Transition metal cobalt complex, preparation method and application thereof, and catalyst composition
By designing a combination of a diimide pyridine transition metal cobalt complex containing a large sterically hindered heterocyclic aromatic group and a cocatalyst, the problem of temperature sensitivity of the cobalt complex in catalytic polymerization was solved, and catalysis with high activity and thermal stability was achieved. The effect is suitable for industrial production and preparation of functional polymers.
Patent Information
- Application Number
- CN202310321628.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-01
AI Technical Summary
Existing transition metal cobalt complexes are temperature sensitive during the catalytic polymerization process, causing polymer properties to change with temperature, and it is difficult to obtain catalysts with high activity and thermal stability, which limits their industrial application.
A diimine pyridine transition metal cobalt complex containing a large sterically hindered heterocyclic aromatic group was designed, prepared by condensation reaction with an aniline compound and the compound CoX2, combined with methylaluminoxane or triisobutylaluminum modified methane Aloxane is used as a cocatalyst to optimize the structure and reaction conditions of the catalytic system.
It achieves improved catalytic activity and enhanced thermal stability, can maintain high reactivity at higher temperatures, is suitable for industrial production, prepares highly linear polyethylene wax and has the potential of functional polymers.
Smart Images

Figure CN118724983A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyolefin catalysts, and in particular to a transition metal cobalt complex and a preparation method and application thereof, and a catalyst composition. Background Art
[0002] The mechanical properties of polyethylene depend largely on the branching degree and branching type, crystal structure and molecular weight of the material. According to the density and branching degree of polyethylene, it mainly includes the following types: ultra-high molecular weight polyethylene (UHMWPE), ultra-low molecular weight polyethylene (ULMWPE or PE-Wax), high-density polyethylene (HDPE), linear low-density polyethylene (LLDPE), low-density polyethylene (LDPE), etc. Among them, ultra-high molecular weight polyethylene, as a thermoplastic engineering plastic with excellent comprehensive performance, has always attracted much attention. In addition, ultra-low molecular weight polyethylene, namely polyethylene wax, is widely used in the manufacturing process of polyvinyl chloride (PVC) and plays an important role in the processing of PVC product masterbatch and other products.
[0003] Polyethylene wax is an ultra-low molecular weight polyethylene composed of ethylene monomer chains, with a relative molecular mass of 1000-6000 and a melting point of about 90-120°C. Polyethylene wax has excellent mechanical properties, wear resistance and heat resistance, and has good lubricity, dispersibility and fluidity. It has good compatibility with other polyolefin resins and can be used as a processing aid for pipes, films, cables and other plastics and rubbers.
[0004] The inventors have been committed to the design and development of olefin polymerization catalysts and the exploration of catalytic processes, and have done a lot of work around transition metal catalysts and ligands such as N^N, N^N^N. The study found that by regulating the stereo and electronic effects of the ligands, the performance of its ethylene catalysis can be controlled, while ensuring high catalytic activity and further enhancing thermal stability, which has attracted the attention and recognition of international peers (Coord. Chem. Rev. 2017, 350, 68; Coord. Chem. Rev. 2018, 363, 92; Coord. Chem. Rev. 2018, 372, 101; Coord. Chem. Rev. 2019, 385, 208; Coord. Chem. Rev. 2020, 411, 21332; Coord. Chem. Rev. 2020, 416, 213524; Coord. Chem. Rev. 2021, 434, 213788.).
[0005] By further modifying the N-aryl group and introducing large sterically hindered diphenylmethyl or dibenzocycloheptyl groups at the 2-position and / or 4-position, the catalytic activity and thermal stability of the catalytic system can be effectively improved, such as the pyridine diimine cobalt complex (B–E) shown in Formula 1. Compared with complex B (Formula 1, Dalton Trans. 2013, 42, 9188–9197), complex C (Formula 1, Polym. Chem. 2012, 3, 787-793; Polymer 2012, 53, 130-137) introduces another diphenylmethyl group at the para position, and exhibits higher catalytic activity when alkylaluminoxane (MAO) or modified alkylaluminoxane (MMAO) is used as a co-catalyst; cobalt complex D (Formula 1, Sci China Chem 2016, 59, 1291-1300) has no significant improvement in the activity and thermal stability of catalytic ethylene polymerization; cobalt complex E (Formula 1, Molecules 2019, 24, 2007) has made further breakthroughs in thermal stability. When MAO is used as a co-catalyst, the catalytic activity can be maintained at 10 6 g(PE)(molCo) -1 h -1 At the same time, highly linear polyethylene with a relative molecular weight of 8-70 kg / mol was obtained. These research results have played a good reference role in our design of catalysts with high activity and high thermal stability, and have also laid a good foundation for further research.
[0006]
[0007] As a new type of olefin polymerization catalyst, transition metal complexes still face difficulties in related basic research and constraints on the promotion of industrialization. For example, transition metal complexes are sensitive to temperature during the catalytic polymerization process, which causes the properties of the resulting polymer to change with temperature. There are high requirements for the control of the temperature of the polymerization process. Therefore, in addition to improving the preparation conditions and efficiency, how to obtain high-activity ethylene polymerization catalysts with good thermal stability to adapt to industrial production and meet the society's demand for polyethylene wax products has become the core content of scholars' research and is also the key to whether industrialization can be promoted as soon as possible. Summary of the invention
[0008] Based on the above technical problems, the object of the present invention is to provide a transition metal cobalt complex and its preparation method and application, and a catalyst composition, wherein the complex has higher catalytic activity and stability.
[0009] To achieve the above object, the present invention provides a transition metal cobalt complex having a structure as shown in formula (I):
[0010]
[0011] wherein each X is the same or different and is independently selected from F, Cl, Br, I;
[0012] R 1 , R 2 , R 3 , R 4 , R 5 The same or different, each independently selected from one or more R a Substituted with the following groups: H, C 1-6 Alkyl, C 1-6 Alkoxy, C 6-20 Aryl or C 6-20 Heteroatom aromatic group;
[0013] R a Selected from H, F, Cl, Br, I, C 1-6 Alkyl, C 1-6 Alkoxy, C 3-10 Heterocyclic group, C 6-20 Aryl or C 6-20 heteroatom aromatic, and each R a Same or different.
[0014] The transition metal cobalt complex of the present invention, in formula (I), R 1 Selected from C 1-3 Alkyl and Cl; more preferably methyl.
[0015] The transition metal cobalt complex of the present invention, in formula (I), R 2 Selected from C 1-3 Alkyl and Cl; more preferably methyl.
[0016] The transition metal cobalt complex of the present invention, in formula (I), R 3 , R 4 The same or different, each independently selected from H and C 1-6 Alkyl; more preferably all are H.
