of four-membered ring lactone

By preparing four-membered ring lactone monomers based on α-substituted carboxylic acids, α-substituted esters and aldehydes and ketones, and preparing polymers through aldol condensation and condensation reactions, it-P3HB solves the problem of high cost, poor regularity and The problem of difficult recycling has been solved, and the preparation and closed-loop recycling of high-performance polymers have been achieved.

CN118724844AActive Publication Date: 2024-10-01SICHUAN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310313290.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-01
Estimated Expiration
2043-03-28

AI Technical Summary

Technical Problem

In the existing technology, poly-3-hydroxyalkanoate (it-P3HB) prepared by bacterial fermentation has high cost, difficulty in obtaining high isotacticity, poor elongation at break, low melting temperature close to the decomposition temperature, and difficulty in chemical synthesis. The problem of recycling into monomers limits its application.

Method used

The four-membered ring lactone monomer prepared based on α-substituted carboxylic acid, α-substituted ester and aldehydes and ketones is used to prepare the intermediate product β-hydroxy acid through aldol condensation and condensation reaction, and then the four-membered ring is prepared through the condensation reagent The lactone monomer realizes ring-opening polymerization of the polymer, and is hydrolyzed under alkaline conditions to recover β-hydroxy acid, and the ring-closing monomer is obtained again.

Benefits of technology

The prepared polymer has excellent thermal and mechanical properties, with an elongation at break of 559%, a 5% decomposition temperature of 324°C, a melting point of 160-175°C, and a maximum number average molecular weight of 420kg/mol. It can be used in cheap catalysts It polymerizes quickly and can recycle monomers in a closed loop, which solves the problem of difficult recycling of traditional it-P3HB.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004149334650000011
    Figure BDA0004149334650000011
  • Figure BDA0004149334650000021
    Figure BDA0004149334650000021
  • Figure BDA0004149334650000022
    Figure BDA0004149334650000022
Patent Text Reader

Abstract

The invention relates to the technical field of monomer synthesis, polymer synthesis and polymer depolymerization recovery. The invention provides a method for synthesizing the four-membered ring lactone from cheap alpha-substituted acid (ester) and aldehyde ketone compounds, the variety of the four-membered ring lactone is enriched, the synthesized four-membered ring lactone is subjected to ring opening polymerization to prepare a polyhydroxyalkanoate polyester material with excellent performance, the polyester can be degraded and recycled into a four-membered ring lactone monomer through a chemical method, and the polyester material has good application prospects. The problems that in the prior art, polyhydroxyalkanoate is difficult to recycle and degrade, the elongation at break is low, and the processing window is short are effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical fields of polymerization monomer synthesis and polymer synthesis and polymer chemical recovery, and in particular to a method for synthesizing a four-membered ring lactone monomer, a method for ring-opening polymerization of the four-membered ring lactone monomer and a method for degrading the resulting polymer. Background Art

[0002] Since the invention of polymer materials, plastic products have become one of the largest and most widely used man-made materials. A large amount of plastic waste seriously harms our environment. It has become an urgent need to develop an environmentally friendly, degradable and recyclable polymer.

[0003] Polyhydroxyalkanoates (PHAs) prepared by bacterial fermentation are considered to be potential substitutes for general-purpose plastics due to their excellent biocompatibility, biodegradability and good mechanical properties. The most popular among the PHAs is isotactic poly 3-hydroxyalkanoate (it-P3HB), which has performance comparable to that of polypropylene plastic. However, there are still inherent defects that limit the promotion of it-P3HB: (1) the cost of preparing it-P3HB by biological fermentation is high; (2) it-P3HB is prepared by chemical synthesis of β-butyrolactone monomers through ring-opening polymerization, which requires the use of complex and expensive metal complexes and is difficult to obtain it-P3HB with high isotacticity; (3) it-P3HB is hard and brittle, with poor elongation at break (~3%), and commercial it-P3HB cannot be used alone but exists as a component of copolymers; (4) the melting temperature of it-P3HB is close to the decomposition temperature, and the short processing window also limits its application.

[0004] In recent years, the concept of closed-loop recycling has emerged. Polymer scientists are committed to designing a class of polymers that can be completely chemically recycled to monomers, and then the monomers are polymerized to obtain the original polymers. In this way, the properties of the re-prepared polymers will not be lost, and the decomposition products leaking into the environment can also be reduced. However, it-P3HB is difficult to degrade and recycle to monomers because the hydrogen atom at the α-position of the carbonyl group is easy to eliminate. Therefore, it-P3HB is also difficult to hydrolyze to obtain small molecule compounds with a single component. Summary of the invention

[0005] In view of the above-mentioned shortcomings, the purpose of the present invention is to provide a novel method for the synthesis of four-membered ring lactone monomers, the polymerization of four-membered ring lactone monomers and the degradation of polymers. The method broadens the synthesis route of four-membered ring lactone monomers and designs novel four-membered ring lactone monomers. The synthesis method of these monomers is simple, and the polymers obtained by their ring-opening polymerization can be used as substitutes for P3HB. The polymer obtained by the ring-opening polymerization of the four-membered ring lactone designed by the present invention has excellent performance, is strong and tough, has an elongation at break of 559%, a 5% decomposition temperature of 324°C, a polymer melting point of 160-175°C, and a maximum number average molecular weight of 420kg / mol. The obtained polymer can be hydrolyzed under alkaline conditions to obtain a small molecule β-hydroxy acid with uniform composition, and the β-hydroxy acid can be ring-closed to obtain a four-membered ring lactone monomer again.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] The present invention provides a four-membered ring lactone monomer prepared based on α-substituted carboxylic acid, α-substituted ester and aldehyde ketone compound, and its general structural formula is as follows:

[0008]

[0009] Among them, each R 1 , R 2 , R 3 and R 4 R is independently hydrogen, alkyl, cycloalkyl, alkoxy, aryl, halogen, heteroaryl, substituted alkyl, substituted alkoxy, substituted aryl, substituted heteroaryl, or 1 , R 2 , R 3 and R 4 The carbon atom connected thereto and / or the adjacent carbon atom independently form a cycloalkyl group, a heteroaryl group or an aryl group.

