Fluorine-containing high-frequency low-dielectric low-moisture-absorption high-temperature-resistant resin as well as preparation method and application thereof
Through self-made phenol-cyanogen halide synthesis technology containing fluorinated bisphenol, a high-frequency, low-dielectric, low-hygroscopic, high-temperature-resistant cyanate ester resin was prepared, which solved the problems of performance degradation and process complexity in the existing technology, and achieved Cyanate ester resin with high frequency, low dielectric, low moisture absorption and heat resistance is suitable for high frequency applications in aerospace and electronic information fields.
Patent Information
- Application Number
- CN202410935272.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-01
AI Technical Summary
While the existing low-dielectric cyanate resin preparation method reduces the dielectric constant and loss tangent, it will also lead to a decrease in other properties of the resin matrix. The process is complex and difficult to produce stably, and cannot meet the needs of high-end products in the aerospace and electronic information fields. The requirements include low frequency dielectric, low moisture absorption and high temperature resistance.
Using self-made fluorine-containing, low-molecular polarization density bisphenol through the 'phenol-cyanogen halide method' synthesis technology, a high-frequency, low-dielectric, low-hygroscopic, high-temperature-resistant cyanate ester resin is prepared. By regulating the reaction conditions and catalyst dripping speed, Ensure the reaction temperature and yield, and obtain cyanate ester resin with excellent dielectric properties and heat resistance.
A cyanate ester resin with low molecular polarization density, high frequency, low dielectric, low moisture absorption and high temperature resistance is realized. It has low dielectric constant and loss tangent. It is suitable for the resin matrix of wave-transmitting composite materials and improves the performance of radar radomes. , manufacturing performance of copper-clad laminates and HDI laminated films.
Smart Images

Figure BDA0004941129390000031 
Figure BDA0004941129390000041 
Figure BDA0004941129390000051
Abstract
Description
Technical Field
[0001] The present invention relates to a low-dielectric, low-hygroscopic, high-temperature-resistant cyanate resin matrix for radar antenna covers, copper-clad boards and high-density interconnect (HDI) laminate films and a preparation method thereof, belonging to the technical field of functional polymer materials. Background Art
[0002] Low dielectric resin matrix is a key material for the manufacture of products such as radar antenna covers in the aerospace field, copper clad laminates and HDI laminated films in the electronic information field. As far as weapon radar antenna covers are concerned, with the continuous development of modern radar technology, the precision and accuracy of its detection are getting higher and higher. In order to ensure that the radar antenna system can fully exert its effectiveness, the wave-transmitting composite material is required to have a high wave transmittance, that is, the composite material is required to have a low dielectric constant (ε) and loss tangent (tanδ). In addition, it should also meet the requirements of low moisture absorption and heat resistance under extreme use environments. The dielectric properties, moisture absorption rate and heat resistance of composite materials depend to a large extent on the resin matrix. As far as the manufacture of copper clad laminates and HDI laminated films is concerned, the higher the dielectric constant and loss tangent values, the slower the signal transmission efficiency and the greater the loss. As communication technology continues to develop towards high-frequency bands, the transmission band frequency is high, the wavelength is short, the diffraction ability is poor, and the signal transmission attenuation is large under high-frequency transmission conditions, which requires a resin matrix with a broadband low dielectric constant and low loss tangent. It can be seen that the fields of aerospace, electronic information, etc. are in urgent need of high-frequency, low-dielectric, low-hygroscopic, and high-temperature resistant resin matrices.