[0017] The transition metal cobalt complex of the present invention, in formula (I),
[0018] R 1 =R 2 =Me, X is Cl, R 3 , R 4 , R 5 All are H; or
[0019] R 1 =R 2 =Et, X is Cl, R 3 , R 4 , R 5All are H; or
[0020] R 1 =R 2 =iPr, X is Cl, R 3 , R 4 , R 5 All are H; or
[0021] R 1 =Me, R 2 =Et, X is Cl, R 3 , R 4 , R 5 All are H; or
[0022] R 1 =R 2 =Cl, X is Cl, R 3 , R 4 , R 5 Both are H.
[0023] To achieve the above object, the present invention also provides a method for preparing the transition metal cobalt complex, comprising the following steps:
[0024] The aniline compound represented by formula (II) is subjected to condensation reaction with 2-acetylpyridine and compound CoX2 to obtain a metal complex represented by formula (I);
[0025]
[0026] wherein each X is the same or different and is independently selected from F, Cl, Br, I;
[0027] R 1 , R 2 , R 3 , R 4 , R 5 The same or different, each independently selected from one or more R a Substituted with the following groups: H, C 1-6 Alkyl, C 1-6 Alkoxy, C 6-20 Aryl or C 6-20 Heteroatom aromatic group;
[0028] R a Selected from H, F, Cl, Br, I, C 1-6 Alkyl, C 1-6 Alkoxy, C 3-10 Heterocyclic group, C 6-20 Aryl or C 6-20 heteroatom aromatic, and each R a Same or different.
[0029] In the present invention, the term "C 1-6 The term "alkyl" refers to a straight or branched chain alkyl group having 1 to 6 carbon atoms, such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, sec-butyl, pentyl, and neopentyl.
[0030] The term "C 1-6 "Alkoxy" is to be understood as meaning preferably a linear or branched, saturated, monovalent hydrocarbon radical of the formula -O-alkyl, for example methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, sec-butoxy, tert-butoxy, pentyloxy, isopentyloxy, hexyloxy or the isomers thereof.
[0031] The term "C 3-10 "Heterocyclyl" is understood to mean preferably a group of the formula -N / O / S-cycloalkyl having 3 to 10 carbon atoms. The heterocyclyl may be linked to the remainder of the molecule via any of the carbon atoms or the nitrogen atom, if present. In particular, the heterocyclyl may include, but is not limited to: a 4-membered ring, such as azetidinyl, oxetanyl; a 5-membered ring, such as tetrahydrofuranyl, dioxolyl, pyrrolidinyl, imidazolidinyl, pyrazolidinyl, pyrrolinyl; or a 6-membered ring, such as tetrahydropyranyl, piperidinyl, morpholinyl, dithianyl, thiomorpholinyl, piperazinyl or trithianyl; or a 7-membered ring, such as diazepanyl. Optionally, the heterocyclyl It may be benzo-fused. The heterocyclic group may be bicyclic, for example, but not limited to, a 5,5-membered ring, such as a hexahydrocyclopenta[c]pyrrole-2(1H)-yl ring, or a 5,6-membered bicyclic ring, such as a hexahydropyrrolo[1,2-a]pyrazine-2(1H)-yl ring. The ring containing nitrogen atoms may be partially unsaturated, i.e., it may contain one or more double bonds, for example, but not limited to, 2,5-dihydro-1H-pyrrolyl, 4H-[1,3,4]thiadiazinyl, 4,5-dihydrooxazolyl or 4H-[1,4]thiazinyl, or it may be benzo-fused, for example, but not limited to, dihydroisoquinolinyl. According to the present invention, the heterocyclic group is non-aromatic.
[0032] The term "C 6-20 "Aryl" is understood to mean preferably a monovalent aromatic or partially aromatic monocyclic, bicyclic or tricyclic hydrocarbon ring having 6 to 20 carbon atoms, preferably "C 6-14 The term "C 6-14 "Aryl" is understood to mean preferably a monovalent aromatic or partially aromatic monocyclic, bicyclic or tricyclic hydrocarbon ring ("C 6-14 or a ring having 9 carbon atoms ("C9 aryl"), for example indanyl or indenyl, or a ring having 10 carbon atoms ("C 10aryl), such as tetrahydronaphthyl, dihydronaphthyl or naphthyl, or a ring having 13 carbon atoms ("C 13 aryl), such as fluorenyl, or a ring having 14 carbon atoms ("C 14 "aryl"), for example anthracenyl.
[0033] The term "C 6-20 "Heteroatom aryl" is understood to mean preferably a group of the formula -N-aryl or -N-heteroaryl. Examples of monocyclic heteroaryl groups include, but are not limited to, thienyl, furanyl, pyrrolyl, oxazolyl, thiazolyl, imidazolyl, pyrazolyl, isoxazolyl, isothiazolyl, oxadiazolyl, triazolyl, thiadiazolyl, thia-4H-pyrazolyl, and the like, and benzo derivatives thereof, such as benzofuranyl, benzothienyl, benzoxazolyl, benzisoxazolyl, benzo imidazolyl, benzotriazolyl, indazolyl, indolyl, isoindolyl, etc.; or pyridyl, pyridazinyl, pyrimidinyl, pyrazinyl, triazinyl, etc., and benzo derivatives thereof, such as quinolyl, quinazolinyl, isoquinolyl, etc.; or azinyl, indolizinyl, purinyl, etc., and benzo derivatives thereof; or cinnolinyl, phthalazinyl, quinazolinyl, quinoxalinyl, naphthyridinyl, pteridinyl, carbazolyl, acridinyl, phenazinyl, phenothiazinyl, phenoxazinyl, etc.
[0034] In the preparation method of the present invention, the added form of the compound CoX2 is not limited, and it can be a cobalt halide, or a hydrate or solvate of a halide, for example, it can be CoCl2 or CoCl2·6H2O.
[0035] In the preparation method of the present invention, the condensation reaction is carried out under oxygen-free conditions, for example, under the protection of an inert gas such as nitrogen.
[0036] In the preparation method of the present invention, the condensation reaction is carried out under the catalysis of an organic acid; the organic acid is one or more of formic acid, acetic acid and p-toluenesulfonic acid, preferably acetic acid.
[0037] In the preparation method of the present invention, the condensation reaction is carried out under heating reflux for 6 to 12 hours, preferably 8 to 10 hours.
[0038] In the preparation method of the present invention, the molar ratio of the compound CoX2 to the aniline compound represented by formula (II) is 1:2-3, preferably 1:2-2.5, and more preferably 1:2.5.
