Self-emulsifying waterborne epoxy resin, emulsion and preparation method
By introducing a self-emulsifying water-based epoxy resin with a hydrophilic block branch structure, the problem of difficult to balance VOC and solid content in water-based epoxy resin emulsion is solved, and a water-based epoxy resin with high solid content, zero VOC and good stability is achieved. emulsion, and the preparation process is environmentally friendly and low-cost.
Patent Information
- Application Number
- CN202310335245.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult for existing water-based epoxy resin emulsions to meet the requirements of low VOC and high solid content at the same time. The presence of too much water will affect the curing speed and curing performance, and co-solvents are often added, resulting in high VOC content.
By introducing a self-emulsifying water-based epoxy resin with a hydrophilic block branch structure, and using a modifier to perform a ring-opening polymerization reaction on the epoxy resin, a block-branched self-emulsifying water-based epoxy resin is formed, which can be mixed with water without the need for a co-solvent. Emulsifies to form a high-solids, zero-VOC water-based epoxy resin emulsion.
A water-based epoxy resin emulsion with zero VOC, high solid content (up to 70% or more), small particle size, uniform dispersion, mechanical stability and freeze-thaw stability has been achieved. The preparation method is simple, low-cost, environmentally friendly and has no secondary use. pollute.
Smart Images

Figure CN118725255A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a waterborne epoxy resin, in particular to a self-emulsifying waterborne epoxy resin, and also to a waterborne epoxy resin emulsion and a preparation method, belonging to the technical field of polymer materials. Background Art
[0002] With the increasing environmental awareness of consumers, reducing VOC has become an important indicator for the sustainable development of the epoxy resin industry. In particular, in recent years, the national environmental protection department has successively issued a number of mandatory environmental regulations, with stricter VOC indicators. Green and environmentally friendly products with low VOC content have become an urgent need for the market and consumers.
[0003] Waterborne epoxy resin emulsion usually refers to a stable dispersion system prepared in the form of particles or droplets dispersed in a dispersion medium with water as the continuous phase. The solid content is generally about 50%. There are two types: external emulsification type and self-emulsification type. It has the characteristics of low VOC content. However, the presence of too much water has a great influence on the curing speed and curing performance of waterborne epoxy, so high solid content waterborne epoxy resin emulsion has become a hot spot pursued by everyone.
[0004] It is difficult to meet the requirements of low VOC and high solid content in waterborne epoxy resin emulsion. In the prior art, the content of co-solvent in waterborne epoxy resin emulsion is 5-20%, and the solid content of common high solid content waterborne epoxy resin emulsion is 55-60%. Summary of the invention
[0005] In view of the shortcomings of the prior art, the first object of the present invention is to provide a self-emulsifying waterborne epoxy resin having zero VOC content and self-emulsifying characteristics.
[0006] The second object of the present invention is to provide a waterborne epoxy resin emulsion which has no co-solvent, zero VOC content, high solid content, small particle size, uniform dispersion, and good mechanical stability, storage stability and freeze-thaw stability.
[0007] The third object of the present invention is to provide a method for preparing an aqueous epoxy resin emulsion. The method is simple to operate, low in cost, does not generate secondary pollution, and is energy-saving and environmentally friendly.
[0008] In order to achieve the above technical objectives, the present invention provides a self-emulsifying waterborne epoxy resin, characterized in that it has the following structural expression:
[0009]
[0010] Where R is -H or -CH3, and the structural expression of R' is
[0011]
[0012] or
[0013] or
[0014] or
[0015] x=2~10, y=2~40, n=0~5.
[0016] The waterborne epoxy resin in the present invention contains hydrophilic block branches in its structure, so it has the characteristic of self-emulsification.
[0017] As a preferred solution, the molecular weight of the self-emulsifying waterborne epoxy resin is no more than 6,000.
[0018] The present invention also provides a water-based epoxy resin emulsion, which comprises the self-emulsifying water-based epoxy resin and water.
[0019] Since the waterborne epoxy resin structure contains hydrophilic block branches, the block branched hydrophilic structure makes the emulsification process easier to achieve than a simple block hydrophilic structure, so it can be mixed with water and emulsified to form a 0VOC high-solid content emulsion without a co-solvent.
[0020] As a preferred solution, the content of the self-emulsifying waterborne epoxy resin is 55-75wt%.