[0010] Furthermore, each R 1 , R 2 , R 3 and R 4 are independently hydrogen, C1-C 10 Alkyl, C3~C6 cycloalkyl, C1~C 10 Alkoxy, C6~C 14 Aryl, halogen, 5-6 membered heteroaryl, substituted C1~C 10 Alkyl, substituted C1~C 10 Alkoxy, with one or more R 1a Substituted C6~C 14 Aryl, one or more R 1a Substituted 5-6 membered heteroaryl or R 1 , R 2 , R3 and R 4 The carbon atom connected thereto and / or the adjacent carbon atom independently form a C3-C7 cycloalkyl group, a 5-6 membered heteroaryl group or a phenyl group; R 1a C1~C 10 Alkyl, C1~C 10 Alkoxy or halogen.

[0011] Furthermore, each R 1 , R 2 , R 3 and R 4 are independently hydrogen, fluorine, chlorine, bromine, iodine, methyl, ethyl, tert-butyl, isopropyl, cyclopropyl, cyclobutyl, cyclohexyl, furanyl, pyridyl, biphenyl, 2-phenylbiphenyl, trityl, isopropyl, benzyl, adamantyl, C1-C3 perfluoroalkoxy, C1-C3 perfluoroalkyl, arylmethylene, heteroarylmethylene, arylmethine or heteroarylmethine.

[0012] The second object of the present invention is to provide a method for preparing the above-mentioned four-membered ring lactone monomer, comprising: preparing an intermediate product, β-hydroxy acid, by condensing an α-substituted ester, an α-substituted carboxylic acid and an aldehyde or ketone compound, and then preparing a four-membered ring lactone monomer by a condensation reagent, and separating and purifying the reaction product after the reaction is completed to obtain;

[0013] The reaction structure of the method for preparing the four-membered ring lactone monomer in the present invention is as follows:

[0014]

[0015] Among them, the general structural formula of α-substituted ester and α-substituted acid compounds is as follows:

[0016]

[0017] R 1 , R 2 , and R 5 R is independently hydrogen, alkyl, cycloalkyl, alkoxy, aryl, halogen, heteroaryl, substituted alkyl, substituted alkoxy, substituted aryl, substituted heteroaryl, or 1 , R 2 , and R 5 The carbon atom connected thereto and / or the adjacent carbon atom independently form a cycloalkyl group, a heteroaryl group or an aryl group.

[0018] Furthermore, R 1 , R 2 , and R 5 are independently hydrogen, C1-C 10 Alkyl, C3~C6 cycloalkyl, C1~C 10Alkoxy, C6~C 14 Aryl, halogen, 5-6 membered heteroaryl, substituted C1~C 10 Alkyl, substituted C1~C 10 Alkoxy, with one or more R 1a Substituted C6~C 14 Aryl, one or more R 1a Substituted 5-6 membered heteroaryl or R 1 , R 2 , and R 5 The carbon atom connected thereto and / or the adjacent carbon atom independently form a C3-C7 cycloalkyl group, a 5-6 membered heteroaryl group or a phenyl group; R 1a C1~C 10 Alkyl, C1~C 10 Alkoxy or halogen.

[0019] Furthermore, R 1 , R 2 , and R 5 are independently hydrogen, fluorine, chlorine, bromine, iodine, methyl, ethyl, tert-butyl, isopropyl, cyclopropyl, cyclobutyl, cyclohexyl, furanyl, pyridyl, biphenyl, 2-phenylbiphenyl, trityl, isopropyl, benzyl, adamantyl, C1-C3 perfluoroalkoxy, C1-C3 perfluoroalkyl, arylmethylene, heteroarylmethylene, arylmethine or heteroarylmethine.

[0020] Among them, the general structural formula of aldehyde and ketone compounds is as follows:

[0021]

[0022] R 3 and R 4 R is independently hydrogen, alkyl, cycloalkyl, alkoxy, aryl, halogen, heteroaryl, substituted alkyl, substituted alkoxy, substituted aryl, substituted heteroaryl, or 3 and R 4 The carbon atom connected thereto and / or the adjacent carbon atom independently form a cycloalkyl group, a heteroaryl group or an aryl group.

[0023] Furthermore, R 3 and R 4 are independently hydrogen, C1-C 10 Alkyl, C3~C6 cycloalkyl, C1~C 10 Alkoxy, C6~C 14 Aryl, halogen, 5-6 membered heteroaryl, substituted C1~C 10 Alkyl, substituted C1~C 10 Alkoxy, with one or more R 2a Substituted C6~C 14Aryl, one or more R 1a Substituted 5-6 membered heteroaryl or R 3 and R 4 The carbon atom connected thereto and / or the adjacent carbon atom independently form a C3-C7 cycloalkyl group, a 5-6 membered heteroaryl group or a phenyl group; R 2a C1~C 10 Alkyl, C1~C 10 Alkoxy or halogen.

[0024] Furthermore, R 3 and R 4 are independently hydrogen, fluorine, chlorine, bromine, iodine, methyl, ethyl, tert-butyl, isopropyl, cyclopropyl, cyclobutyl, cyclohexyl, furanyl, pyridyl, biphenyl, 2-phenylbiphenyl, trityl, isopropyl, benzyl, adamantyl, C1-C3 perfluoroalkoxy, C1-C3 perfluoroalkyl, arylmethylene, heteroarylmethylene, arylmethine or heteroarylmethine.