[0039] The preparation method of the present invention further comprises the step of purifying the obtained metal complex represented by formula (I), wherein the purification method comprises the following steps:
[0040] A) removing volatile substances from the metal complex represented by formula (I) to obtain a concentrated solution, and adding the concentrated solution into an organic solvent for precipitation;
[0041] b) subjecting the material precipitated in step a) to solid-liquid separation, washing the solid phase with an organic solvent and drying it.
[0042] Wherein, the organic solvent is an anhydrous organic solvent.
[0043] To achieve the above objectives, the present invention also provides a catalyst composition, including a main catalyst and, optionally, a co-catalyst, wherein the main catalyst is the transition metal cobalt complex, and the co-catalyst is one or more of aluminoxane, alkylaluminum and alkylaluminum chloride.
[0044] The catalyst composition of the present invention, wherein the aluminoxane is methylaluminoxane (MAO) and / or triisobutylaluminum-modified methylaluminoxane (MMAO); the alkyl group in the alkylaluminum and alkylaluminum chloride is selected from C 1-3 Alkyl; the alkylaluminum chloride is preferably diethylaluminum chloride (Et2AlCl) and / or dimethylaluminum chloride (Me2AlCl).
[0045] The catalyst composition of the present invention has a molar ratio of the metal Al in the co-catalyst to the central metal Co in the transition metal cobalt complex of (500-4000):1, preferably a molar ratio of (1000-3500):1, for example, 1000:1, 1500:1, 1750:1, 2000:1, 2250:1, 2500:1, 2750:1, 3250:1.
[0046] In the catalyst composition of the present invention, when the co-catalyst is methylaluminoxane, the molar ratio of the metal Al in the methylaluminoxane to the central metal Co in the transition metal cobalt complex is (2000-3000):1, and the more preferred molar ratio is 2500:1, for example, 2200:1, 2300:1, 2400:1, 2550:1, 2700:1, 2950:1;
[0047] When the co-catalyst is triisobutylaluminum-modified methylaluminoxane, the molar ratio of the metal Al in the triisobutylaluminum-modified methylaluminoxane to the central metal Co in the transition metal cobalt complex is (1000-2500):1, and the more preferred molar ratio is 1750:1, for example, 1200:1, 1500:1, 1750:1, 2000:1, 2250:1;
[0048] When the co-catalyst is alkyl aluminum, the molar ratio of the metal Al in the alkyl aluminum to the central metal Co in the transition metal cobalt complex is (200-2000):1, for example, 300:1, 500:1, 800:1, 1000:1, 1500:1;
[0049] When the co-catalyst is alkylaluminum chloride, the molar ratio of metal Al in the alkylaluminum chloride to the central metal Co in the transition metal cobalt complex is (200-2000):1, for example, 300:1, 500:1, 800:1, 1000:1, or 1500:1.
[0050] To achieve the above object, the present invention also provides a use of the transition metal cobalt complex or the catalyst composition in catalyzing olefin polymerization.
[0051] The transition metal cobalt complex or catalyst composition provided by the present invention is particularly suitable for the polymerization reaction of ethylene.
[0052] When the transition metal cobalt complex or catalyst composition provided by the present invention is used to catalyze the polymerization reaction, the polymerization reaction conditions are conventional reaction conditions in the art, such as the polymerization reaction temperature can be 30-100°C, specifically 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C; preferably 30-70°C; the polymerization reaction time can be 5-60min, specifically 30min; the polymerization reaction pressure can be 0.5-10atm, specifically 10atm; the polymerization reaction solvent can be selected from one or more of toluene, o-xylene, dichloromethane, ethanol, tetrahydrofuran, hexane or cyclohexane.
[0053] Beneficial effects of the present invention:
[0054] 1. The diiminopyridine transition metal complex containing a large sterically hindered heterocyclic aromatic group provided by the present invention has the following structural characteristics: the aniline on both sides of the metal center is in a symmetrical structure, and the large sterically hindered heterocyclic aromatic group substituent at the 5 position of the aniline. Under the synergistic effect of this structure, the system has higher catalytic activity and stability, and can be used as a catalyst in ethylene polymerization. It has high reaction activity and has extremely strong control performance on polyethylene molecular weight; highly linear polyethylene wax can be prepared. For example, when methylaluminoxane (MAO) or methylaluminoxane (MMAO) modified with triisobutylaluminum is used as a cocatalyst, the activity of the cobalt complex in catalyzing ethylene polymerization can reach 7.4×10 6 g(PE)(mol Co) -1 h -1 The weight average molecular weight (M) of polyethylene prepared by this type of catalyst w ) fluctuates between 1.1–8.1 kg / mol and can be used to prepare special high-end commercial polyethylene wax products.
[0055] 2. The transition metal cobalt complex of diimine pyridine containing large sterically hindered heterocyclic aromatic group provided by the present invention exhibits high thermal stability in catalyzing ethylene polymerization. Even at a high temperature of 70°C, the catalytic activity can still be maintained at 2.2×10 6 g(PE)(mol Co) -1 h -1 , which meets the operating temperature of industrial production and has the prospect of further industrial application.
[0056] 3. The transition metal cobalt complex provided by the present invention can be used to prepare polyethylene wax products with unsaturated bonds at the ends, thereby further preparing functionalized polyethylene wax, thereby obtaining high-value functional polymers or devices.
[0057] 4. The present invention provides a method for preparing a diiminopyridine intermediate and a transition metal complex of an N-aryl group-introduced bulky heterocyclic aromatic acridine, wherein the preparation process has the advantages of mild reaction conditions, short cycle, and simple operating conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 Schematic diagram of the crystal structure of the complex Co-4 of Example 9.
[0059] Figure 2 This is the H-NMR spectrum of the polymer obtained in Example 11f).
[0060] Figure 3 This is the thermal NMR carbon spectrum of the polymer obtained in Example 16i). DETAILED DESCRIPTION
[0061] The present invention is described in detail below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art in this field can make some non-essential improvements and adjustments to the present invention based on the above content of the present invention.
[0062] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0063] Unless otherwise specified, the concentrations in the following examples are molar concentrations.
[0064] The methylaluminoxane (MAO for short) and triisobutylaluminum-modified methylaluminoxane (MMAO for short) used in Examples 11-20 were purchased from AkzoNobel, USA. The Al / Co in the following examples refers to the molar ratio of the metal Al in the cocatalyst MAO or MMAO to the Co in the added metal complex catalyst.
[0065] Molecular weight (M) of the polymers obtained in Examples 11-20 Ethylene polymerization w ) were determined by conventional high temperature GPC method, and the melting point (T m ) were determined according to the conventional DSC method, and the polymerization activity of the polymers were calculated according to the following formula: polymerization activity = polymer yield / (catalyst dosage*polymerization time).