[0003] Compared with phenolic resin, epoxy resin and bismaleimide resin, cyanate resin forms a highly symmetrical cross-linked triazine ring structure after curing, which gives it excellent dielectric properties (dielectric constant 2.85-3.20, loss tangent ≤0.012), high temperature resistance, low moisture absorption rate and shrinkage rate. It is considered to be an "ideal radar antenna cover resin matrix" and is also widely used as a copper clad laminate and HDI laminate film resin matrix. The development of high-frequency low-dielectric cyanate resin has been widely reported. ZL201610880331.8 reported a low dielectric cyanate modified resin and its preparation method. Using m-trifluoromethylphenol mTFMP and epichlorohydrin ECH as raw materials, a low dielectric fluorine-containing compound 2-((3-(trifluoromethyl)phenoxy)methyl)ethylene oxide mTFMPMO was prepared by alkylation reaction, and then added to the bisphenol A cyanate BADCy resin matrix to prepare a modified cyanate resin. The resin has excellent dielectric properties, outstanding mechanical properties and excellent heat resistance. The dielectric constant of the cyanate resin was reduced from 3.0 to 2.69-2.83, and the loss tangent was reduced from 8.1×10 -3 Reduced to 6.7×10 -3 ~8.0×10 -3, the bending strength is increased from 112.9MPa in the prior art to 121.8MPa-142.5MPa. ZL200810243502.1 reports a method for preparing a cyanate resin with low dielectric constant and low loss tangent. Hollow glass microspheres, silane coupling agent and catalyst are introduced into the cyanate resin matrix. Through this modification method, the dielectric constant and loss tangent of the cyanate resin are reduced, the heat resistance is improved, the mechanical properties are reduced, and the water absorption rate is reduced.
[0004] The current methods for preparing low dielectric cyanate esters are mainly copolymerization modification and introduction of hollow glass microspheres. However, these modification methods still have some problems. As for copolymerization modification, the introduction of copolymer components will reduce the dielectric constant and loss tangent of the cyanate ester resin matrix, while also reducing other properties of the resin matrix. For example, the introduction of epoxy resin modifiers will reduce the moisture and heat resistance of the cyanate ester resin. The modification of hollow glass microspheres depends largely on the dispersion of the hollow glass microsphere filler. Only when the hollow glass microspheres are evenly dispersed in the resin matrix can the modified cyanate ester present excellent comprehensive performance. Summary of the invention
[0005] Purpose of the invention: In view of the urgent need for high-frequency, low-dielectric cyanate resins in the fields of aerospace and electronic information, the present invention provides a high-frequency, low-dielectric, low-hygroscopic, high-temperature resistant cyanate resin and a synthesis method thereof. Based on homemade fluorine-containing, low molecular polarization density bisphenol, a new cyanate resin is synthesized through the "phenol-cyanogen halide method" synthesis technology, which solves the technical problems of reducing other properties of the resin matrix and process difficulties in the methods of preparing low-dielectric cyanate resins such as copolymerization modification and hollow glass microsphere filling modification.
[0006] Technical solution: In order to achieve the above-mentioned purpose, the present invention proposes a method for preparing a fluorine-containing high-frequency low-dielectric, low-hygroscopic, high-temperature resistant resin, comprising the following steps:
[0007] The first step is to dissolve bisphenol in mixed solvent I to prepare a reaction solution, and reduce the temperature of the reaction solution to ≤-15°C; the second step is to add cyanogen halide to the reaction solution, and the molar ratio of bisphenol: cyanogen halide is 1:1.8 to 1:2.2; the third step is to drop the catalyst into the reaction solution to start the reaction; the molar ratio of catalyst: cyanogen halide is 1:1, and the temperature of the reaction solution is ensured to be ≤5°C by adjusting the catalyst drop rate. After the catalyst is added, continue to keep warm for 2h to 4h until the reaction is completed; the fourth step is to pour the reaction solution into the mixed solvent II, crystals are precipitated, and then filtered and dried to obtain cyanate ester crystals; the fifth step is to place the cyanate ester crystals in a mold for curing to obtain a cyanate ester resin cured product.
[0008] Furthermore, the bisphenol is one of bisphenol T, bisphenol D and bisphenol H.
[0009] Furthermore, the mixed solvent I is any one or more of acetone, butanone, ethanol, butanol, isopropanol, dioxane, ethanol, toluene, and xylene.
[0010] Furthermore, the cyanogen halide is one or more of cyanogen bromide and cyanogen chloride.