[0025] Furthermore, the specific process of the preparation method of the four-membered ring lactone monomer is:

[0026] At -78°C, under the protection of inert gas, add α-substituted ester or α-substituted acid to tetrahydrofuran or hexane solution containing lithium diisopropylamide (LDA), react at -78°C for 0.5-2h, then add aldehyde ketone compound to the reaction device, continue to react for 0.5-2h, then add strong alkali aqueous solution to the reaction device, continue to react for 8-12h, and after the reaction is completed, separate and purify the reaction product to obtain the intermediate product β-hydroxy acid.

[0027] The β-hydroxy acid is dissolved in a solvent, a condensing agent is added thereto, and the reaction is carried out for 8-12 hours. After the reaction is completed, the reaction product is separated and purified to obtain a four-membered ring lactone monomer;

[0028] Furthermore, the solvent is a conventional organic solvent, such as dichloromethane, tetrahydrofuran, 1,4-dioxane, toluene, N,N-dimethylformamide, acetonitrile, water, ethanol and methanol, preferably dichloromethane.

[0029] Furthermore, the strong base is an inorganic alkali metal hydroxide, such as sodium hydroxide, lithium hydroxide, potassium hydroxide, preferably sodium hydroxide.

[0030] Further, the condensing agent is 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, dicyclohexylcarbodiimide, N,N-diisopropylcarbodiimide, 2-(7-azabenzotriazole)-N,N,N',N'-tetramethyluronium hexafluorophosphate, benzotriazole-N,N,N',N'-tetramethyluronium hexafluorophosphate, propyl phosphoric anhydride, N,N-carbonyldiimidazole, 1-hydroxybenzotriazole, thionyl chloride, benzotriazole-1-yl-oxytripyrrolidinophosphorus hexafluorophosphate, p-toluenesulfonyl chloride, p-toluenesulfonic anhydride, trifluoroacetic anhydride, trifluoromethanesulfonic anhydride, preferably 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 1-hydroxybenzotriazole.

[0031] The third object of the present invention is to provide a polyester prepared from the above-mentioned four-membered ring lactone monomer, and the specific reaction structure formula is as follows:

[0032]

[0033] Among them, each R 1 , R 2 , R 3 and R 4 R is independently hydrogen, alkyl, cycloalkyl, alkoxy, aryl, halogen, heteroaryl, substituted alkyl, substituted alkoxy, substituted aryl, substituted heteroaryl, or 1 , R 2 , R 3 and R 4 The carbon atom connected thereto and / or the adjacent carbon atom independently form a cycloalkyl group, a heteroaryl group or an aryl group.

[0034] Furthermore, each R 1 , R 2 , R 3 and R 4 are independently hydrogen, C1-C 10 Alkyl, C3~C6 cycloalkyl, C1~C 10 Alkoxy, C6~C 14 Aryl, halogen, 5-6 membered heteroaryl, substituted C1~C 10 Alkyl, substituted C1~C 10 Alkoxy, with one or more R 1a Substituted C6~C 14 Aryl, one or more R 1a Substituted 5-6 membered heteroaryl or R 1 , R 2 , R 3 and R 4 The carbon atom connected thereto and / or the adjacent carbon atom independently form a C3-C7 cycloalkyl group, a 5-6 membered heteroaryl group or a phenyl group; R 1aC1~C 10 Alkyl, C1~C 10 Alkoxy or halogen.

[0035] Furthermore, each R 1 , R 2 , R 3 and R 4 are independently hydrogen, fluorine, chlorine, bromine, iodine, methyl, ethyl, tert-butyl, isopropyl, cyclopropyl, cyclobutyl, cyclohexyl, furanyl, pyridyl, biphenyl, 2-phenylbiphenyl, trityl, isopropyl, benzyl, adamantyl, C1-C3 perfluoroalkoxy, C1-C3 perfluoroalkyl, arylmethylene, heteroarylmethylene, arylmethine or heteroarylmethine.

[0036] The present invention also provides a method for preparing the above polymer, comprising the following steps:

[0037]

[0038] Adding a four-membered ring lactone monomer, a catalyst, and an initiator into a reaction device, reacting at 60-200° C. for 10 seconds to 48 hours, and separating and purifying the reaction product to obtain;

[0039] The molar ratio of the four-membered ring lactone monomer, the catalyst and the initiator is 10-50000:0-5:0-5.

[0040] Furthermore, the initiator includes alkyl alcohol, alkyl mercaptan, benzyl alcohol or benzyl mercaptan, etc.

[0041] Furthermore, at temperatures above 60°C, without the addition of initiators or catalysts, the monomers can be polymerized to obtain polyesters.

[0042] Furthermore, the solvent is a conventional organic solvent, such as dichloromethane, dimethyl sulfoxide, tetrahydrofuran, N-methylpyrrolidone, N,N-dimethylformamide and toluene, etc., preferably toluene.

[0043] Furthermore, the monomers can be bulk polymerized to prepare polyesters without adding solvents.

[0044] Further, the catalyst is a conventional organic base and a metal Lewis acid catalyst, such as triethylamine, diisopropylethylamine, 1,5,7-triazidobicyclo(4.4.0)dec-5-ene 1,8-Diazabispiro[5.4.0]undec-7-ene Phosphazene base t BuP4 Stannous acetate, triethylaluminum, aluminum chloride, titanium chloride, zinc chloride and zinc acetate, etc., preferably 1,5,7-triazidobicyclo(4.4.0)dec-5-ene

[0045] In addition, the present invention also provides a method for preparing a monomer by hydrolyzing a polymer into a small molecule β-hydroxycarboxylic acid under strong alkaline conditions and then ring-closing the β-hydroxy acid. The specific reaction structure is shown below:

[0046]

[0047] Under heating conditions, a polymer and a strong base are added to a solvent, and the reaction is refluxed for 8-48 hours. After the reaction is completed, the reaction product is separated and purified to obtain an intermediate product, β-hydroxy acid. β-hydroxy acid is dissolved in a solvent, a condensing agent is added thereto, and the reaction is carried out for 8-12 hours. After the reaction is completed, the reaction product is separated and purified to recover a four-membered ring lactone monomer; the present invention can achieve 90% conversion of the polymer into the corresponding four-membered ring lactone monomer.