[0066] All synthesized compounds described below were confirmed by infrared and elemental analysis.
[0067] Examples 1-10 were prepared by the following reaction scheme:
[0068]
[0069] Example 1
[0070] Preparation of 2,6-dimethyl-4-acridineaniline (A1)
[0071] 2,6-Dimethylaniline (1.45 g, 12 mmol) and 9-hydroxyacridine (3 g, 15 mmol) were placed in a 250 mL round bottom flask. The mixture was stirred under nitrogen at 130 ° C for 30 minutes, and then a catalytic amount of ZnCl2 in HCl solution was added dropwise. The reaction mixture was further heated for 2 hours, and after cooling, the solid was dissolved in DCM (200 mL). It was filtered and washed twice with a saturated solution of ammonium chloride and sodium chloride. The organic portion was collected, dried over anhydrous Na2SO4, and concentrated under reduced pressure. The product was recrystallized from DCM using n-heptane to obtain a white crystalline solid (1.25 g, 34%).
[0072] The structural confirmation data are as follows:
[0073] 1 H NMR (400MHz,CDCl3,TMS): 1 H NMR (400MHz, CDCl3, TMS): δ7.18(t,J=3.8Hz,2H,Ar-H),7.16(m,4H,Ar-H),7.09(t,J=7.0Hz,2H,Ar-H),6.76(s,2H,Ar-H m ),5.08(s,1H,–CH–)2.8(s,2H,NH2),2.10(s,6H,–CH3).
[0074] 13C NMR (100MHz, CDCl3, TMS):d 151.1,141.3,136.3,129.8,128.2,127.5,125.2,123.1,121.9,116.3,77.3,77.0,76.7,43.6,17.7
[0075] Example 2
[0076] Preparation of 2,6-diethyl-4-acridineaniline (A2)
[0077] 2,6-Diethylaniline (1.79 g, 12 mmol) and 9-hydroxyacridine (3 g, 15 mmol) were placed in a 250 mL round bottom flask. The mixture was stirred under nitrogen at 130 ° C for 30 minutes, and then a catalytic amount of ZnCl2 in HCl solution was added dropwise. The reaction mixture was further heated for 2 hours, and after cooling, the solid was dissolved in DCM (200 mL). It was filtered and washed twice with a saturated solution of ammonium chloride and sodium chloride. The organic portion was collected, dried over anhydrous Na2SO4, and concentrated under reduced pressure. The product was recrystallized from DCM using n-heptane to obtain a white crystalline solid (1.26 g, 38%).
[0078] The structural confirmation data are as follows:
[0079] 1 H NMR (400MHz, CDCl3, TMS): δ7.15(t,J=3.8Hz,2H,Ar-H),7.12–7.06(m,4H,Ar-H),6.96(t,J=3.8Hz,2H,Ar-H),6.76(s,2H,Ar-H m ),5.12(s,1H,–CH–),3.51(s,2H,NH2),2.49–2.43(m,4H,–CH2–),1.18(t,J=7.6Hz,6H,–CH3).
[0080] 13 C NMR (100MHz, CDCl3, TMS): d 151.1, 140.1, 136.3, 129.7, 128.0, 127.4, 126.2, 125.3, 123.1, 116.3, 77.3, 77.0, 76.7, 43.9, 24.4, 13.0.
[0081] Example 3
[0082] Preparation of 2,6-diisopropyl-4-acridineaniline (A3)
[0083] 2,6-Diisopropylaniline (2.12 g, 12 mmol) and 9-hydroxyacridine (3 g, 15 mmol) were charged into a 250 mL round bottom flask. The mixture was stirred under nitrogen at 130 °C for 30 minutes, and then a catalytic amount of ZnCl2 in HCl solution was added dropwise. The reaction mixture was further heated for 2 hours and after cooling, the solid was dissolved in DCM (200 mL). It was filtered and washed twice with a saturated solution of ammonium chloride and sodium chloride. The organic portion was collected, dried over anhydrous Na2SO4, and concentrated under reduced pressure. The product was recrystallized from DCM using n-heptane to obtain a white crystalline solid (1.30 g, 36%).
[0084] The structural confirmation data are as follows:
[0085] 1 H NMR (400MHz, CDCl3, TMS): δ7.15 (t, J=6.8Hz, 2H, Ar-H), 7.10–7.05 (m, 4H, Ar-H), 6.95 (t, J=7.4Hz, 2H, Ar-H), 6.81(s,2H,Ar-H),5.13(s,1H,–CH–),3.51(s,2H,NH2),2.89–2.80(m,2H,–CH–),1.27(t,J=4.4Hz,12H,–CH3).
[0086] 13 C NMR (100MHz, CDCl3, TMS): d 151.3, 138.8, 136.0, 132.6, 129.6, 127.4, 125.5, 123.0, 77.3, 77.0, 76.7, 44.3, 28.0, 22.4.
[0087] Example 4
[0088] Preparation of 2-methyl-6-ethyl-4-acridineaniline (A4)
[0089] 2-Methyl-6-ethylaniline (1.62 g, 12 mmol) and 9-hydroxyacridine (3 g, 15 mmol) were placed in a 250 mL round bottom flask. The mixture was stirred for 30 minutes under nitrogen at 130 ° C, and then a catalytic amount of ZnCl2 in HCl solution was added dropwise. The reaction mixture was further heated for 2 hours, and after cooling, the solid was dissolved in DCM (200 mL). It was filtered and washed twice with a saturated solution of ammonium chloride and sodium chloride. The organic portion was collected, dried over anhydrous Na2SO4, and concentrated under reduced pressure. The product was recrystallized from DCM using n-heptane to obtain a white crystalline solid (1.01 g, 32%).
[0090] The structural confirmation data are as follows:
[0091] 1 H NMR (400MHz, CDCl3, TMS): d 7.11 (t, J=4.2Hz, 2H, Ar-H), 7.09–6.96 (m, 4H, Ar-H), 6.95 (t, J=4Hz, 2H, Ar-H), 6.81 (s, 1H, Ar-H m ),6.72(s,1H,Ar-H m ),5.11(s,1H,–CH–),3.51(s,2H,NH2),2.51–2.45(m,2H,–CH2–),2.09(s,3H,–CH3),1.39(t,J=4Hz,3H,–CH3).
[0092] 13 C NMR (100MHz, CDCl3, TMS):d 151.1,140.7,136.3,129.7,128.2,127.6,127.5126.3,125.3,123.1,122.4,116.3,77.4,77.0,76.7,43.8,24.4,17.8,13.1.
