Full perylene-based PDI receptor for non-fullerene organic solar cell and synthesis method of full perylene-based PDI receptor
By designing the A-D-A type receptor NP-FPDI, using N-cyclized perylene and fused perylene diimide structures, we solved the problems of poor energy level tunability and self-aggregation of fullerene receptors, and improved the performance of organic solar cells. Charge carrier mobility and photovoltaic efficiency.
Patent Information
- Application Number
- CN202410814704.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-01
AI Technical Summary
Existing fullerene receptors in organic solar cells have problems such as poor energy level tunability, low visible light absorption, high synthesis and purification costs, and unstable morphology. The photovoltaic efficiency of perylene diimide derivatives lags behind, mainly due to The strong self-aggregation of PDI monomer leads to micron-scale phase separation in the blend film.
N-cyclized perylene (NP) was used as the central donor core to synthesize non-fullerene acceptors, and an A-D-A type acceptor (NP-FPDI) was designed by connecting two electron-deficient fused perylene diimides (FPDI). To enhance π-conjugation and intermolecular π-π interactions, and reduce excessive aggregation between molecules.
By designing NP-FPDI acceptors, the ordered stacking of molecules and charge carrier mobility are enhanced, the photovoltaic performance of organic solar cells is improved, and higher charge carrier mobility and photovoltaic efficiency are achieved.
Smart Images

Figure CN118724926A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of non-fullerene receptors, and in particular to a perylene-based PDI receptor for non-fullerene organic solar cells and a synthesis method thereof. Background Art
[0002] Bulk heterojunction (BHJ) organic solar cells (OSCs) have made remarkable progress due to their inherent advantages of low cost, light weight and flexibility. In the past decade, fullerene derivatives have been used as classical electron acceptors in organic solar cells due to their large electron affinity, isotropy of charge transfer and high electron mobility. The power conversion efficiency (PCE) of fullerene derivative-based organic solar cells has reached 11%. Although fullerenes and their derivatives have many advantages, they have some intrinsic defects that limit their wide application in the field of electronics, such as poor energy level tunability, low visible light absorption, high synthesis and purification costs, and unstable morphology. Nowadays, non-fullerene acceptors have broken the dominance of fullerene-based acceptors in the field of OPVs. Among various non-fullerene acceptors, perylene diimide (PDI) is a pioneer in the development of n-type electron acceptors and a widely used electron accepting unit because of their good absorption, high electron mobility, low energy level, and chemical and environmental stability. However, the photovoltaic efficiency of perylene diimide derivatives lags behind other non-fullerene acceptors, with the main drawback being the strong tendency of PDI monomers to self-aggregate, which leads to micrometer-scale phase separation in the blend films. To address this issue, a simple strategy is to directly connect the PDI units at the bay position with spacers (benzene, thiophene, benzodithiophene, porphyrin, etc.) via single bonds to synthesize distorted conformations of dimers, trimers, or tetramers. Therefore, the distorted geometry of the PDI acceptor can reduce the strong intermolecular aggregation and thus reduce the domain size when blended with polymer donors. On the one hand, this approach seems to help reduce excessive aggregation, but on the other hand, it may cause severe distortion of the PDI acceptor, resulting in excessive reduction of π-π stacking, which in turn leads to poor photovoltaic performance of organic solar cells. Summary of the invention
[0003] The technical problem to be solved by the present invention is: to overcome the shortcomings of the prior art, to provide a perylene-based PDI receptor for non-fullerene organic solar cells and a synthesis method thereof, to use N-cyclized perylene (NP) as a central donor nucleus to synthesize the non-fullerene receptor, and to design an ADA-type receptor (NP-FPDI) by connecting two electron-deficient fused perylene diimides (FPDI), which not only helps to enhance π-conjugation, but also enhances intermolecular π-π interactions and orderly stacking of molecules, thereby leading to higher charge carrier mobility.
[0004] The technical solution of the present invention is:
[0005] On the one hand, the present invention provides a method for synthesizing a perylene-based PDI receptor for a non-fullerene organic solar cell, wherein compound 1, compound 2 and K2PO3 are dissolved in a mixed solvent of tetrahydrofuran and H2O, Pd(dppf)Cl2 is added in a nitrogen atmosphere, and then refluxed to obtain a compound NP-FPDI; after cooling to room temperature, the solvent is removed under reduced pressure, and the residue is purified by silica gel column chromatography and eluted with petroleum ether and CH2Cl2 to obtain a dark red solid NP-FPDI, which is a perylene-based PDI receptor; wherein the structural formula of compound 1 is as follows:
[0006]
[0007] The structural formula of compound 2 is shown below:
[0008]
[0009] Wherein, R is a C5 or C6 alkyl group.