[0048] Furthermore, the solvent is a conventional organic solvent, such as dichloromethane, tetrahydrofuran, 1,4-dioxane, toluene, N,N-dimethylformamide, acetonitrile, water, ethanol and methanol, preferably tetrahydrofuran and water.

[0049] Furthermore, the strong base is an inorganic alkali metal hydroxide, such as sodium hydroxide, lithium hydroxide, potassium hydroxide, preferably sodium hydroxide.

[0050] Further, the condensing agent is 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, dicyclohexylcarbodiimide, N,N-diisopropylcarbodiimide, 2-(7-azabenzotriazole)-N,N,N',N'-tetramethyluronium hexafluorophosphate, benzotriazole-N,N,N',N'-tetramethyluronium hexafluorophosphate, propyl phosphoric anhydride, N,N-carbonyldiimidazole, 1-hydroxybenzotriazole, thionyl chloride, benzotriazole-1-yl-oxytripyrrolidinophosphorus hexafluorophosphate, p-toluenesulfonyl chloride, p-toluenesulfonic anhydride, trifluoroacetic anhydride, trifluoromethanesulfonic anhydride, preferably 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 1-hydroxybenzotriazole.

[0051] The polymer obtained by the preparation method of the present invention has excellent thermal and mechanical properties: the elongation at break of the polymer reaches 559%, the 5% decomposition temperature is 360°C, the melting point of the polymer is 160-175°C, and the maximum number average molecular weight can reach 420kg / mol.

[0052] It should be noted that the term "substituted" in the present invention means that the hydrogen atoms and / or carbon atoms in the basic structure have been replaced by hydrocarbon groups and / or functional groups, and / or heteroatoms or groups containing heteroatoms. Therefore, the term hydrocarbon group includes groups containing heteroatoms. For the purpose of this article, heteroatoms are defined as any atom other than carbon and hydrogen. For example, methylcyclopentadiene (Cp) is a Cp group (which is the basic structure) substituted with a methyl group, which can also be called a methyl functional group, ethanol is an ethyl group (which is the basic structure) substituted with an -OH functional group, and pyridine is a phenyl group in which the carbon in the basic structure of the benzene ring is replaced with a nitrogen atom.

[0053] It is to be understood that for the purposes of this article, when a group is listed, it represents the basic structure (group type) of the group and all other groups formed when the group is substituted as described above. The alkyl groups listed, etc. include all isomers, including cyclic isomers as required, for example, butyl includes n-butyl, 2-methylpropyl, 1-methylpropyl, tert-butyl and cyclobutyl (and analogous substituted cyclopropyl); pentyl includes n-pentyl, cyclopentyl, 1-methylbutyl, 2-methylbutyl, 3-methylbutyl, 1-ethylpropyl and neopentyl (and analogous substituted cyclobutyl and cyclopropyl). Cyclic compounds with substitutions include all isomeric forms, for example, methylphenyl will include o-methylphenyl, m-methylphenyl and p-methylphenyl; dimethylphenyl will include 2,3-dimethylphenyl, 2,4-dimethylphenyl, 2,5-dimethylphenyl, 2,6-diphenylmethyl, 3,4-dimethylphenyl and 3,5-dimethylphenyl.

[0054] In summary, the present invention has the following advantages:

[0055] The present invention proposes a method for preparing strained four-membered ring lactone based on cheap and diverse α-substituted esters, α-substituted carboxylic acids and aldehyde and ketone compounds. The preparation method is simple and easy to operate, and enriches the structural types of four-membered ring lactones. The yield of strained ring lactone monomers can be greatly improved by adjusting the substituents, and different substituents can also adjust the properties of the polymer;

[0056] The four-membered ring lactone prepared by the present invention can be rapidly polymerized in the presence of a cheap catalyst, the catalyst loading rate is high, the molar ratio of the monomer to the catalyst is greater than 50000:1, the molecular weight of the prepared polymer is 10-420kg / mol, and the dispersion coefficient is

[0057] The P3HB-like polymer prepared by the present invention has superior performance, and all indicators are better than it-P3HB polymers produced by biological fermentation or chemical synthesis. The elongation at break of it-P3HB is 3-5%, the decomposition temperature is 275°C, and the tensile strength is about 32MPa. The polymer prepared by the present invention has an elongation at break of up to 559%, a decomposition temperature of 324°C, a tensile strength of 36MPa, and a yield strength of 39MPa, which is comparable to commercial polypropylene materials.