[0093] Example 5
[0094] Preparation of 2,6-chloro-4-acridineaniline (A5)
[0095] 2,6-Dichloroaniline (1.94 g, 12 mmol) and 9-hydroxyacridine (3 g, 15 mmol) were placed in a 250 mL round bottom flask. The mixture was stirred under nitrogen at 130 ° C for 30 minutes, and then a catalytic amount of ZnCl2 in HCl solution was added dropwise. The reaction mixture was further heated for 2 hours, and after cooling, the solid was dissolved in DCM (200 mL). It was filtered and washed twice with a saturated solution of ammonium chloride and sodium chloride. The organic portion was collected, dried over anhydrous Na2SO4, and concentrated under reduced pressure. The product was recrystallized from DCM using n-heptane to obtain a white crystalline solid (1.30 g, 36%).
[0096] The structural confirmation data are as follows:
[0097] 1 H NMR (400MHz, CDCl3, TMS): d 7.15 (t, J=3.8Hz, 2H, Ar-H), 7.12–7.06 (m, 4H, Ar-H), 6.96 (t, J=3.8Hz, 2H, Ar-H), 6.76 (s, 2H, Ar-H m ),5.12(s,1H),3.51(s,2H,NH2).
[0098] 13 C NMR (100MHz, CDCl3, TMS): d 151.1,141.7,135.3,129.4,128.1,127.8,127.5126.2,125.6,122.3,119.1,77.4,77.4,76.3,42.7,23.3,22.5.
[0099] Example 6
[0100] Preparation of 2,6-bis[1-(4-acridine-2,6-dimethylphenylimino)ethyl]-pyridylcobalt dichloride (Co-1)
[0101] Cobalt complex Co-1(R 1 =R 2 =Me, X is Cl, R 3 , R 4 , R 5 All H) were synthesized in one pot. A Schlenk tube was loaded with 2,6-diacetylpyridine (0.03 g, 0.20 mmol), 2,6-dimethyl-4-acridinylaniline (0.20 g, 0.60 mmol) and CoCl2 (0.02 g, 0.20 mmol) and refluxed with acetic acid (30 mL). The reaction was continued at 120 °C for 6 hours and the volatiles were evaporated using a pump to obtain a concentrated solution. The cobalt complex was precipitated using ether (20 mL), filtered, washed with ether (3×15 mL), and isolated as an air-stable green powder in good yield (0.15 g, 78%).
[0102] The structural confirmation data are as follows:
[0103] FT-IR(cm -1 ):3230(w),3001(w)1652(ν(C=N),m),1595(w),1577(w),1536
[0104] (w),1479(s),1450(s),1372(w),1303(w),1301(w),1250(s),1214(w),1148(w) ,1118(w),1118(w),1096(w),1032(w),946(w),879(m),811(w),751(s),658(w).
[0105] Elemental analysis: C 51 H 41 Cl2CoN5 (855.77) Theoretical value: 71.58; H, 5.06; N, 8.18%. Experimental value: C, 71.47; H, 5.05; N, 7.95.
[0106] Example 7
[0107] Preparation of 2,6-bis[1-(4-acridine-2,6-diethylphenylimino)ethyl]-pyridylcobalt dichloride (Co-2)
[0108] Cobalt complex Co-2(R 1 =R 2 =Et, X is Cl, R 3 , R 4 , R 5 All H) were synthesized in one pot. A Schlenk tube was loaded with 2,6-diacetylpyridine (0.03 g, 0.20 mmol), 2,6-diethyl 4-acridinylaniline (0.20 g, 0.60 mmol) and CoCl2 (0.02 g, 0.20 mmol) and refluxed with acetic acid (30 mL). The reaction was continued at 120 °C for 6 hours and the volatiles were evaporated using a pump to obtain a concentrated solution. The cobalt complex was precipitated using ether (20 mL), filtered, washed with ether (3×15 mL), and isolated as an air-stable green powder in good yield (0.17 g, 94%).
[0109] The structural confirmation data are as follows:
[0110] FT-IR(cm -1 ):2965(w),2932(w),2875(w),1623(ν(C=N),w),1576(m),1543
[0111] (w),1478(s),1450(s),1371(w),1323(w),1301(w),1251(w),1211(m),1184(w),115 0(w),1118(w),1095(w),1030(w),981(w),940(w),881(m),808(w),749(s),676(w).
[0112] Elemental analysis: C 55 H 49 Cl2CoN5 (911.88) theoretical value: C, 72.44; H, 5.64; N, 7.68%. Experimental value: C, 72.32; H, 5.62; N, 7.56%.
[0113] Example 8
[0114] Preparation of 2,6-bis[1-(4-acridine-2,6-diisopropylphenylimino)ethyl]-pyridylcobalt dichloride (Co-3)
[0115] Cobalt complex Co-3(R 1 =R2 =iPr, X is Cl, R 3 , R 4 , R 5 All H) were synthesized in one pot. A Schlenk tube was loaded with 2,6-diacetylpyridine (0.03 g, 0.20 mmol), 2,6-diisopropyl 4-acridinylaniline (0.21 g, 0.60 mmol) and CoCl2 (0.02 g, 0.20 mmol) and refluxed with acetic acid (30 mL). The reaction was continued at 120 °C for 6 hours and the volatiles were evaporated using a pump to obtain a concentrated solution. The cobalt complex was precipitated using ether (20 mL), filtered, washed with ether (3×15 mL), and isolated as an air-stable green powder in good yield (0.09 g, 53%).
[0116] The structural confirmation data are as follows:
[0117] FT-IR(cm -1 ):3380(m),2961(m),2868(w),1602(ν(C=N),w),1570(w),1550
[0118] (w),1473(m),1449(s),1369(w),1303(w),1251(s),1211(w),1079(w),1028(w),944(w),833(w),812(w),751(s),657(w).
[0119] Elemental analysis: C 59 H 57 Cl2CoN5 (967.99) theoretical value: C, 73.21; H, 6.14; N, 7.24%. Experimental value: C, 73.40; H, 6.30; N, 6.99%.
[0120] Example 9
[0121] Preparation of 2,6-bis[1-(4-acridinium-2-methyl-6-ethylphenylimino)ethyl]-pyridylcobalt dichloride (Co-4)
[0122] Cobalt complex Co-4(R 1 =Me, R 2 =Et, X is Cl, R 3 , R 4 , R 5All H) were synthesized in one pot. The Schlenk tube was filled with 2,6-diacetylpyridine (0.03 g, 0.20 mmol), 2-methyl-6-ethyl 4-acridinylaniline (0.19 g, 0.60 mmol) and CoCl2 (0.02 g, 0.20 mmol) and refluxed with acetic acid (30 mL). The reaction was continued at 120 ° C for 6 hours, and the volatiles were evaporated using a pump to obtain a concentrated solution. The cobalt complex was precipitated with ether (20 mL), filtered, washed with ether (3×15 mL), and isolated as an air-stable green powder in good yield (0.12 g, 53%). The crystal structure diagram of the product is shown as follows Figure 1 shown.