[0010] Preferably, the molar ratio of compound 1, compound 2, K3PO4 and Pd(dppf)Cl2 is 1:2-3:2-10:0.1-0.2.
[0011] Preferably, the molar volume ratio of compound 1 to the mixed solvent is 1 mmol:300-450 mL.
[0012] Preferably, the volume ratio of tetrahydrofuran to H2O in the mixed solvent is 6-10:1.
[0013] Preferably, reflux for 48-72 hours.
[0014] Preferably, the volume ratio of petroleum ether to CH2Cl2 is 1:1-3.
[0015] On the other hand, the present invention provides a perylene-based PDI acceptor for non-fullerene organic solar cells prepared by the above synthesis method.
[0016] The present invention provides a novel synthesis method of a perylene diimide receptor NP-FPDI, using an NP unit as a central core and surrounded by two electron-deficient fused PDI units to form an acceptor-donor-acceptor (ADA) type receptor. R is an alkyl chain located at the position of the perylene diimide group, which can solve the aggregation problem without disturbing the molecular planarity. The longer the carbon chain of the substituent R, the better the solubility of the PDI tetramer in o-dichlorobenzene, chloroform and other solvents. In solar cells, the fused perylene diimide molecules need to have appropriate solubility and cannot be too large or too small, so C5-C6 alkyl chains are an ideal choice. NP-FPDI has a central biaxial rigid skeleton with a flat NP donor core and connects two twisted fused FPDI units. An N-cyclized perylene (NP) central unit and two fused PDI units are connected by a single bond, which makes the structure more twisted between the central core and the FPDI unit, while the FPDI unit formed by the fusion of two PDI subunits through a naphthalene ring tends to be less twisted (as shown below).
[0017]
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The present invention uses N-cyclized perylene (NP) as a central donor core to synthesize a non-fullerene acceptor, and designs an ADA type acceptor (NP-FPDI) by connecting two electron-deficient fused perylene diimide (FPDI). Due to the dihedral angle between the flat N-cyclized perylene core and the terminal fused PDI unit, the acceptor exhibits a highly distorted conformation between the central donor core unit and the two fused PDI units, which helps to inhibit excessive aggregation during the formation of the blended film. A rigid NP core with FPDI units is used to produce an ADA type acceptor, wherein the NP core (FPDI) with fused PDI is due to the interaction between the NP core and the fused FPDI, σ bonding unlocks the geometric structure, and a locked conformation is caused by the quasi-two-dimensional fused FPDI, which not only helps to enhance π-conjugation, but also enhances the intermolecular π-π interaction and the ordered stacking of molecules, thereby leading to higher charge carrier mobility. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is the hydrogen spectrum of the NP-FPDI receptor prepared in Example 1 of the present invention.
[0021] Figure 2 It is the carbon spectrum of the NP-FPDI receptor prepared in Example 1 of the present invention.
[0022] Figure 3It is the UV-visible light absorption spectra of the PBDB-T donor polymer and the NP-FPDI acceptor prepared in Example 1 of the present invention in the film.
[0023] Figure 4 This is a thermogravimetric analysis diagram of the NP-FPDI receptor prepared in Example 1 of the present invention.
[0024] Figure 5 It is a cyclic voltammetry curve of the NP-FPDI receptor prepared in Example 1 of the present invention.
[0025] Figure 6 Schematic diagram of the energy levels of the NP-FPDI receptor prepared in Example 1 of the present invention.
[0026] Figure 7 4 is a current density and voltage (JV) curve of the PBDB-T:NP-FPDI organic solar cell of Example 1 of the present invention.
[0027] Figure 8 4 is an EQE curve diagram of the PBDB-T:NP-FPDI organic solar cell according to Example 1 of the present invention. DETAILED DESCRIPTION
[0028] In order to enable persons skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention.
