Cyanoethylated cellulose nanocrystal and preparation method thereof

By using sodium hydroxide and sulfuric acid to treat cellulose nanocrystals in the preparation of cyanoethylated cellulose nanocrystals, and reacting with acrylonitrile under low temperature conditions, the problems of structural destruction and crystallinity decrease of cellulose nanocrystals were solved and achieved Efficient cyanoethylation substitution and crystallinity control were achieved to prepare cyanoethylated cellulose nanocrystals with good biocompatibility.

CN118725149APending Publication Date: 2024-10-01CHONGQING LIHONG FINE CHEM +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410967339.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing preparation method of cyanoethylated cellulose nanocrystals cannot retain the rod-like structure of cellulose nanocrystals, resulting in a serious decrease in crystallinity and uneven reaction problems.

Method used

The cotton linters are treated with alkali with sodium hydroxide, and acid hydrolyzed with sulfuric acid. After centrifugal washing, dialysis and freeze-drying, an alkaline aqueous solvent and acrylonitrile are used to perform a cyanoethylation reaction under low temperature conditions, and the reaction temperature and time are controlled. Multiple washing and drying by magnetic stirring and dialysis bags ensure high crystallinity and substitution degree of cellulose nanocrystals.

Benefits of technology

It is possible to retain the rod-like structure and high crystallinity of cellulose nanocrystals under mild reaction conditions, control the degree of cyanoethylation substitution, avoid the occurrence of hydrolysis reactions, and prepare cyanoethyl cyanoethyl with good biocompatibility and environmental friendliness. cellulose nanocrystals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725149A_ABST
    Figure CN118725149A_ABST
Patent Text Reader

Abstract

The preparation method comprises the following steps: S1, preparing a cellulose nanocrystal aqueous suspension, and carrying out freeze drying, grinding and other operations to obtain cellulose nanocrystal powder; s2, redispersing the powder by using an alkaline solvent to obtain a cellulose nanocrystal aqueous suspension; s3, based on a Michael addition reaction, acrylonitrile and hydroxyl on the surface of the cellulose nanocrystal are subjected to a nucleophilic addition reaction, the nucleophilic property of the hydroxyl on the surface of the CNC can be enhanced by increasing the concentration of sodium hydroxide, the reaction activity of the hydroxyl and electron-deficient double bonds in acrylonitrile is enhanced, the reaction is promoted, the addition amount of the acrylonitrile is further accurately measured, and the content of the cellulose nanocrystal in the CNC is increased. The ratio of acrylonitrile to CNC surface hydroxyl in the reaction is controlled, gradient control and crystal form control of the cellulose nanocrystal surface cyanoethyl substitution degree are achieved, and the method has the advantages of being simple in step, low in reagent price, easy in condition control, mild in reaction condition, adjustable in substitution degree and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nano composite materials and relates to cyanoethylated cellulose nanocrystal and a preparation method thereof. Background Art

[0002] Cellulose nanocrystals (CNC) are a new material made from cellulose with high purity, high polymerization degree, high crystallinity and high hydrophilicity. In view of the problems existing in the application of CNC, surface modification of CNC not only improves its dispersibility in different solvents, but also increases its new properties, such as adhesion, high water absorption or hydrophobicity, oil repellency, flame retardancy, acid resistance and ion exchange performance.

[0003] With the development of nanotechnology, cellulose nanocrystals, as a nanostructured form of cellulose, have excellent mechanical, optical, electrochemical and other properties due to their small size, large specific surface area, special structure and other characteristics, and have shown great application potential in the fields of biomedicine, nanocomposites, etc. Therefore, chemical modification reactions continue to play an important role in improving the utilization rate of cellulose nanocrystals in polymer materials. ECNCs with high DS values ​​have unusual dielectric properties, namely high dielectric constants and relatively low dielectric loss factors, and can be used as excellent electromechanical materials, such as solid gel electrolytes, battery separators and other materials.