[0123] The structural confirmation data are as follows:
[0124] FT-IR(cm -1 ):3372(w),2962(w),2284(w),2121(w),1604(ν(C=N),w),1543
[0125] (m),1478(m),1448(s),1373(w),1304(w),1251(s),1210(w),1116(w),1095(w),1029(w),945(w),880(w),812(w),753(s),670(w).
[0126] Elemental analysis: C 53 H 45 Cl2CoN5 (883.83) theoretical value: C, 72.03; H, 5.36, N, 7.92%. Experimental value: C, 72.16; H, 5.49; N, 8.12%.
[0127] Example 10
[0128] Preparation of 2,6-bis[1-(4-acridine-2,6-dichlorophenylimino)ethyl]-pyridylcobalt dichloride (Co-5)
[0129] Cobalt complex Co-5(R 1 =R 2 =Cl, X is Cl, R 3 , R 4 , R 5All H) were synthesized in one pot. A Schlenk tube was loaded with 2,6-diacetylpyridine (0.03 g, 0.20 mmol), 2,6-dichloro-4-acridinylaniline (0.21 g, 0.60 mmol) and CoCl2 (0.02 g, 0.20 mmol) and refluxed with acetic acid (30 mL). The reaction was continued at 120 °C for 6 hours and the volatiles were evaporated using a pump to obtain a concentrated solution. The cobalt complex was precipitated using ether (20 mL), filtered, washed with ether (3×15 mL), and isolated as an air-stable green powder in good yield (0.30 g, 56%).
[0130] The structural confirmation data are as follows:
[0131] FT-IR(cm -1 )::3376(w),2962(w),1604(ν(C=N),w),1547(w),1478(m),1448
[0132] (s),1371(w),1304(w),1251(s),1210(w),1116(w),1095(w),1028(w),944(w),880(w),812(w),752(s),667(w).
[0133] Elemental analysis: C 47 H 29 Cl6CoN3 (937.43) theoretical value: C, 60.22; H, 3.33; N, 7.47%. Experimental value: C, 60.38; H, 3.29; N, 7.34%.
[0134] Example 11: Co-catalyzed ethylene polymerization by complex Co-1 and co-catalyst MAO under high pressure
[0135] a) In an ethylene atmosphere, 25 mL of a toluene solution of catalyst Co-1 (1.5 μmol) was injected into a 250 mL stainless steel autoclave equipped with mechanical stirring, followed by the addition of 25 mL toluene, the required amount of 2.1 mL of cocatalyst MAO (1.46 mol / L in toluene), and the addition of toluene to make the total volume of the solvent 100 mL. At this time, Al / Co = 2000:1. Mechanical stirring was started and maintained at 400 rpm. When the polymerization temperature reached 30°C, ethylene was charged into the reactor and the polymerization reaction began. The ethylene pressure was maintained at 10 atm at 30°C and the polymerization reaction was stirred for 30 min. The reaction solution was neutralized with an ethanol solution acidified with 10% hydrochloric acid to obtain a polymer precipitate, which was washed several times with ethanol and dried at 60°C in vacuum to constant weight. 4.09 g of polymer was weighed, and the polymerization activity was 5.44×10 6 g(PE)(mol Co) -1h -1 The molecular weight of the obtained polymer is M w =5.0kg·mol -1 , molecular weight distribution M w / M n =5.5(M w is the weight average molecular weight of the polymer, M n is the number average molecular weight of the polymer, obtained by GPC test), polymer T m =123.8℃(T m is the melting temperature of the polymer, measured by DSC).
[0136] b) is basically the same as method a) in this embodiment, except that the polymerization temperature is 40°C. Polymerization activity: 6.38×10 6 g(PE)(mol Co) -1 h -1 , polymer molecular weight M w =4.6kg·mol -1 , molecular weight distribution M w / M n =5.1, polymer T m =124.8℃.
[0137] c) is basically the same as method a) in this embodiment, except that the polymerization temperature is 50°C. Polymerization activity: 5.82×10 6 g(PE)(mol Co) -1 h -1 , polymer molecular weight M w =3.5kg·mol -1 , molecular weight distribution M w / M n =3.7, polymer T m =124.4℃.
[0138] d) is basically the same as method a) in this embodiment, except that the polymerization temperature is 60°C. Polymerization activity: 2.72×10 6 g(PE)(mol Co) -1 h -1 , polymer molecular weight M w =2.3kg·mol -1 , molecular weight distribution M w / M n =2.5, polymer T m =124.6℃.
[0139] e) is basically the same as method b) in this example, except that 2.3 mL of the cocatalyst MAO (1.46 mol / L in toluene) makes Al / Co = 2250:1. Polymerization activity: 7.01×10 6 g(PE)(mol Co) -1 h -1 , polymer molecular weight M w =3.4 kg·mol -1 , molecular weight distribution M w / M n =1.8, polymer T m =122.4℃.
[0140] f) is basically the same as method b) in this example, except that 2.6 mL of the cocatalyst MAO (1.46 mol / L in toluene) makes Al / Co = 2500:1. Polymerization activity: 7.43×10 6 g(PE)(mol Co) -1 h -1 , polymer molecular weight M w =2.7 kg·mol -1 , molecular weight distribution M w / M n =1.9, polymer T m =122.1℃.
[0141] Take 10 mg of the obtained polymer, dissolve it in 3 ml of deuterated 1,1,2,2-tetrachloroethane, and test the polymer at 100 °C. 1 H data, such as Figure 2 As shown, the signal is accumulated 64 times.
[0142] Take 60 mg of the obtained polymer, dissolve it in 3 ml of deuterated 1,1,2,2-tetrachloroethane, and test the polymer at 100 °C. 13 C data, such as Figure 3 The signal is accumulated 3000 times.
[0143] g) is basically the same as method b) in this example, except that 2.9 mL of the cocatalyst MAO (1.46 mol / L in toluene) makes Al / Co = 2750:1. Polymerization activity: 5.62×10 6 g(PE)(mol Co) -1 h -1 , polymer molecular weight M w =1.6kg·mol -1 , molecular weight distribution M w / M n =1.9, polymer T m =123.1℃.