[0058] In addition, the polymer developed by the present invention can be converted back to β-hydroxy acid small molecules in equivalent yield, and then the ring is closed to prepare a four-membered ring lactone monomer, thereby realizing closed-loop recycling of the polymer, solving the problem that traditional P3HB polymers are difficult to recycle to monomers. BRIEF DESCRIPTION OF THE DRAWINGS

[0059] Figure 1 The four-membered ring lactone monomer BL-Me2 prepared in the present invention H NMR spectrum of

[0060] Figure 2 The four-membered ring lactone monomer BL-Me2 prepared in the present invention NMR carbon spectrum;

[0061] Figure 3 The polyester P(BL-Me2) prepared in the present invention H NMR spectrum of

[0062] Figure 4 The polyester P(BL-Me2) prepared in the present invention 's NMR carbon spectrum;

[0063] Figure 5 The thermogravimetric analysis (TGA) spectrum of the polyester P(BL-Me2) prepared in the present invention;

[0064] Figure 6 The differential scanning calorimetry (DSC) spectrum of the polyester P(BL-Me2) prepared in the present invention;

[0065] Figure 7 The size exclusion chromatography (SEC) spectrum of the polyester P(BL-Me2) prepared in the present invention;

[0066] Figure 8 The matrix-assisted laser desorption / ionization-time of flight mass spectrometry (MALDI-TOF MS) spectrum of the cyclic polyester P(BL-Me2) prepared in the present invention;

[0067] Fig. 9 The stress-strain curve of the polyester P(BL-Me2) prepared in the present invention is repeated five times continuously;

[0068] Fig.10It is a comparison chart of the H NMR spectrum of the four-membered ring lactone BL-Me2 prepared in Example 1 of the present invention, the C NMR spectrum of the polyester P(BL-Me2) prepared in Example 2, the H NMR spectrum of the β-hydroxy acid prepared by hydrolysis of the polyester in Example 3, and the H NMR spectrum of the four-membered ring lactone prepared by ring-closing the β-hydroxy acid in Example 4;

[0069] Fig.11 The four-membered ring lactone monomer prepared in the present invention n Bu-Me2 H NMR spectrum;

[0070] Fig.12 is the H NMR spectrum of the mixture obtained by hydrolysis of the commercially available P3HB polymer in the present invention; DETAILED DESCRIPTION

[0071] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all of the embodiments.

[0072] Therefore, the following detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present invention.

[0073] Example 1

[0074] This example provides a method for preparing a four-membered ring lactone monomer BL-Me2, and the reaction route is as follows:

[0075]

[0076] The specific reaction steps in the above preparation route are as follows:

[0077] 1. Synthesis of Compound A

[0078] At -78 ° C, under the protection of inert gas, 300 mL of ethyl isobutyrate (227 mmol) in tetrahydrofuran was added dropwise to a solution of lithium diisopropylamide in tetrahydrofuran (1.1 equivalents, 250 mmol, 2M). After the addition was complete, the reaction was continued at -78 ° C for one hour. A solution of acetaldehyde in THF (5M, 250 mmol, 50 mL) was slowly added to the reaction system and reacted at room temperature for another 30 minutes. Then 500 mL of 1 mol / L sodium hydroxide aqueous solution was added thereto and reacted at room temperature overnight. The aqueous phase was separated and collected, and the aqueous phase was washed twice with 100 mL of ether, and the aqueous phase was acidified to pH = 2-5 with aqueous hydrochloric acid, and the aqueous phase was extracted with ethyl acetate five times, using 200 mL of ethyl acetate each time. The combined organic phase was dried over anhydrous sodium sulfate, and the solvent was removed under vacuum to obtain pure compound A (24.7 g, 82% yield).

[0079] 2. Synthesis of compound BL-Me2

[0080] At 0°C, triethylamine (1.5 equivalents, 281 mmol), 1-hydroxybenzotriazole (1.1 equivalents, 206 mmol) and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (1.1 equivalents, 206 mmol) were added to 1000 mL of a dichloromethane solution of compound A (24.7 g, 187 mmol) in sequence, and the mixture was reacted at room temperature for 8-12 hours. The organic phase was washed with 300 mL of water and 300 mL of saturated brine in sequence. The organic phase was dried over anhydrous sodium sulfate, and the solvent was removed under vacuum to obtain a transparent liquid, pure four-membered ring lactone monomer BL-Me2 (18.1 g, 85% yield), NMR spectrum, Figure 1 and Figure 2 .

[0081] Using Example 1 as a template, we synthesized other monomers and β-hydroxycarboxylic acids. The prepared monomers and β-hydroxy acids are partially characterized as follows:

[0082] 1 H NMR (400MHz, CDCl3) δ4.43 (q, J = 6.4Hz, 1H), 1.44 (d, J = 6.4Hz, 3H), 1.41 (s, 3H), 1.24 (s, 3H).

[0083] 1H NMR (400MHz, CDCl3) δ4.22(dd,J=8.7,5.1Hz,1H),1.82–1.55(m,2H),1.55–1.31(m,7H),1.49–1.28(m,3H),1.26(s,3H),0.93(t,J=7.0Hz,3H).

[0084] 1 H NMR (400MHz, CDCl3) δ3.94 (q, J = 6.5Hz, 1H), 1.21 (s, 3H), 1.19 (s, 3H), 1.19 (d, J = 8Hz, 3H).

[0085] 1 H NMR (400MHz, CDCl3) δ3.60 (s, 2H), 1.24 (s, 6H).

[0086] 1 H NMR (400MHz, CDCl3) δ3.68(s,2H),2.01(m,2H),1.65–1.27(m,8H).

[0087] 1 H NMR (400MHz, CDCl3) δ4.19 (q, J = 7.1Hz, 2H), 1.23 (s, 6H), 1.19 (s, 6H).

[0088] Example 2

[0089] This example provides a method for preparing polyester P(BL-Me2) by bulk polymerization of a four-membered ring lactone monomer BL-Me2, and the reaction route is as follows:

[0090]

[0091] The catalyst is 1,5,7-triazidebicyclo(4.4.0)dec-5-ene (TBD) The initiator is Ph2CHCH2OH;

[0092] The specific preparation steps of the above reaction route are:

[0093] Ph2CHCH2OH (0.51 mg, 0.0026 mmol) and TBD (0.37 mg, 0.0026 mmol) were added to a 20 mL glass reaction bottle with a tetrafluoroethylene lined lid, and then the monomer BL-Me2 (3 g, 26 mmol) was added to the reaction device, heated to 100 ° C, and bulk polymerized for 30 hours. At this time, the molar ratio of monomer, catalyst, and initiator was 10000:1:1. 5 mL of chloroform solution with a mass concentration of 10 mg / mL benzoic acid was added to dissolve the product, and 20 μL of the solution was taken for 1 H NMR analysis was used to determine the conversion rate. The remaining reaction solution was poured into 300 mL of methanol to precipitate the polymer. The precipitated solid was filtered, washed with methanol three times, and dried in a vacuum oven at 60 °C for 12 h to obtain a white polymer P(BL-Me2). Figure 3 .