[0029] Example 1
[0030] The synthesis method of the perylene-based PDI acceptor for non-fullerene organic solar cells in this embodiment is as follows:
[0031] Compound 1 (50 mg, 0.067 mmol), compound 2 (300 mg, 0.2 mmol) and K3PO4 (140 mg, 0.66 mmol) were dissolved in a mixed solvent of 20 mL tetrahydrofuran and 2 mL H2O, and then degassed; Pd(dppf)Cl2 (10 mg, 0.013 mmol) was added in a nitrogen atmosphere, degassed again for 10 min, and then refluxed and stirred at 90°C for 48 h to obtain compound NP-FPDI; after cooling to room temperature, the reaction mixture was poured into water, and the product was extracted in dichloromethane (CH2Cl2); the solvent was then evaporated under reduced pressure, and the residue was purified by silica gel column chromatography and eluted with petroleum ether and CH2Cl2 in a volume ratio of 1:2 to obtain dark red solid NP-FPDI (yield 71%), which is the perylene PDI receptor; wherein compound 1 is prepared according to the literature MJSung, S.Yoon, S.-K.Kwon, Y.-H.Kim, DSChung, ACS Appl It was prepared by the method provided in Mater Interfaces, 8(45)(2016), pp.31172-31178, and the structural formula is shown below:
[0032]
[0033] Compound 2 was prepared according to the method provided in Sisto, Thomas J. and Zhong, Yu and Zhang, Boyuan and Trinh, M. Tuan and Miyata, Kiyoshi and Zhong, Xinjue and Zhu, X.-Y. and Steigerwald, Michael L. and Ng, Fay and Nuckolls, Colin. JACS., 2017, 139, 5648-5651, and the structural formula is shown below:
[0034]
[0035] The structural formula of NP-FPDI is as follows:
[0036]
[0037] In the present embodiment, the synthesis process of NP-FPDI is as follows:
[0038]
[0039] The hydrogen and carbon spectra of NP-FPDI are as follows: Figure 1-2 As shown: 1H NMR(500MHZ,C2D2Cl4)δ:11.73-11.59(m,6H),10.82-10.73(m,6H),10.54(br,4H),10.19-10.05(m,5H),9.76-9.57(m,4H),9.36-8.91 (m,5H),6.66-6.45(m,8H),6.16(d,J=34.45Hz,2H),3.68-3.56(m,17H),3.35-3.22(m,16H),2.67-2.58(m,118H),2.37-1.92(m,56H); 13 C NMR (125MHz, CDCl3, δ):141.49,134.31,134.04,133.72,129.09,127.35,126.91,126.59,126.12,125.81,124.38,123.9 0,122.43,55.15,32.43,31.80,29.96,29.62,29.39,29.08,26.76,26.64,22.60,14.10.HRMS-MALDI(m / z):calcd.for(C 224 H 249 N9O 16 ):3320.8947; found,3320.8944.
[0040] The UV-visible absorption spectrum of the NP-FPDI receptor prepared in this example in the film is as follows: Figure 3 As shown in the figure, NP-FPDI shows four distinct absorption peaks in the range of 400-600nm and a weak and broad peak in the range of 600-800nm. The four distinct peaks appearing in the shorter wavelength region can be attributed to the fused PDI (FPDI) unit, while the weak absorption peak in the longer wavelength region represents the intramolecular charge transfer (ICT) effect between the electron-donating NP core and the electron-withdrawing fused PDI (FPDI) unit. The peak intensity of NP-FPDI is higher due to the intramolecular push-pull effect, which enables the intramolecular charge transfer from the NP donor core to the fused PDI unit. Figure 3 The UV-visible absorption spectrum of the PBDB-T donor polymer is also shown, with an absorption wavelength range of 500–700 nm, which is completely complementary to the absorption of NP-FPDI.
[0041] At the same time, the obtained compound NP-FPDI was subjected to thermogravimetric analysis, and the results were as follows Figure 4As shown in Figure 1, the decomposition temperature of 5wt.% NP-FPDI is 385°C, indicating that the compound NP-FPDI has good thermal stability. The electrochemical properties of NP-FPDI were measured on a working carbon electrode by cyclic voltammetry in a CH3CN solution containing 0.1M Bu4NPF6 as an electrolyte and ferrocene / ferrocene (Fc / Fc+) as an internal reference standard, as shown in Figure 1. Figure 5 As shown in the figure, it can be seen that the initial oxidation potential (E ox ) is 0.534 V. The HOMO / LUMO energy level is calculated by the formula E HOMO / E LUMO =-e[E ox / E red +4.8+E (Fc / Fc+) ](eV) calculation, E (Fc / Fc+) =0.534V, HOMO energy level is -5.4eV, LUMO energy level is -3.6eV (such as Figure 6 The photovoltaic performance of this PDI-based acceptor was evaluated in an inverted device structure: ITO / ZnO(30nm) / PBDB-T:NP-FPDI / MoO3(8.5nm) / Ag(100nm).
[0042] The photoelectric conversion efficiency (PCE) and open circuit voltage (V oc ), short circuit current (J sc ), fill factor (FF) test, Figure 7 The current density versus voltage (JV) curves of the organic solar cell devices are presented. The active layer was prepared by spin coating a solution of PBDB-T and NP-FPDI in o-dichlorobenzene (o-DCB) with a polymer concentration of 4 mg / mL. Figure 8 The EQE curve of PBDB-T:NP-FPDI organic solar cells is given. The weight ratio of PBDB-T donor to NP-FPDI acceptor and the film thickness were carefully optimized, and finally the optimal weight ratio of PBDB-T donor to NP-FPDI acceptor was 1:1, and the optimal thickness of the active layer was about 100nm. The cast device of PBDB-T:NP-FPDI achieved a PCE of 6.62%, V oc 0.88V, J sc 11.73 mA / cm 2 , the filling factor (FF) is 64.28%. Then, after adding 0.7% DIO as an additive, a PCE of 7.14% can be obtained, J sc 12.52mA / cm 2 , V oc It is 0.88V and FF is 64.85%.