[0004] The traditional preparation conditions of cyanoethylated cellulose make the cyanoethylated cellulose difficult to process, with very large losses and cannot be processed uniformly and effectively. At the same time, the presence of alkaline conditions mixed with urea and NaOH will destroy the crystal structure of CNC. Urea is not used to prevent the disintegration, dissolution and even degradation of CNC particle crystals. The purpose of controlling the reaction temperature to a low temperature and limiting the time to less than 3 hours is also to prevent the destruction of the CNC structure. In addition, the high reaction temperature and its coupling with the alkaline solution will seriously damage the CNC structure. The increase in reaction time and temperature may be conducive to substitution, and it is easy to destroy the CNC structure while promoting the occurrence of hydrolysis reactions, resulting in extremely low substitution degree. Therefore, a method for preparing cyanoethylated cellulose nanocrystals under mild reaction conditions is needed to balance the highest substitution effect without destroying CNC. Summary of the invention

[0005] In view of this, in order to solve the problems of the existing cyanoethylated cellulose nanocrystal preparation method that the rod-like structure of the cellulose nanocrystal cannot be retained, the crystallinity is seriously reduced, and the reaction is unbalanced, the present invention provides a cyanoethylated cellulose nanocrystal and a preparation method thereof, wherein cotton linters are subjected to alkali treatment with sodium hydroxide, the cotton linters are subjected to acid hydrolysis with sulfuric acid, the CNC is prepared after centrifugal washing, dialysis and freeze-drying, and the influence of alkaline conditions on the crystallinity of cellulose nanocrystals, and the influence of the molar stoichiometric ratio of acrylonitrile to the surface hydroxyl groups of cellulose nanocrystals on the degree of cyanoethylation substitution of cellulose nanocrystals and its mechanism are explored.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing cyanoethylated cellulose nanocrystals comprises the following steps:

[0008] S1, treating cotton linters with alkali and acid respectively to remove amorphous regions in cellulose, followed by multiple centrifugal washing and dialysis treatments to obtain an aqueous suspension of cellulose nanocrystals, freeze-drying the cellulose nanocrystal suspension and grinding it to obtain cellulose nanocrystal (CNC) powder;

[0009] S2, the cellulose nanocrystal powder prepared in step S1 is dispersed to 1.0-1.5 mol / LOH - A cellulose nanocrystal aqueous suspension was prepared in an alkaline aqueous solvent of a certain concentration, and the nucleophilicity of the hydroxyl groups on the surface of CNC was enhanced by increasing the concentration of the alkaline aqueous solvent.

[0010] S3, adding the aqueous suspension of cellulose nanocrystals prepared in step S2 and the acrylonitrile solution into a reaction bottle in a molar ratio of cellulose nanocrystals to acrylonitrile of 1:(10-40), reacting for 2-3 hours at a temperature of 5°C to 10°C with magnetic stirring at 200-350r / min to achieve gradient control of the degree of cyanoethyl substitution on the surface of the cellulose nanocrystals and crystal form control; after the reaction is completed, adding 50mL of distilled water for redispersion to terminate the reaction, and adding acetic acid to adjust the pH to 6-7 to prevent hydrolysis of the reaction;

[0011] S4, washing the reaction product in step S3 by centrifugation for multiple times, dialyzing it using a dialysis bag, and freeze-drying it to obtain cyanoethylated (ECNC) powder;

[0012] S5. Use polycrystalline X-ray powder diffractometer and atomic force microscope to characterize the morphology, crystal form and crystallinity of the cyanoethylated CNC powder prepared in step S4.

[0013] Furthermore, the alkaline solution used in the alkaline treatment in step S1 is a 1.25 mol / L NaOH aqueous solution, and the acid solution used in the acid treatment is a 64% by mass sulfuric acid aqueous solution.

[0014] Furthermore, in step S2, the alkaline aqueous solvent is a 1.0 mol / L NaOH aqueous solution.

[0015] Furthermore, the acrylonitrile solution in step S3 is an electrophilic reagent for the nucleophilic addition reaction between acrylonitrile and the hydroxyl groups on the surface of cellulose nanocrystals. The amount of acrylonitrile solution used determines the number of double bonds available for the hydroxyl groups on the surface of CNC to attack in the reaction. The molar ratio of cellulose nanocrystals to acrylonitrile is 1:20. The stirring method uses magnetic stirring. The reaction temperature is controlled in an ice bath condition, and the cyanoethylated cellulose nanocrystals are obtained by mixing.

[0016] Furthermore, the rotation speed of the centrifugal washing in step S4 is 5000-8000 r / min, and the dialysis treatment uses a dialysis bag with a molecular weight of 14000D.

[0017] Furthermore, the structural characterization in step S5 showed that the cellulose nanocrystals retained the cellulose type I crystal form after surface cyanoethylation modification, and retained the rod-like structure of the cellulose nanocrystals.

[0018] The cyanoethylated cellulose nanocrystals are prepared according to the above-mentioned cyanoethylated cellulose nanocrystal preparation method.