[0021] The invention also provides a method for preparing a water-based epoxy resin emulsion, which comprises the following steps: mixing an epoxy resin with a modifier to carry out a ring-opening polymerization reaction to obtain a self-emulsifying water-based epoxy resin; mixing the self-emulsifying water-based epoxy resin with water, stirring and emulsifying the emulsion; the epoxy resin comprises at least one of bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin, bisphenol F type epoxy resin and phenolic epoxy resin; and the modifier comprises at least one of JEFFAMINEM-2070, JEFFAMINE M-2095 and MEP-1207.
[0022] The present invention modifies the epoxy resin by a modifier, thereby opening the epoxy resin ring and introducing a hydrophilic segment in the epoxy resin structure in the form of a branched chain to form a block branched self-emulsifying waterborne epoxy resin, so that the waterborne epoxy resin emulsion with good stability and high solid content can be obtained by adding water for emulsification without adding a co-solvent.
[0023] As a preferred solution, the molecular weight of the bisphenol A epoxy resin is no more than 1500.
[0024] As a preferred solution, the mass ratio of the epoxy resin to the modifier is 80-95:5-20. Controlling the amount of the modifier within a suitable range is conducive to obtaining a self-emulsifying waterborne epoxy resin with excellent performance. If the amount is too small, the ideal emulsification effect cannot be achieved, the emulsion stability is not good enough, and it is easy to stratify for a long time. If the amount is too large, the hydrophilicity of the modified resin is too strong, which affects the water resistance of the product.
[0025] As a preferred solution, the conditions for the ring-opening polymerization reaction are: temperature of 70-100° C. and time of 1.5-6 h.
[0026] As a preferred solution, the mass ratio of the self-emulsifying waterborne epoxy resin to water is 55-75:25-45.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] (1) The obtained waterborne epoxy resin has the characteristics of self-emulsification and stable structure;
[0029] (2) The water-based epoxy resin emulsion has no co-solvent, has zero VOC content, and can have a solid content of more than 70%. It has a small particle size, with an average particle size of less than 0.5 microns, is evenly dispersed, and has good mechanical stability, storage stability, and freeze-thaw stability. Among them, at room temperature, it does not stratify or settle when centrifuged at 4000 rpm for 30 minutes; it does not stratify or settle when stored indoors at room temperature for 2 years; and it can recover to its original state after being stored at -20 to 30°C for one week and then transferred to room temperature for one day;
[0030] (3) The preparation method is simple, low-cost, does not produce secondary pollution, and is energy-saving and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a particle size distribution diagram of the waterborne epoxy resin emulsion prepared in Example 1 of the present invention.
[0032] Figure 2 This is a particle size distribution diagram of the water-based epoxy resin emulsion prepared in Example 2 of the present invention.
[0033] Figure 3 This is a particle size distribution diagram of the waterborne epoxy resin emulsion prepared in Example 3 of the present invention.
[0034] Figure 4 This is a particle size distribution diagram of the water-based epoxy resin emulsion prepared in Example 4 of the present invention. DETAILED DESCRIPTION
[0035] The present invention is further described in detail below in conjunction with the embodiments, but is not limited thereto. Of course, this cannot be used to limit the scope of the present invention, and therefore equivalent changes made according to the claims of the present invention still fall within the scope covered by the present invention.
[0036] The modifier MEP-1207 in the present invention is purchased from Wuxi Akeli Technology Co., Ltd.
[0037] Example 1
[0038] The synthetic raw materials of the block branched self-emulsifying waterborne epoxy resin in this embodiment are configured according to the following mass parts:
[0039] 20wt% phenolic epoxy resin;
[0040] 67wt% bisphenol F epoxy resin;
[0041] 8wt% JEFFAMINEM-2095;
[0042] 5wt%MEP-1207.
[0043] Among them, the phenolic epoxy resin is NPPN-638S produced by Nanya Electronic Materials (Kunshan) Co., Ltd., and the bisphenol F epoxy resin is NPEF-170 produced by Nanya Electronic Materials (Kunshan) Co., Ltd.
[0044] The 0VOC high solid content waterborne epoxy resin emulsion in this embodiment comprises the following components in parts by weight:
[0045] Block branched self-emulsifying waterborne epoxy resin 58%;
[0046] Deionized water 42%.