[0043] Example 2
[0044] The synthesis method of the perylene-based PDI acceptor for non-fullerene organic solar cells in this embodiment is as follows:
[0045] Compound 1 (50 mg, 0.067 mmol), compound 2 (255 mg, 0.17 mmol) and K3PO4 (72 mg, 0.34 mmol) were dissolved in a mixed solvent of 24 mL tetrahydrofuran and 4 mL H2O, and degassed again for 10 min; Pd(dppf)Cl2 (8.46 mg, 0.011 mmol) was added in a nitrogen atmosphere, and then refluxed and stirred at 90°C for 48 h to obtain compound NP-FPDI; after cooling to room temperature, the reaction mixture was poured into water, and the product was extracted in dichloromethane (CH2Cl2); the solvent was then evaporated under reduced pressure, and the residue was purified by silica gel column chromatography and eluted with petroleum ether and CH2Cl2 in a volume ratio of 1:2 to obtain dark red solid NP-FPDI (yield 58%), which is the perylene PDI receptor. The preparation method of compound 1 and compound 2 is the same as that of Example 1.
[0046] In the present embodiment, the synthesis process of NP-FPDI is as follows:
[0047]
[0048] Example 3
[0049] The synthesis method of the perylene-based PDI acceptor for non-fullerene organic solar cells in this embodiment is as follows:
[0050] Compound 1 (50 mg, 0.067 mmol), compound 2 (225 mg, 0.15 mmol) and K3PO4 (43 mg, 0.2 mmol) were dissolved in a mixed solvent of 26 mL tetrahydrofuran and 4 mL H2O, and then degassed; Pd(dppf)Cl2 (5.38 mg, 0.007 mmol) was added in a nitrogen atmosphere, degassed again for 10 min, and then refluxed and stirred at 90°C for 48 h to obtain compound NP-FPDI; after cooling to room temperature, the reaction mixture was poured into water, and the product was extracted in dichloromethane (CH2Cl2); the solvent was then evaporated under reduced pressure, and the residue was purified by silica gel column chromatography and eluted with petroleum ether and CH2Cl2 in a volume ratio of 1:2 to obtain dark red solid NP-FPDI (yield 48%), which is the perylene PDI receptor. The preparation method of compound 1 and compound 2 is the same as that of Example 1.
[0051] In the present embodiment, the synthesis process of NP-FPDI is as follows:
[0052]
Claims
1. A method for synthesizing a perylene-based PDI acceptor for non-fullerene organic solar cells, characterized in that: Compound 1, compound 2 and K2PO3 are dissolved in a mixed solvent of tetrahydrofuran and H2O, Pd(dppf)Cl2 is added in a nitrogen atmosphere, and then refluxed to obtain compound NP-FPDI; after cooling to room temperature, the solvent is removed under reduced pressure, and the residue is purified by silica gel column chromatography and eluted with petroleum ether and CH2Cl2 to obtain solid NP-FPDI, which is a perylene PDI receptor; wherein the structural formula of compound 1 is as follows: The structural formula of compound 2 is shown below: Wherein, R is a C5 or C6 alkyl group.
2. The method for synthesizing a perylene-based PDI acceptor for non-fullerene organic solar cells according to claim 1, characterized in that: The molar ratio of compound 1, compound 2, K3PO4 and Pd(dppf)Cl2 is 1:2-3:2-10:0.1-0.
2.
3. The method for synthesizing a perylene-based PDI acceptor for non-fullerene organic solar cells according to claim 1, characterized in that: The molar volume ratio of compound 1 to the mixed solvent is 1 mmol:300-450 mL.
4. The method for synthesizing a perylene-based PDI acceptor for non-fullerene organic solar cells according to claim 1, characterized in that: The volume ratio of tetrahydrofuran to H2O in the mixed solvent is 6-10:
1.
5. The method for synthesizing a perylene-based PDI acceptor for non-fullerene organic solar cells according to claim 1, characterized in that: Reflux for 48-72h.
6. The method for synthesizing a perylene-based PDI acceptor for non-fullerene organic solar cells according to claim 1, characterized in that: The volume ratio of petroleum ether to CH2Cl2 is 1:1-3.
7. A perylene-based PDI acceptor for non-fullerene organic solar cells prepared by the synthesis method according to any one of claims 1 to 6.