[0011] Furthermore, the catalyst is one or more of 70% sodium hydroxide aqueous solution, diethylamine, pyridine, triethylamine, and diisopropylethylamine.
[0012] Furthermore, the mixed solvent II is one or more of ethanol, butanol and water.
[0013] A fluorine-containing high-frequency low-dielectric, low-hygroscopic, high-temperature resistant resin is a cyanate resin, which is a mixture of one or more of bisphenol D cyanate, bisphenol T cyanate and bisphenol H cyanate; its molecular structure is:
[0014]
[0015] A fluorine-containing high-frequency low-dielectric, low-hygroscopic, high-temperature resistant resin can be used as a resin matrix for wave-transmitting composite materials and is used in radar antenna covers, copper-clad plates, and laminated films.
[0016] Beneficial technical effects: The three fluorine-containing bisphenols designed and prepared by the present invention reduce the molecular polarization density by introducing fluorine atoms, thereby giving the cyanate ester product high-frequency low dielectric constant and low loss tangent characteristics; due to the low surface energy and excellent chemical inertness of fluorine atoms, the cyanate ester product is endowed with excellent environmental resistance such as chemical resistance and corrosion resistance and low moisture absorption rate; in addition, the CF bond energy is relatively high at 453kJ·mol-1, which is more stable and requires higher energy to decompose the bond. The fluorine atoms cover the CC bonds of the main chain skeleton and play a protective role, thereby improving the heat decomposition temperature and heat resistance of the cyanate ester product. Based on the three bisphenols, a cyanate ester resin with low molecular weight planning density, high frequency low dielectric, low moisture absorption and high temperature resistance is synthesized. The resin has a low dielectric constant and loss tangent, can be used as a resin matrix for wave-transmitting composite materials, and has great application prospects in the manufacturing fields of radar antenna covers, copper-clad boards, laminated films, etc. DETAILED DESCRIPTION
[0017] The present invention is further described below in conjunction with implementation cases, which are only some implementation cases or certain specific implementation forms of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0018] In view of the technical bottlenecks of current preparation methods of low dielectric cyanate resins, such as copolymerization modification and hollow filler filling modification, which exist in reducing the dielectric constant at the expense of other properties of the cyanate resin, complex processes, and difficulty in stable production, the present invention takes molecular structure design-fluorinated bisphenol synthesis-cyanate synthesis as a technical route, provides a high-frequency low dielectric, low moisture absorption, high temperature resistant cyanate resin and a synthesis method thereof, and provides a high-frequency low dielectric material foundation for the manufacture of radar antenna covers in the aerospace field and the production of copper clad laminates and HDI laminated films in the electronic information field.
[0019] The present invention designs and prepares three fluorine-containing (bisphenol T, bisphenol D and bisphenol H) low molecular polarization density bisphenols; the molecular structural formulas of the three bisphenols bisphenol T, bisphenol D and bisphenol H are:
[0020]
[0021] , three cyanate resins with low molecular weight planning density, high frequency low dielectric constant, low moisture absorption and high temperature resistance were synthesized by the "phenol-cyanogen halide" method. The three fluorinated bisphenols designed and prepared by the present invention reduce the molecular polarization density by introducing fluorine atoms, thereby giving the cyanate products high frequency low dielectric constant and low loss tangent characteristics; due to the low surface energy and excellent chemical inertness of fluorine atoms, the cyanate products are given excellent environmental resistance such as chemical resistance and corrosion resistance as well as low moisture absorption rate; in addition, the CF bond energy is relatively high at 453 kJ·mol -1 , more stable, and higher energy is required to decompose the bond. The fluorine atom covers the CC bond of the main chain skeleton and plays a protective role, thereby improving the thermal decomposition temperature and heat resistance of the cyanate ester product.