[0047] The following is the preparation process of 0VOC high solid content water-based epoxy resin emulsion:
[0048] (1) Novolac epoxy resin NPPN-638S, bisphenol F epoxy resin, JEFFAMINEM-2095, and MEP-1207 were added into a reaction kettle at once according to the above raw material ratio, heated to 100° C., and reacted for 2 hours to obtain a block branched self-emulsifying waterborne epoxy resin.
[0049] (2) The block branched self-emulsifying waterborne epoxy resin obtained in step 1 was placed in an emulsifying kettle, and deionized water in the above ratio was added at a speed of 1500 rpm for emulsification to obtain a waterborne epoxy resin emulsion with a solid content of 58%. The average particle size D50 of the emulsion was tested to be 0.233 μm.
[0050] Example 2
[0051] The synthetic raw materials of the block branched self-emulsifying waterborne epoxy resin in this embodiment are configured according to the following mass parts:
[0052] 80wt% phenolic epoxy resin;
[0053] 5wt% hydrogenated bisphenol A epoxy resin;
[0054] 15wt%JEFFAMINEM-2070.
[0055] The bisphenol A epoxy resin is CYD-128 produced by Baling Petrochemical Co., Ltd., and the hydrogenated bisphenol A epoxy resin is CYDH-300 produced by Baling Petrochemical Co., Ltd.
[0056] The 0VOC high solid content waterborne epoxy resin emulsion in this embodiment comprises the following components in parts by weight:
[0057] Block branched self-emulsifying waterborne epoxy resin 60%;
[0058] Deionized water 40%.
[0059] The following is the preparation process of 0VOC high solid content water-based epoxy resin emulsion:
[0060] (1) Bisphenol A epoxy resin E-51, hydrogenated bisphenol A epoxy resin, and JEFFAMIN E-2070 were added to a reaction kettle in the above proportions, heated to 75° C., and reacted for 5 hours to obtain a block branched self-emulsifying waterborne epoxy resin.
[0061] (2) The block branched self-emulsifying waterborne epoxy resin obtained in step 1 is placed in an emulsifying kettle, and deionized water in the above proportion is added at a speed of 800 rpm for emulsification to obtain a waterborne epoxy resin emulsion with a solid content of 60%. The average particle size D50 of the emulsion is tested to be 0.296 μm.
[0062] Example 3
[0063] The synthetic raw materials of the block branched self-emulsifying waterborne epoxy resin in this embodiment are configured according to the following mass parts:
[0064] 42wt% phenolic epoxy resin;
[0065] 50wt% hydrogenated bisphenol A epoxy resin;
[0066] 8wt% JEFFAMINEM-2095.
[0067] Among them, the phenolic epoxy resin is NPPN-631 produced by Nanya Electronic Materials (Kunshan) Co., Ltd., and the hydrogenated bisphenol A epoxy resin is CYDH-300 produced by Baling Petrochemical Co., Ltd.
[0068] The 0VOC high solid content waterborne epoxy resin emulsion in this embodiment comprises the following components in parts by weight:
[0069] Block branched self-emulsifying waterborne epoxy resin 65%;
[0070] Deionized water 35%.
[0071] The following is the preparation process of 0VOC high solid content water-based epoxy resin emulsion:
[0072] (1) Phenolic epoxy resin NPPN-631, CYDH-300 and JEFFAMINEM-2095 were added into a reaction kettle according to the above ratio, heated to 90° C., and reacted for 3.0 hours to obtain a block branched self-emulsifying waterborne epoxy resin.
[0073] (2) The block branched self-emulsifying waterborne epoxy resin obtained in step 1 is placed in an emulsifying kettle, and deionized water in the above proportion is added at a speed of 1200 rpm for emulsification to obtain a waterborne epoxy resin emulsion with a solid content of 65%. The average particle size D50 of the emulsion is tested to be 0.333 μm.
[0074] Example 4
[0075] The synthetic raw materials of the block branched self-emulsifying waterborne epoxy resin in this embodiment are configured according to the following mass parts:
[0076] 82wt% phenolic epoxy resin;
[0077] 18wt% JEFFAMINEM-2095.
[0078] Among them, the phenolic epoxy resin is NPPN-631 produced by Nanya Electronic Materials (Kunshan) Co., Ltd.