[0144] h) is basically the same as method c) in this example, except that 3.2 mL of the cocatalyst MAO (1.46 mol / L in toluene) makes Al / Co=3000:1. Polymerization activity: 5.02×10 6 g(PE)(mol Co) -1 h -1 , polymer molecular weight M w =2.0kg·mol -1 , molecular weight distribution M w / M n =2.1, polymer T m =124.4℃.
[0145] Example 12: Co-catalyzed ethylene polymerization under high pressure by complex Co-2 and co-catalyst MAO
[0146] Basically the same as Example 11b), except that the main catalyst is Co-2. Polymerization activity: 4.6×10 6 g(PE)(molCo) -1 h -1 , polymer molecular weight M w =8.0kg·mol -1 , molecular weight distribution M w / M n =3.4, polymer T m =125.7℃.
[0147] Example 13: Co-catalyzed ethylene polymerization under high pressure by complex Co-3 and co-catalyst MAO
[0148] Basically the same as Example 11b), except that the main catalyst is Co-3. Polymerization activity: 1.4×10 6 g(PE)(molCo) -1 h -1 , polymer molecular weight M w =8.1kg·mol -1 , molecular weight distribution M w / M n =3.5, polymer T m =126.1℃.
[0149] Example 14: Co-catalyzed ethylene polymerization under high pressure by complex Co-4 and co-catalyst MAO
[0150] Basically the same as Example 11b), except that the main catalyst is Co-4. Polymerization activity: 4.9×10 6 g(PE)(molCo) -1 h -1, polymer molecular weight M w =3.0kg·mol -1 , molecular weight distribution M w / M n =2.3, polymer T m =124.6℃.
[0151] Example 15: Co-catalyzed ethylene polymerization under high pressure by complex Co-5 and co-catalyst MAO
[0152] Basically the same as Example 11b), except that the main catalyst is Co-5. This catalytic combination has no catalytic activity for ethylene polymerization.
[0153] Example 16 Complex Co-1 and co-catalyst MMAO jointly catalyze ethylene polymerization under high pressure
[0154] a) In an ethylene atmosphere, 25 mL of a toluene solution of catalyst Co-1 (1.5 μmol) was injected into a 250 mL stainless steel autoclave equipped with mechanical stirring, followed by the addition of 25 mL toluene, the required amount of 1.5 mL of co-catalyst MMAO (2.00 mol / L in n-hexane), and the addition of toluene to make the total volume of the solvent 100 mL. At this time, Al / Co = 2000:1. Mechanical stirring was started and maintained at 400 rpm. When the polymerization temperature reached 30°C, ethylene was charged into the reactor and the polymerization reaction began. The ethylene pressure was maintained at 10 atm at 30°C and the polymerization reaction was stirred for 30 min. The reaction solution was neutralized with an ethanol solution acidified with 10% hydrochloric acid to obtain a polymer precipitate, which was washed several times with ethanol and dried at 60°C in vacuum to constant weight. 0.6 g of polymer was weighed, and the polymerization activity was: 0.7×10 6 g(PE)(mol Co) -1 h -1 The molecular weight of the obtained polymer is M w =4.7 kg·mol -1 , molecular weight distribution M w / M n =4.6(M w is the weight average molecular weight of the polymer, M n is the number average molecular weight of the polymer, obtained by GPC test), polymer T m =124.5℃(T m is the melting temperature of the polymer, measured by DSC).
[0155] b) is basically the same as method a) in this embodiment, except that the polymerization temperature is 40°C. Polymerization activity: 3.6×10 6 g(PE)(mol Co) -1 h -1 , polymer molecular weight Mw =3.2kg·mol -1 , molecular weight distribution M w / M n =4.3, polymer T m =122.7℃.
[0156] c) is basically the same as method a) in this embodiment, except that the polymerization temperature is 50°C. Polymerization activity: 2.3×10 6 g(PE)(mol Co) -1 h -1 , polymer molecular weight M w =2.2kg·mol -1 , molecular weight distribution M w / M n =2.8, polymer T m =123.5℃.
[0157] d) is basically the same as method a) in this embodiment, except that the polymerization temperature is 60°C. Polymerization activity: 2.3×10 6 g(PE)(mol Co) -1 h -1 , polymer molecular weight M w =1.2kg·mol -1 , molecular weight distribution M w / M n =1.7, polymer T m =121.9℃.
[0158] e) is basically the same as method a) in this embodiment, except that the polymerization temperature is 70°C. Polymerization activity: 2.2×10 6 g(PE)(mol Co) -1 h -1 , polymer molecular weight M w =1.1kg·mol -1 , molecular weight distribution M w / M n =1.7, polymer T m =120.6℃.
[0159] f) is basically the same as method b) in this example, except that 0.8 mL of the cocatalyst MMAO (2.00 mol / L in n-hexane) makes Al / Co = 1000:1. Polymerization activity: 4.1×10 6 g(PE)(mol Co) -1 h -1 , polymer molecular weight M w =1.2kg·mol -1 , molecular weight distribution M w / M n =2.1, polymer T m =122.4℃.
[0160] g) is basically the same as method b) in this example, except that 0.9 mL of the cocatalyst MMAO (2.00 mol / L in n-hexane) makes Al / Co = 1250:1. Polymerization activity: 4.3×10 6 g(PE)(mol Co) -1 h -1 , polymer molecular weight M w =1.3kg·mol -1 , molecular weight distribution M w / M n =1.8, polymer T m =122.5℃.
[0161] h) is basically the same as method b) in this example, except that 1.1 mL of the cocatalyst MMAO (2.00 mol / L in n-hexane) is used to make Al / Co = 1500:1. Polymerization activity: 10.9×10 6 g(PE)(mol Co) -1 h -1 , polymer molecular weight M w =6.4kg·mol -1 , molecular weight distribution M w / M n =3.0, polymer T m =128.0℃.
[0162] i) is basically the same as method b) in this example, except that 1.3 mL of the cocatalyst MMAO (2.00 mol / L in n-hexane) makes Al / Co = 1750:1. Polymerization activity: 5.5×10 6 g(PE)(mol Co) -1 h -1 , polymer molecular weight M w =1.2kg·mol -1 , molecular weight distribution M w / M n =2.3, polymer T m =121.8℃.
[0163] Example 17: Co-catalyzed ethylene polymerization under high pressure by complex Co-2 and co-catalyst MMAO
[0164] Basically the same as Example 16i), except that the main catalyst is Co-2. Polymerization activity: 3.1×10 6 g(PE)(molCo) -1 h-1 , polymer molecular weight M w =4.4 kg·mol -1 , molecular weight distribution M w / M n =3.0, polymer T m =125.4℃.