[0022] The cyanate synthesis route adopted by the present invention is:
[0023]
[0024] Specifically, the process includes the following four steps: the first step is to dissolve bisphenol in mixed solvent I to prepare a reaction solution, turn on the refrigeration and stirring system, and reduce the temperature of the reaction solution to ≤-15°C; the second step is to add cyanogen halide to the reaction solution, and the molar ratio of bisphenol to cyanogen halide is 1:1.8 to 1:2.2; the third step is to then drop a catalyst into the reaction solution to start the reaction, and the molar ratio of catalyst to cyanogen halide is 1:1. By adjusting the catalyst dropwise addition speed, the temperature of the reaction solution is ensured to be ≤5°C, and after the catalyst is added, the temperature is kept warm for 2h to 4h, and the reaction is terminated; the fourth step is to pour the reaction solution into mixed solvent II, and crystals are precipitated, and then filtered and dried to obtain cyanate ester crystals. The molecular structures of bisphenol T, bisphenol D and bisphenol H cyanate are as follows:
[0025]
[0026] Example 1
[0027] First, bisphenol D is dissolved in a mixed solvent of acetone, butanone and ethanol, the refrigeration and stirring system is turned on, the temperature of the reaction solution is lowered to -25°C, cyanogen bromide is added to the reaction solution, the molar ratio of bisphenol: cyanogen halide is 1:2, and then a composite catalyst of 70% sodium hydroxide aqueous solution, diethylamine and pyridine is added dropwise to the reaction solution to start the reaction, the molar ratio of catalyst: cyanogen halide is 1:1, the temperature of the reaction solution is always ≤5°C, after the catalyst is added dropwise, the temperature is kept warm for 2 hours, the reaction is completed, the reaction solution is poured into a mixed solvent of butanol and ethanol, crystals are precipitated, and then filtered and dried to obtain cyanate crystals.
[0028] The cyanate yield of this embodiment is 99.0%. The cyanate crystals prepared above are placed in a mold, put into an oven, and cured at 100° C., 120° C., 140° C., 160° C., 180° C., and 200° C. for 2 hours, respectively, to obtain a cyanate resin cured product, which has a glass transition temperature of 252° C. (GB / T 40396), a compressive strength of 141.0 MPa (GB / T 2567), a flexural strength of 152.0 MPa (GB / T 2570), a dielectric constant of 2.57 at 10 GHz, a dielectric loss of 0.006 (GB / T 5597), and a water absorption of 1.2% (GB / T 1462).
[0029] Example 2
[0030] First, bisphenol T is dissolved in a mixed solvent of isopropanol, acetone, dioxane and ethanol, the refrigeration and stirring system is turned on, the temperature of the reaction solution is lowered to -30°C, cyanogen chloride is added to the reaction solution, the molar ratio of bisphenol: cyanogen halide is 1:1.8, and then diisopropylethylamine is added dropwise to the reaction solution to start the reaction, the molar ratio of catalyst: cyanogen halide is 1:1, and the temperature of the reaction solution is always ≤5°C. After the catalyst is added dropwise, the temperature is kept warm for 4 hours. After the reaction is completed, the reaction solution is poured into a mixed solvent of butanol and water, crystals are precipitated, and then filtered and dried to obtain cyanate crystals.
[0031] The cyanate yield of this embodiment is 99.3%. The cyanate crystals prepared above are placed in a mold, put into an oven, and cured at 100° C., 120° C., 140° C., 160° C., 180° C., and 200° C. for 2 hours, respectively, to obtain a cyanate resin cured product, which has a glass transition temperature of 194° C. (GB / T 40396), a compressive strength of 140.7 MPa (GB / T 2567), a flexural strength of 96.0 MPa (GB / T 2570), a dielectric constant of 2.55 at 10 GHz, a dielectric loss of 0.004 (GB / T 5597), and a water absorption of 1.4% (GB / T1462).