[0094] In this example, the obtained product P(BL-Me2) was tested by nuclear magnetic resonance (NMR), and the results showed that the conversion rate of the monomer was 85%. 13 C NMR ( Figure 4 ), the analysis showed that the polymer was a random polymer. Thermogravimetric analysis (TGA) results showed that ( Figure 5 ), the thermal decomposition temperature of the polymer is 324°C. Differential scanning calorimetry (DSC) was used to detect the melting temperature and glass transition of P(BL-Me2). The results showed that ( Figure 6 ), the melting temperature of P(BL-Me2) prepared in this example is 175°C; the molecular weight of the polymer was determined by size exclusion chromatography (SEC), and the results showed that ( Figure 7 ), the polymer molecular weight is 420 kg / mol, and the dispersion coefficient The stress-strain curve of the tested polymer ( Fig. 9 ), the elongation at break of the polymer prepared in this embodiment can reach 559%, the tensile strength is 36MPa, the yield strength is 39MPa, and the Young's modulus is 2.2GPa. Thermogravimetric analysis of the polymer shows that the 5% decomposition temperature of P(BL-Me2) prepared in this embodiment is 324°C, and the maximum decomposition temperature is 360°C.

[0095] Example 3

[0096] This example provides a method for hydrolyzing polyester back to small molecule β-hydroxy acid A, and the reaction route is as follows:

[0097]

[0098] The specific preparation steps of the above reaction route are:

[0099] 25 mL of tetrahydrofuran solution of P(BL-Me2) (polymer P(BL-Me2) prepared in Example 2, 5 mmol, 571 mg), 25 mL of sodium hydroxide aqueous solution (2 mol / L) and 0.5 mL of methanol were added to a 75 mL sealed tube, heated to 100 °C, and the mixture was sealed and stirred for 48 hours. Cooled to room temperature, the reaction solution was diluted with 50 mL of saturated sodium chloride aqueous solution and washed with 20 mL of ether. The collected aqueous phase was acidified to pH 2-5, and the aqueous phase was extracted 5 times with 50 mL of ethyl acetate. The combined organic phase was dried over anhydrous sodium sulfate, and the solvent was removed in vacuo to obtain pure compound A (100% yield).

[0100] Example 4

[0101] This example provides a method for synthesizing a four-membered ring lactone monomer BL-Me2 using A prepared in Example 3 as a raw material, and the reaction scheme is as follows:

[0102]

[0103] The specific preparation steps of the above reaction route are:

[0104] At 0°C, triethylamine (1.5 equivalents, 7.5 mmol), 1-hydroxybenzotriazole (1.1 equivalents, 5.5 mmol) and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (1.1 equivalents, 5.5 mmol) were added to a dichloromethane solution of 25 mL of compound A (Compound A prepared in Example 3, 661 mg, 5 mmol) in sequence, and the mixture was reacted at room temperature for 8-12 hours. The organic phase was washed with 20 mL of water and 20 mL of saturated brine in sequence. The organic phase was dried over anhydrous sodium sulfate, and the solvent was removed under vacuum to obtain a transparent liquid, pure four-membered ring lactone monomer BL-Me2 ( Fig.10 , 514 mg, 90% yield).

[0105] Example 5

[0106] This example provides a four-membered ring lactone monomer n Preparation of polyester P( n The reaction scheme is as follows:

[0107]

[0108] The catalyst is 1,5,7-triazidobicyclo(4.4.0)dec-5-ene (TBD), and the initiator is Ph2CHCH2OH; the specific preparation steps of the above reaction route are:

[0109] Ph2CHCH2OH (1 mg, 0.005 mmol) and TBD (0.7 mg, 0.005 mmol) were added to a 4 mL glass reaction bottle with a tetrafluoroethylene lined lid, and the monomers were added to the reaction apparatus. n Bu-Me2 (156 mg, 1 mmol) was heated to 100°C and bulk polymerized for 40 minutes. At this time, the molar ratio of monomer, catalyst, and initiator was 200:1:1. 1 mL of 10 mg / mL benzoic acid chloroform solution was added to dissolve the product, and 20 μL of the solution was taken for 1 H NMR analysis was used to determine the conversion rate. The remaining reaction solution was poured into 50 mL of methanol to precipitate the polymer. The precipitated solid was filtered, washed with methanol three times, and dried in a vacuum drying oven at 60 ° C for 12 h to obtain a white polymer P( n Bu-Me2).

[0110] In this example, the obtained product P( n The results of nuclear magnetic resonance (NMR) detection of Bu-Me2 showed that the conversion rate of the monomer was 83%;

[0111] Example 6

[0112] This example provides a method for preparing polyester P(BL-Me2) by solution polymerization of a four-membered ring lactone monomer BL-Me2 catalyzed by TBD, and the reaction route is as follows:

[0113]

[0114] The catalyst is 1,5,7-triazidobicyclo(4.4.0)dec-5-ene (TBD), and the initiator is Ph2CHCH2OH; the specific preparation steps of the above reaction route are:

[0115] Ph2CHCH2OH (1 mg, 0.005 mmol) and TBD (0.7 mg, 0.005 mmol) were added to a 4 mL glass reaction bottle with a tetrafluoroethylene lined lid, and then the monomer BL-Me2 (114 mg, 1 mmol) and 385 μL of toluene were added to the reaction device, heated to 100 °C, and sealed for reaction for 5 hours. At this time, the molar ratio of monomer, catalyst, and initiator was 200:1:1. 1 mL of chloroform solution with a mass concentration of 10 mg / mL benzoic acid was added to dissolve the product, and 20 μL of the solution was taken for 1 The conversion rate was determined by H NMR analysis. The remaining reaction solution was poured into 50 mL of methanol to precipitate the polymer. The precipitated solid was filtered, washed three times with methanol, and then dried in a vacuum drying oven at 60 °C for 12 h to obtain a white polymer P(BL-Me2).