[0165] Example 18: Co-catalyzed ethylene polymerization under high pressure by complex Co-3 and co-catalyst MMAO
[0166] Basically the same as Example 16i), except that the main catalyst is Co-3. Polymerization activity: 2.5×10 6 g(PE)(molCo) -1 h -1 , polymer molecular weight M w =8.0kg·mol -1 , molecular weight distribution M w / M n =5.7, polymer T m =128.6℃.
[0167] Example 19: Co-catalyzed ethylene polymerization under high pressure by complex Co-4 and co-catalyst MAO
[0168] Basically the same as Example 16i), except that the main catalyst is Co-4. Polymerization activity: 4.5×10 6 g(PE)(molCo) -1 h -1 , polymer molecular weight M w =3.6 kg·mol -1 , molecular weight distribution M w / M n =4.3, polymer T m =123.5℃.
[0169] Example 20: Co-catalyzed ethylene polymerization under high pressure by complex Co-5 and co-catalyst MMAO
[0170] Basically the same as Example 16i), except that the main catalyst is Co-5. This catalytic combination has no catalytic activity for ethylene polymerization.
[0171] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.
Claims
1. A transition metal cobalt complex, characterized in that: Having a structure as shown in formula (I): wherein each X is the same or different and is independently selected from F, Cl, Br, I; R 1 , R 2 , R 3 , R 4 , R 5 The same or different, each independently selected from one or more R a Substituted with the following groups: H, C 1-6 Alkyl, C 1-6 Alkoxy, C 6-20 Aryl or C 6-20 Heteroatom aromatic group; R a Selected from H, F, Cl, Br, I, C 1-6 Alkyl, C 1-6 Alkoxy, C 3-10 Heterocyclic group, C 6-20 Aryl or C 6-20 heteroatom aromatic, and each R a Same or different.
2. The transition metal cobalt complex according to claim 1, characterized in that In formula (I), R 1 Selected from C 1-3 Alkyl and Cl; more preferably methyl.
3. The transition metal cobalt complex according to claim 1, characterized in that In formula (I), R 2 Selected from C 1-3 Alkyl and Cl; more preferably methyl.
4. The transition metal cobalt complex according to claim 1, characterized in that In formula (I), R 3 , R 4 The same or different, each independently selected from H and C 1-6 Alkyl; more preferably all are H.
5. The transition metal cobalt complex according to claim 1, characterized in that In formula (I), R 1 =R 2 =Me, X is Cl, R 3 , R 4 , R 5 All are H; or R 1 =R 2 =Et, X is Cl, R 3 , R 4 , R 5 All are H; or R 1 =R 2 =iPr, X is Cl, R 3 , R 4 , R 5 All are H; or R 1 =Me, R 2 =Et, X is Cl, R 3 , R 4 , R 5 All are H; or R 1 =R 2 =Cl, X is Cl, R 3 , R 4 , R 5 Both are H.
6. The method for preparing the transition metal cobalt complex according to any one of claims 1 to 5, characterized in that: The following steps are involved: The aniline compound represented by formula (II) is subjected to condensation reaction with 2-acetylpyridine and compound CoX2 to obtain a metal complex represented by formula (I); wherein each X is the same or different and is independently selected from F, Cl, Br, I; R 1 , R 2 , R 3 , R 4 , R 5 The same or different, each independently selected from one or more R a Substituted with the following groups: H, C 1-6 Alkyl, C 1-6 Alkoxy, C 6-20 Aryl or C 6-20 Heteroatom aromatic group; R a Selected from H, F, Cl, Br, I, C 1-6 Alkyl, C 1-6 Alkoxy, C 3-10 Heterocyclic group, C 6-20 Aryl or C 6-20 heteroatom aromatic, and each R a Same or different.
7. The preparation method according to claim 6, characterized in that: The condensation reaction is carried out under anaerobic conditions.
8. The preparation method according to claim 6, characterized in that: The condensation reaction is carried out under the catalysis of an organic acid; the organic acid is one or more of formic acid, acetic acid and p-toluenesulfonic acid, preferably acetic acid.
9. The preparation method according to claim 6, characterized in that: The condensation reaction is carried out under heating reflux for 6 to 12 hours, preferably 8 to 10 hours.
10. The preparation method according to claim 6, characterized in that: The molar ratio of the compound CoX2 to the aniline compound represented by the formula (II) is 1:2-3, preferably 1:2-2.5, and more preferably 1:2.
5.
11. The preparation method according to claim 6, characterized in that: The method further comprises the step of purifying the obtained metal complex represented by formula (I), wherein the purification method comprises the following steps: A) removing volatile substances from the metal complex represented by formula (I) to obtain a concentrated solution, and adding the concentrated solution into an organic solvent for precipitation; b) subjecting the material precipitated in step a) to solid-liquid separation, washing the solid phase with an organic solvent and drying it. Wherein, the organic solvent is an anhydrous organic solvent.
12. A catalyst composition, characterized in that It comprises a main catalyst and, optionally, a co-catalyst, wherein the main catalyst is the transition metal cobalt complex according to any one of claims 1 to 5, and the co-catalyst is one or more of aluminoxane, alkylaluminum and alkylaluminum chloride.
13. The catalyst composition according to claim 12, characterized in that The aluminoxane is methylaluminoxane and / or triisobutylaluminum-modified methylaluminoxane; the alkyl group in the alkylaluminum and alkylaluminum chloride is selected from C 1-3 Alkyl; the alkylaluminum chloride is preferably diethylaluminum chloride and / or dimethylaluminum chloride.
14. The catalyst composition according to claim 12, characterized in that The molar ratio of the metal Al in the co-catalyst to the central metal Co in the transition metal cobalt complex is (500-4000):1, and the preferred molar ratio is (1000-3500):
1.
15. The catalyst composition according to claim 14, characterized in that When the co-catalyst is methylaluminoxane, the molar ratio of the metal Al in the methylaluminoxane to the central metal Co in the transition metal cobalt complex is (2000-3000):1, and the more preferred molar ratio is 2500:1; When the co-catalyst is triisobutylaluminum-modified methylaluminoxane, the molar ratio of the metal Al in the triisobutylaluminum-modified methylaluminoxane to the central metal Co in the transition metal cobalt complex is (1000-2500):1, and the more preferred molar ratio is 1750:1; When the co-catalyst is alkyl aluminum, the molar ratio of the metal Al in the alkyl aluminum to the central metal Co in the transition metal cobalt complex is (200-2000):1; When the co-catalyst is alkylaluminum chloride, the molar ratio of metal Al in the alkylaluminum chloride to the central metal Co in the transition metal cobalt complex is (200-2000):1;.
16. Use of the transition metal cobalt complex according to any one of claims 1 to 5 or the catalyst composition according to any one of claims 12 to 15 in catalyzing olefin polymerization reactions.