[0019] The beneficial effects of the present invention are:

[0020] 1. The method for preparing cyanoethylated cellulose nanocrystals disclosed in the present invention has both mild reaction conditions and high degree of substitution. The method for preparing cyanoethylated cellulose nanocrystals is that after the introduction of cyanoethyl, the rod-like structure and crystallinity of the cellulose nanocrystals are basically completely retained, and the gradient regulation of the degree of substitution is achieved; and in order to ensure that the crystal form of the cellulose nanocrystals is not destroyed, a single cyanoethylated alkaline solvent is used, and no other alkaline reagents (such as isopropanol, ethanol, urea and other substances) are added, so as to achieve high crystallinity of the cyanoethylated cellulose nanocrystals; the reaction temperature of this experiment is low, which is conducive to inhibiting the occurrence of other side reactions and preventing the hydrolysis of cyanoethyl; it can achieve the hydrolysis of cellulose nanocrystals and the cyanoethylation reaction of cellulose nanocrystals. As a nanomaterial with good biocompatibility and environmental friendliness, cyanoethylated cellulose nanocrystals have broad market prospects and application potential, and have high market competitiveness in the context of sustainable development.

[0021] 2. The preparation method of cyanoethylated cellulose nanocrystals disclosed in the present invention can enhance the nucleophilicity of the hydroxyl group on the surface of CNC by increasing the concentration of sodium hydroxide, thereby enhancing the reaction activity with the electron-deficient double bond in acrylonitrile to promote the reaction. Further, by accurately measuring the amount of acrylonitrile added and controlling the ratio of acrylonitrile to the hydroxyl group on the surface of CNC in the reaction, gradient control of the cyanoethyl substitution degree on the surface of cellulose nanocrystals and crystal form control are achieved. However, too high alkaline conditions will destroy the crystalline region of the cellulose nanocrystals, causing serious damage to their crystallinity. The present invention adopts a novel method for preparing cyanoethylated cellulose nanocrystals, while achieving high crystallinity and high substitution of cyanoethylated cellulose nanocrystals. The method has the advantages of simple steps, low price of reagents used, easy control of conditions, mild reaction conditions, and adjustable substitution degree.

[0022] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:

[0024] Figure 1 The flowchart of the preparation method of cyanoethylated cellulose nanocrystals of the present invention is as follows;

[0025] Figure 2 This is a flow chart of the reaction principle of cyanoethylated cellulose nanocrystals of the present invention;

[0026] Figure 3 This is an atomic force microscope image of the dicyanoethylated cellulose nanocrystals of the example at a microscopic scale of 4000 nm;

[0027] FIG4(a) is a Fourier transform infrared spectrometer characterization spectrum of cyanoethylated cellulose nanocrystals of Example 2; FIG4(b) is a Fourier transform infrared spectrometer characterization spectrum of cyanoethylated cellulose nanocrystals of Comparative Example 1;

[0028] Figure 5 The XRD patterns of the dicyanoethylated cellulose nanocrystals in Example 1 at different substitution degrees. DETAILED DESCRIPTION

[0029] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0030] Embodiment 1

[0031] n(-AN) / (-OH)=16.67 / 1、C NaOH =0.236M cyanoethylated cellulose nanocrystal preparation method (such as Figure 1 , Figure 2 As shown), comprising the following steps:

[0032] (1) Alkali treatment of cotton linters: 2 wt% NaOH solution was used to treat cotton linters for 12-14 h to remove lignin and hemicellulose;

[0033] (2) Preparation of sulfuric acid: 64 wt % sulfuric acid was prepared using 252 mL of 98 wt % concentrated sulfuric acid and 248 mL of distilled water in an ice bath.

[0034] (3) Place the alkali-treated cotton in step (1) in a round-bottom flask, add sulfuric acid into the round-bottom flask, and react at a temperature of 40°C-50°C with mechanical stirring at 200-350 r / min for 60-70 min. After the reaction is completed, quench the reaction with 50 mL of distilled water;

[0035] (4) The reaction product in step (3) is centrifuged and washed, dialyzed using a 14000D molecular weight dialysis bag, and freeze-dried to obtain CNC powder.

[0036] (5) 1-2 g of CNC powder from step (4) was placed in a beaker, 10-20 mL of 1.0-1.5 mol / L NaOH solution was added, and then 15.4 mL of acrylonitrile was added. The mixture was stirred at 200-300 r / min at 5-10° C. for 2-3 h. After the reaction was completed, ice water was used to quench the reaction.

[0037] (6) The reaction product of step (5) was centrifuged and washed, dialyzed using a 14000D molecular weight dialysis bag, and freeze-dried to obtain ECNC powder.