[0079] The 0VOC high solid content waterborne epoxy resin emulsion in this embodiment comprises the following components in parts by weight:
[0080] Block branched self-emulsifying waterborne epoxy resin 72%;
[0081] Deionized water 28%.
[0082] The following is the preparation process of 0VOC high solid content water-based epoxy resin emulsion:
[0083] (1) Phenolic epoxy resin NPPN-631 and JEFFAMINEM-2095 were added into a reaction kettle according to the above ratio, heated to 85°C, and reacted for 3.5 hours to obtain a block branched self-emulsifying waterborne epoxy resin.
[0084] (2) The block branched self-emulsifying waterborne epoxy resin obtained in step 1 was placed in an emulsifying kettle, and deionized water in the above proportion was added at a speed of 1000 rpm for emulsification to obtain a waterborne epoxy resin emulsion with a solid content of 72%. The average particle size D50 of the emulsion was tested to be 0.341 μm.
[0085] The waterborne epoxy resin emulsions prepared in all embodiments of the present invention were compared with the commercially available externally emulsified waterborne epoxy resin emulsion CYDW102-W50 and the commercially available self-emulsified waterborne epoxy resin emulsion CYDW112-W50 with a block polyether hydrophilic structure. The results are shown in Table 1.
[0086] Table 1
[0087]
[0088]
[0089] As can be seen from Table 1, the solid content, stability and low temperature resistance of the waterborne epoxy resin emulsion of the present invention are significantly higher than those of CYDW102-W50 and CYDW112-W50, and the co-solvent content is 0, which is significantly lower than that of CYDW102-W50 and CYDW112-W50.
Claims
1. A self-emulsifying waterborne epoxy resin, characterized in that: With the following structural expression: Where R is -H or -CH3, and the structural expression of R' is x=2~10, y=2~40, n=0~5.
2. A self-emulsifying waterborne epoxy resin according to claim 1, characterized in that: The molecular weight of the self-emulsifying waterborne epoxy resin is no more than 6,000.
3. A water-based epoxy resin emulsion, characterized in that: The invention comprises the self-emulsifying waterborne epoxy resin according to claim 1 or 2 and water.
4. A water-based epoxy resin emulsion according to claim 3, characterized in that: The content of the self-emulsifying waterborne epoxy resin is 55-75wt%.
5. The method for preparing a water-based epoxy resin emulsion according to claim 3 or 4, characterized in that: The epoxy resin and the modifier are mixed to carry out a ring-opening polymerization reaction to obtain a self-emulsifying waterborne epoxy resin; the self-emulsifying waterborne epoxy resin is mixed with water and stirred for emulsification to obtain; The epoxy resin includes at least one of bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin, bisphenol F epoxy resin, and novolac epoxy resin; The modifier includes at least one of JEFFAMINEM-2070, JEFFAMINE M-2095 and MEP-1207.
6. The method for preparing an aqueous epoxy resin emulsion according to claim 5, characterized in that: The molecular weight of the bisphenol A epoxy resin is no more than 1500.
7. The method for preparing an aqueous epoxy resin emulsion according to claim 5, characterized in that: The mass ratio of the epoxy resin to the modifier is 80-95:5-20.
8. The method for preparing a waterborne epoxy resin emulsion according to any one of claims 5 to 7, characterized in that: The conditions of the ring-opening polymerization reaction are: temperature of 70-100° C. and time of 1.5-6 hours.
9. The method for preparing a waterborne epoxy resin emulsion according to claim 5, characterized in that: The mass ratio of the self-emulsifying waterborne epoxy resin to water is 55-75:25-45.
Citation Information
Patent Citations
Diluent-free self-emulsifying waterborne epoxy resin emulsion and preparation method thereof
CN101955589A
Low-VOC (Volatile Organic Compound) self-emulsifying solid epoxy resin water-based emulsion and preparation method thereof
CN101974162A
Non-ionic aqueous epoxy resin emulsion and its preparation method
CN102229701A
Special waterborne epoxy emulsion for stoving varnish and preparation method thereof
CN111647175A
Waterborne epoxy emulsifier, preparation method and application thereof
CN113896896A
Cited By
Solvent-free waterborne epoxy film forming matter as well as preparation method and application thereof
CN121064488A