[0116] In this example, the obtained product P(BL-Me2) was subjected to nuclear magnetic resonance (NMR) detection, and the results showed that the monomer conversion rate was 87%; the obtained product P(BL-Me2) was monitored by size exclusion chromatography (SEC), and the results showed that the number average molecular weight of the polymer obtained in this embodiment was 62.6 kg / mol, and the polydispersity coefficient

[0117] Example 7

[0118] This example provides t The method for preparing polyester P(BL-Me2) by solution polymerization of four-membered ring lactone monomer BL-Me2 catalyzed by BuP4, the reaction route of which is as follows:

[0119]

[0120] The catalyst is a phosphazene base t BuP4 The initiator is Ph2CHCH2OH; the specific preparation steps of the above reaction route are:

[0121] Ph2CHCH2OH (1 mg, 0.005 mmol) and t BuP4 (3.2 mg, 0.005 mmol) was added to a 4 mL glass reaction bottle with a tetrafluoroethylene lined lid, and then the monomer BL-Me2 (114 mg, 1 mmol) and 385 μL of toluene were added to the reaction device, heated to 100 ° C, and sealed for 5 hours. At this time, the molar ratio of monomer, catalyst, and initiator was 200:1:1. 1 mL of chloroform solution with a mass concentration of 10 mg / mL benzoic acid was added to dissolve the product, and 20 μL of the solution was taken for 1 The conversion rate was determined by H NMR analysis. The remaining reaction solution was poured into 50 mL of methanol to precipitate the polymer. The precipitated solid was filtered, washed three times with methanol, and then dried in a vacuum drying oven at 60 °C for 12 h to obtain a white polymer P(BL-Me2).

[0122] In this example, the obtained product P(BL-Me2) was subjected to nuclear magnetic resonance (NMR) detection ( Fig.11 ), the results showed that the conversion rate of the monomer was 100%, of which the polymerization yield was 73% and the oligomer yield was 27%; the obtained product P(BL-Me2) was monitored by size exclusion chromatography (SEC), and the results showed that the number average molecular weight of the polymer obtained in this embodiment was 13.5 kg / mol, and the polydispersity coefficient

[0123] Comparative Example 1

[0124] This example provides a method for hydrolyzing a commercially available it-P3HB polymer into a small molecule compound, which is similar to the method in Example 3, except that the polymer to be hydrolyzed is replaced by commercially available P3HB instead of P(BL-Me2). The reaction scheme is as follows:

[0125]

[0126] In this example, the mixture obtained by hydrolysis was subjected to nuclear magnetic resonance (NMR) detection ( Fig.12 ), the results showed that the mixture contained 36% of β-hydroxy acid 3-BA, 18% of crotonic acid 3-CA and 27% of 3-MBA. This is because the hydrogen atom at the α position of the P3HB carbon group is easily eliminated under alkaline conditions.

[0127] The above contents are merely examples and explanations of the structure of the present invention. Any modification or supplement made to the described specific embodiments or replacement by similar methods by technicians in the relevant field without creative work still falls within the scope of protection of this patent.

Claims

1. A four-membered ring lactone monomer synthesized based on α-substituted carboxylic acid, α-substituted ester and aldehyde ketone compound, characterized in that: The general structural formula is shown below: Among them, each R 1 , R 2 , R 3 and R 4 R is independently hydrogen, alkyl, cycloalkyl, alkoxy, aryl, halogen, heteroaryl, substituted alkyl, substituted alkoxy, substituted aryl, substituted heteroaryl, or 1 , R 2 , R 3 and R 4 The carbon atom connected thereto and / or the adjacent carbon atom independently form a cycloalkyl group, a heteroaryl group or an aryl group.

2. The four-membered ring lactone monomer according to claim 1, characterized in that Each R 1 , R 2 , R 3 and R 4 are independently hydrogen, C1-C 10 Alkyl, C3~C6 cycloalkyl, C1~C 10 Alkoxy, C6~C 14 Aryl, halogen, 5-6 membered heteroaryl, substituted C1~C 10 Alkyl, substituted C1~C 10 Alkoxy, with one or more R 1a Substituted C6~C 14 Aryl, one or more R 1a Substituted 5-6 membered heteroaryl or R 1 , R 2 , R 3 and R 4 The carbon atom connected thereto and / or the adjacent carbon atom independently form a C3-C7 cycloalkyl group, a 5-6 membered heteroaryl group or a phenyl group; R 1a C1~C 10 Alkyl, C1~C 10 Alkoxy or halogen.

3. The four-membered ring lactone monomer according to claim 2, characterized in that Each R 1 , R 2 , R 3 and R 4 are independently hydrogen, fluorine, chlorine, bromine, iodine, methyl, ethyl, tert-butyl, isopropyl, cyclopropyl, cyclobutyl, cyclohexyl, furanyl, pyridyl, biphenyl, 2-phenylbiphenyl, trityl, isopropyl, benzyl, adamantyl, C1-C3 perfluoroalkoxy, C1-C3 perfluoroalkyl, arylmethylene, heteroarylmethylene, arylmethine or heteroarylmethine.