[0038] Embodiment 2

[0039] n(-AN) / (-OH)=16.67 / 1、C NaOH =1M cyanoethylated cellulose nanocrystal preparation method, comprising the following steps:

[0040] (1) Alkali treatment of cotton linters: 2 wt% NaOH solution was used to treat cotton linters for 12-14 h to remove lignin and hemicellulose;

[0041] (2) Preparation of sulfuric acid: 64 wt % sulfuric acid was prepared using 252 mL of 98 wt % concentrated sulfuric acid and 248 mL of distilled water in an ice bath.

[0042] (3) Place the alkali-treated cotton in step (1) in a round-bottom flask, add sulfuric acid into the round-bottom flask, and react at a temperature of 40°C-50°C with mechanical stirring at 200-350 r / min for 60-70 min. After the reaction is completed, quench the reaction with 50 mL of distilled water;

[0043] (4) The reaction product in step (3) is centrifuged and washed, dialyzed using a 14000D molecular weight dialysis bag, and freeze-dried to obtain CNC powder.

[0044] (5) 1-2 g of CNC powder from step (4) was placed in a beaker, 10-20 mL of 1.0-1.5 mol / L NaOH solution was added, and then 15.4 mL of acrylonitrile was added. The mixture was stirred at 200-300 r / min at 5-10° C. for 2-3 h. After the reaction was completed, ice water was used to quench the reaction.

[0045] (6) The reaction product of step (5) was centrifuged and washed, dialyzed using a 14000D molecular weight dialysis bag, and freeze-dried to obtain ECNC powder.

[0046] Comparative Example 1

[0047] Using a mixture ratio of cellulose nanocrystal (CNC) surface hydroxyl group and acrylonitrile (AN) in different molar ratios (n(-AN) / (-OH)=10 / 1), the reaction was carried out at a temperature of 5-10°C and at a speed of 200-300 r / min using magnetic stirring for 2-3 hours, and quenched with 50 mL of distilled water after the reaction was completed;

[0048] The cyanoethylated cellulose nanocrystals synthesized using this ratio (characterized by the absence of infrared characteristic peaks, not belonging to cyanoethylated cellulose nanocrystals) were not successfully synthesized because the ratio of n(-AN) / (-OH) was too small and C NaOH If the concentration is too low, the nucleophilicity of the hydroxyl groups on the CNC surface will be insufficient, and the CNC surface hydroxyl groups will not be able to fully react with acrylonitrile.

[0049] Comparative Example 2

[0050] Using a mixed solution of cellulose nanocrystal (CNC) surface hydroxyl group and acrylonitrile (AN) in different molar ratios (n(-AN) / (-OH)=34.364 / 1), the reaction was carried out at a temperature of 5-10°C and at a speed of 200-300 r / min with magnetic stirring for 2-3 hours, and quenched with 50 mL of distilled water after the reaction was completed;

[0051] The cyanoethylated cellulose nanocrystals synthesized in this comparative example (substitution degree is 60.768%, compared with Example 2 (n(-AN) / (-OH)=16.67 / 1), the substitution degree decreases when the raw material AN is nearly doubled. The reason is that the substitution degree has reached the maximum value, or as the acrylonitrile feed of CNC increases, the reaction sites of the hydroxyl groups on the surface of CNC have all reacted with AN, and the substitution degree cannot be increased any further.

[0052] Elemental analysis test of cyanoethylated cellulose nanocrystals prepared in Example 1, Example 2 and Comparative Example 1 and Comparative Example 2

[0053] The nitrogen, hydrogen, oxygen and carbon content of cyanoethylated cellulose nanocrystals prepared with different molar ratios of n(-AN) / (-OH) were measured by a fully automatic elemental analyzer. The cyanoethyl substitution degree of cyanoethylated cellulose nanocrystals under different reaction ratios was calculated, and the results are shown in Table 1. Table 1

[0054]

[0055] Figure 3 The atomic force microscope image of the cyanoethylated cellulose nanocrystals of Example 2 at a microscopic scale of 4000 nm. The AFM characterization spectrum shows that the morphology of the prepared cyanoethylated cellulose nanocrystals is the same as that of cellulose nanocrystals, which indicates that the method for preparing cyanoethylated cellulose nanocrystals can maintain the rod-like structure of CNC.