[0032] Example 3
[0033] First, bisphenol H is dissolved in a mixed solvent of acetone, ethanol and toluene, and the refrigeration and stirring system is turned on to reduce the temperature of the reaction solution to -21°C. Cyanogen chloride and cyanogen bromide are added to the reaction solution, and the molar ratio of bisphenol: cyanogen halide is 1:2.2. Then, pyridine and triethylamine are added dropwise to the reaction solution to start the reaction. The molar ratio of catalyst: cyanogen halide is 1:1. The temperature of the reaction solution is always ≤5°C. After the catalyst is added dropwise, the temperature is kept warm for 3 hours. When the reaction is completed, the reaction solution is poured into a mixed solvent of butanol and water. Crystals are precipitated, which are then filtered and dried to obtain cyanate crystals.
[0034] The cyanate yield of this embodiment is 98.9%. The cyanate crystals prepared above are placed in a mold, put into an oven, and cured at 100° C., 120° C., 140° C., 160° C., 180° C., and 200° C. for 2 hours, respectively, to obtain a cyanate resin cured product, which has a glass transition temperature of 247° C. (GB / T 40396), a compressive strength of 151 MPa (GB / T 2567), a flexural strength of 120.0 MPa (GB / T 2570), a dielectric constant of 2.65 at 10 GHz, a dielectric loss of 0.007 (GB / T 5597), and a water absorption rate of 1.8% (GB / T1462).
[0035] Example 4
[0036] First, bisphenol D and bisphenol H are dissolved in a mixed solvent of acetone, ethanol and toluene, and the refrigeration and stirring system is turned on to reduce the temperature of the reaction solution to -21°C. Cyanogen chloride and cyanogen bromide are added to the reaction solution, and the molar ratio of bisphenol: cyanogen halide is 1:2. Subsequently, 70% sodium hydroxide aqueous solution is added to the reaction solution to start the reaction, and the molar ratio of catalyst: cyanogen halide is 1:1. The temperature of the reaction solution is always ≤5°C. After the catalyst is added dropwise, the temperature is kept warm for 4 hours. After the reaction is completed, the reaction solution is poured into a mixed solvent of ethanol and water, and crystals are precipitated. The crystals are then filtered and dried to obtain cyanate crystals.
[0037] The cyanate yield of this embodiment is 99.2%. The cyanate crystals prepared above are placed in a mold, put into an oven, and cured at 100° C., 120° C., 140° C., 160° C., 180° C., and 200° C. for 2 hours, respectively, to obtain a cyanate resin cured product, which has a glass transition temperature of 250° C. (GB / T 40396), a compressive strength of 149.0 MPa (GB / T 2567), a flexural strength of 130.0 MPa (GB / T 2570), a dielectric constant of 2.61 at 10 GHz, a dielectric loss of 0.006 (GB / T 5597), and a water absorption of 1.4% (GB / T 1462).
[0038] Example 5
[0039] First, bisphenol T and bisphenol H are dissolved in a mixed solvent of acetone, ethanol and toluene, and the refrigeration and stirring system is turned on to reduce the temperature of the reaction solution to -21°C. Cyanogen chloride and cyanogen bromide are added to the reaction solution, and the molar ratio of bisphenol: cyanogen halide is 1:1.9. Subsequently, diethylamine and triethylamine catalysts are added to the reaction solution to start the reaction, and the molar ratio of catalyst: cyanogen halide is 1:1. The temperature of the reaction solution is always ≤5°C. After the catalyst is added dropwise, the temperature is kept warm for 4 hours. After the reaction is completed, the reaction solution is poured into a mixed solvent of ethanol and water, and crystals are precipitated. The crystals are then filtered and dried to obtain cyanate crystals.
[0040] The cyanate yield of this embodiment is 99.4%. The cyanate crystals prepared above are placed in a mold, put into an oven, and cured at 100° C., 120° C., 140° C., 160° C., 180° C., and 200° C. for 2 hours, respectively, to obtain a cyanate resin cured product, which has a glass transition temperature of 250° C. (GB / T 40396), a compressive strength of 149.0 MPa (GB / T 2567), a flexural strength of 126.0 MPa (GB / T 2570), a dielectric constant of 2.64 at 10 GHz, a dielectric loss of 0.006 (GB / T 5597), and a water absorption of 1.5% (GB / T 1462).