4. The method for preparing a four-membered ring lactone monomer according to any one of claims 1 to 3, characterized in that: The following steps are involved: At -78°C, under the protection of inert gas, an α-substituted ester or α-substituted acid is added to a tetrahydrofuran or hexane solution containing lithium diisopropylamide (LDA), and after reacting at -78°C for 0.5-2h, an aldehyde or ketone compound is added to the reaction device, and after continuing the reaction for 0.5-2h, a strong base solution is added to the reaction device, and the reaction is continued for 8-12h. After the reaction is completed, the reaction product is separated and purified to obtain a compound β-hydroxy acid; the β-hydroxy acid is dissolved in a solvent, a condensing agent is added thereto, and the reaction is carried out for 8-12h. After the reaction is completed, the reaction product is separated and purified to obtain a four-membered ring lactone monomer; The solvent is a conventional organic solvent, such as dichloromethane, tetrahydrofuran, 1,4-dioxane, toluene, N,N-dimethylformamide, acetonitrile, water, ethanol and methanol; the strong base is an inorganic alkali metal hydroxide, such as sodium hydroxide, lithium hydroxide, potassium hydroxide, preferably sodium hydroxide; the condensing agent is 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, dicyclohexylcarbodiimide, N,N-diisopropylcarbodiimide, 2-(7-azabenzotriazine) The invention relates to benzotriazole-N,N,N',N'-tetramethyluronium hexafluorophosphate, benzotriazole-N,N,N',N'-tetramethyluronium hexafluorophosphate, propyl phosphoric anhydride, N,N-carbonyldiimidazole, 1-hydroxybenzotriazole, thionyl chloride, benzotriazol-1-yl-oxytripyrrolidinophosphorus hexafluorophosphate, p-toluenesulfonyl chloride, p-toluenesulfonic anhydride, trifluoroacetic anhydride, trifluoromethanesulfonic anhydride, preferably 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 1-hydroxybenzotriazole.

5. A polyester prepared by ring-opening polymerization of the four-membered ring lactone monomers of claims 1 to 4, characterized in that: The general structural formula is shown below: Among them, each R 1 , R 2 , R 3 and R 4 R is independently hydrogen, alkyl, cycloalkyl, alkoxy, aryl, halogen, heteroaryl, substituted alkyl, substituted alkoxy, substituted aryl, substituted heteroaryl, or 1 , R 2 , R 3 and R 4 The carbon atom connected thereto and / or the adjacent carbon atom independently form a cycloalkyl group, a heteroaryl group or an aryl group.

6. A method for preparing the polyester according to claim 5, characterized in that: The following steps are involved: The four-membered ring lactone monomer, catalyst and initiator are added into a reaction device, and a solvent or no solvent is added, and the reaction is carried out at 60-200° C. for 10 s to 48 h, and the reaction product is separated and purified to obtain; The molar ratio of the four-membered ring lactone monomer, the catalyst and the initiator is 10-50000:0-5:0-5; The initiator includes alkyl alcohol, alkyl mercaptan, benzyl alcohol or benzyl mercaptan, etc.; the solvent is a conventional organic solvent, such as dichloromethane, dimethyl sulfoxide, tetrahydrofuran, N-methylpyrrolidone, N,N-dimethylformamide and toluene, etc., preferably toluene; the catalyst is a conventional organic base and a metal Lewis acid catalyst, such as triethylamine, diisopropylethylamine, 1,5,7-triazidobicyclo (4.4.0) dec-5-ene, 1,8-diazobispiro [5.4.0] undec-7-ene, phosphazene base t BuP4, stannous acetate, triethylaluminum, aluminum chloride, titanium chloride, zinc chloride and zinc acetate, etc., preferably 1,5,7-triazidobicyclo(4.4.0)dec-5-ene.

7. A method for hydrolyzing the polyester described in claims 4-5 into small molecular carboxylic acids and then ring-closing to recover four-membered ring lactone monomers, characterized in that: The following steps are involved: Under heating conditions, a polymer and a strong base are added to a solvent, and the reaction is refluxed for 8-48 hours. After the reaction is completed, the reaction product is separated and purified to obtain an intermediate product, β-hydroxy acid, the β-hydroxy acid is dissolved in a solvent, a condensation agent is added thereto, and the reaction is carried out for 8-12 hours. After the reaction is completed, the reaction product is separated and purified to recover a four-membered ring lactone monomer; The solvent is a conventional organic solvent, such as dichloromethane, tetrahydrofuran, 1,4-dioxane, toluene, N,N-dimethylformamide, acetonitrile, water, ethanol and methanol; the strong base is an inorganic alkali metal hydroxide, such as sodium hydroxide, lithium hydroxide, potassium hydroxide, preferably sodium hydroxide; the condensing agent is 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, dicyclohexylcarbodiimide, N,N-diisopropylcarbodiimide, 2-(7-azabenzotriazine) The invention relates to benzotriazole-N,N,N',N'-tetramethyluronium hexafluorophosphate, benzotriazole-N,N,N',N'-tetramethyluronium hexafluorophosphate, propyl phosphoric anhydride, N,N-carbonyldiimidazole, 1-hydroxybenzotriazole, thionyl chloride, benzotriazol-1-yl-oxytripyrrolidinophosphorus hexafluorophosphate, p-toluenesulfonyl chloride, p-toluenesulfonic anhydride, trifluoroacetic anhydride, trifluoromethanesulfonic anhydride, preferably 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 1-hydroxybenzotriazole.

Citation Information

Patent Citations

  • Recyclable polymer based on six-membered ring lactone and preparation method

    CN112961330A

  • Recyclable polymers based on ring-fused gamma-butyrolactones

    US20190040191A1