[0056] FIG4( a ) is a Fourier transform infrared spectrometer characterization spectrum of cyanoethylated cellulose nanocrystals in Example 2; Fourier transform infrared spectroscopy was used to characterize cyanoethylated cellulose nanocrystals, and a new characteristic peak of 2250 cm -1 , the corresponding stretching vibration is the characteristic absorption peak of -CN, and has a high degree of substitution;

[0057] FIG4( b ) is a Fourier transform infrared spectrometer characterization spectrum of the cyanoethylated cellulose nanocrystals of the comparative example 1; the Fourier transform infrared spectrometer characterizes the cyanoethylated cellulose nanocrystals, and no obvious characteristic peak 2250 cm -1 , corresponding to the stretching vibration of -CN, and the absorption peak is small, and the cyanoethylation effect is not significant.

[0058] Figure 5The XRD diagram of the dicyanoethylated cellulose nanocrystals in the embodiment has a crystallinity index of 83.93%. Figure 5 It can be seen from the analysis that all characteristic peaks of cellulose nanocrystals exist in the cyanoethylated cellulose nanocrystals prepared by the present invention, including (1-10), (110), (200), and (004). From the characteristic crystal peaks of XRD and the crystallinity, it can be judged that the cellulose nanocrystals maintain the cellulose type I crystal form after surface cyanoethylation modification, and retain the rod-like structure of cellulose nanocrystals.

[0059] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing cyanoethylated cellulose nanocrystals, characterized in that: The following steps are involved: S1, treating cotton linters with alkali and acid respectively to remove amorphous regions in cellulose, followed by multiple centrifugal washing and dialysis treatments to obtain an aqueous suspension of cellulose nanocrystals, freeze-drying the cellulose nanocrystal suspension and grinding it to obtain cellulose nanocrystal (CNC) powder; S2, the cellulose nanocrystal powder prepared in step S1 is dispersed to 1.0-1.5 mol / LOH - A cellulose nanocrystal aqueous suspension was prepared in an alkaline aqueous solvent of a certain concentration, and the nucleophilicity of the hydroxyl groups on the surface of CNC was enhanced by increasing the concentration of the alkaline aqueous solvent. S3, adding the aqueous suspension of cellulose nanocrystals prepared in step S2 and the acrylonitrile solution into a reaction bottle in a molar ratio of cellulose nanocrystals to acrylonitrile of 1:(10-40), reacting for 2-3 hours at a temperature of 5°C to 10°C with magnetic stirring at 200-350r / min to achieve gradient control of the degree of cyanoethyl substitution on the surface of the cellulose nanocrystals and crystal form control; after the reaction is completed, adding 50mL of distilled water for redispersion to terminate the reaction, and adding acetic acid to adjust the pH to 6-7 to prevent hydrolysis of the reaction; S4, washing the reaction product in step S3 by centrifugation for multiple times, dialyzing it using a dialysis bag, and freeze-drying it to obtain cyanoethylated (ECNC) powder; S5. Use polycrystalline X-ray powder diffractometer and atomic force microscope to characterize the morphology, crystal form and crystallinity of the cyanoethylated CNC powder prepared in step S4.

2. The method for preparing cyanoethylated cellulose nanocrystals according to claim 1, characterized in that: In step S1, the alkaline solution used for the alkaline treatment is a 1.25 mol / L NaOH aqueous solution, and the acid solution used for the acid treatment is a 64% by mass sulfuric acid aqueous solution.

3. The method for preparing cyanoethylated cellulose nanocrystals according to claim 2, characterized in that: In step S2, the alkaline aqueous solvent is a 1.0 mol / L NaOH aqueous solution.

4. The method for preparing cyanoethylated cellulose nanocrystals according to claim 3, characterized in that: The acrylonitrile solution in step S3 is an electrophilic reagent for the nucleophilic addition reaction between acrylonitrile and the surface hydroxyl groups of cellulose nanocrystals. The amount of acrylonitrile solution used determines the number of double bonds available for the hydroxyl groups on the CNC surface to attack in the reaction. The molar ratio of cellulose nanocrystals to acrylonitrile is 1:

20. The stirring method uses magnetic stirring. The reaction temperature is controlled in an ice bath condition, and the cyanoethylated cellulose nanocrystals are obtained by mixing.

5. The method for preparing cyanoethylated cellulose nanocrystals according to claim 4, characterized in that: The rotation speed of the centrifugal washing in step S4 is 5000-8000 r / min, and the dialysis treatment uses a dialysis bag with a molecular weight of 14000D.

6. The method for preparing cyanoethylated cellulose nanocrystals according to claim 5, characterized in that: The structural characterization in step S5 showed that the cellulose nanocrystals retained the cellulose type I crystal form after surface cyanoethylation modification, and retained the rod-like structure of the cellulose nanocrystals.