[0041] Those skilled in the art will appreciate that, unless otherwise specifically defined, all technical terms used above have the same meanings as those generally understood by ordinary technicians in the field to which the present invention belongs; all the above specific implementation methods and specific cases further illustrate the purpose, technical solutions and beneficial technical effects of the present invention in detail. It should also be understood that the above description is only some specific implementation methods and cases of the present invention, and is not intended to limit the present invention. On the contrary, any other modifications, equivalent substitutions, improvements, etc. made within the design ideas and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a fluorine-containing high-frequency low-dielectric, low-hygroscopic, high-temperature resistant resin, characterized in that: The following steps are involved: Step 1: dissolving bisphenol in mixed solvent I to prepare a reaction solution, and lowering the temperature of the reaction solution to ≤-15°C; Step 2: Add cyanogen halide to the reaction solution, the molar ratio of bisphenol to cyanogen halide is 1:1.8 to 1:2.2; Step 3: Add the catalyst dropwise to the reaction solution to start the reaction; The molar ratio of catalyst to cyanogen halide is 1:
1. The catalyst dropping speed is adjusted to ensure that the temperature of the reaction solution is ≤5°C. After the catalyst is added, the temperature is kept for 2h to 4h until the reaction is completed. Step 4: Pour the reaction solution into the mixed solvent II, crystals are precipitated, and then filtered and dried to obtain cyanate crystals. Step 5: placing the cyanate ester crystals in a mold and curing them to obtain a cyanate ester resin cured product.
2. The method for preparing a fluorine-containing high-frequency low-dielectric, low-hygroscopic, high-temperature resistant resin according to claim 1, characterized in that: The bisphenol is one of bisphenol T, bisphenol D and bisphenol H; the molecular structure is:
3. The method for preparing a fluorine-containing high-frequency low-dielectric, low-hygroscopic, high-temperature resistant resin according to claim 1, characterized in that: The mixed solvent I is any one or more of acetone, butanone, ethanol, butanol, isopropanol, dioxane, ethanol, toluene and xylene.
4. The method for preparing a fluorine-containing high-frequency low-dielectric, low-hygroscopic, high-temperature resistant resin according to claim 1, characterized in that: The cyanogen halide is one or more of cyanogen bromide and cyanogen chloride.
5. The method for preparing a fluorine-containing high-frequency low-dielectric, low-hygroscopic, high-temperature resistant resin according to claim 1, characterized in that: The catalyst is one or more of 70% sodium hydroxide aqueous solution, diethylamine, pyridine, triethylamine and diisopropylethylamine.
6. The method for preparing a fluorine-containing high-frequency low-dielectric, low-hygroscopic, high-temperature resistant resin according to claim 1, characterized in that: The mixed solvent II is one or more of ethanol, butanol and water.
7. A fluorine-containing high-frequency low-dielectric, low-hygroscopic, high-temperature resistant resin, which is a cyanate resin, and is a mixture of one or more of bisphenol D cyanate, bisphenol T cyanate and bisphenol H cyanate; its molecular structure is:
8. A fluorine-containing high-frequency low-dielectric, low-hygroscopic, high-temperature resistant resin is used as a resin matrix for wave-transmitting composite materials and is used in radar antenna covers, copper-clad laminates, and laminated films.
Citation Information
Cited By
Preparation method of modified cyanate ester resin
CN119823573A
Low-dielectric, high-temperature-resistant and thermo-oxidative polymer and preparation method thereof
CN120842566A
Silicon-containing thermo-oxidative aging resistant cyanate ester resin and synthesis method thereof
CN120842567A
Silicon-containing heat-resistant and oxygen-aging-resistant cyanate ester resin and synthesis method thereof
CN120842567B
Ultralow dielectric and high thermal conductivity composite material based on fluorine-fluorine self-assembly and preparation method and application thereof
CN121975171A