Additive containing epoxy siloxane, anti-ionizing radiation aromatic polyester material and preparation method of anti-ionizing radiation aromatic polyester material
By using epoxy siloxane as an anti-radiation additive in aromatic polyester materials, the problems of radiation embrittlement and radiation yellowing of aromatic polyester materials under high ionizing radiation are solved, and the radiation resistance under high radiation doses is achieved. The mechanical properties are maintained and the radiation resistance toughness is improved, which has good industrial application prospects.
Patent Information
- Application Number
- CN202410973761.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-01
AI Technical Summary
Aromatic polyester materials are prone to radiation embrittlement and radiation yellowing under high ionizing radiation. Traditional anti-radiation agents cannot effectively solve this problem and aggravate the radiation yellowing phenomenon.
Fully saturated chain, high boiling point epoxy siloxane is used as the anti-radiation additive, combined with aromatic polyester materials, and aromatic polyester materials that are resistant to ionizing radiation are prepared through processes such as stirring and smelting. Epoxy siloxane additives The molecular structure does not contain aromatic hydrocarbon groups, which avoids radiation yellowing and toxicity problems.
It maintains the mechanical rigidity and toughness of the material under high radiation doses, significantly improves the radiation resistance, avoids radiation embrittlement, and has good industrial application prospects.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of radiation-resistant modification of materials, and in particular to an epoxysiloxane-containing additive, an ionizing radiation-resistant aromatic polyester material and a preparation method thereof. Background Art
[0002] When plastics and other organic polymers are exposed to ionizing radiation such as high-energy electromagnetic waves, high-energy ion currents, and high-energy electron beams, the original molecular chains will be broken by high-energy impacts, forming free radicals or ionized fragment end groups. Then, these broken chain links tend to be mainly radiolytic or mainly cross-linked, depending on the chemical structure properties. In most cases, the continuous accumulation of high radiation doses will eventually cause the overall polymer material to tend to be radiolytic, showing adverse consequences such as radiation embrittlement and radiation yellowing of the material on a macro scale. At present, the widely used radiation disinfection of imported and exported goods, radiation sterilization of medical supplies, and nuclear power plant cable equipment all encounter the ionizing radiation hazards of plastics and other polymer parts or packaging materials. Therefore, the development of radiation-resistant formulas for plastics and other polymer materials has practical significance and economic value.
[0003] Aromatic polyesters are a common class of materials in general-purpose plastics. They mainly tend to crosslink under ionizing radiation. However, due to the rigidity of the benzene ring units, excessive self-crosslinking caused by radiation makes this type of material face the problem of radiation embrittlement. Traditional benzene-containing anti-radiation additives cannot overcome this contradiction, and at the same time aggravate the radiation yellowing phenomenon caused by the presence of aromatic units in the additives. Summary of the invention
[0004] The present invention aims to provide a fully saturated chain, high boiling point, easy-to-mix anti-radiation additive system to address the shortcomings of common aromatic anti-radiation agents that are prone to radiation yellowing and radiation embrittlement under high ionizing radiation doses. Compared with other traditional anti-radiation formulations, this formulation system does not have the disadvantage of radiation yellowing, and can maintain or even improve the mechanical rigidity and toughness of aromatic polyester materials under radiation doses of several hundred kGy.
[0005] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0006] An additive, suitable for the formulation system of aromatic polyester anti-ionizing radiation, the additive is mainly composed of epoxysiloxane, wherein the additive can be selected from: 3-(2,3-epoxypropoxy)propyltrimethoxysilane, 3-(2,3-epoxypropoxy)propyltriethoxysilane, etc., any organic silicon compound with a molecular structure similar to the form of (R1O)3Si-R2-O-R3-(CHOCH)-, wherein R n represents an alkyl group, and -(CHOCH)- represents an epoxy group.
[0007] As a possible implementation, further, the aromatic polyester is a polycarboxylate containing a benzene ring functional group structure, such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polybutylene terephthalate adipate (PBAT) and other polyesters containing aromatic structures.
[0008] The present invention also provides an aromatic polyester material resistant to ionizing radiation, comprising an aromatic polyester raw material and the above-mentioned additive.
[0009] As a possible implementation, further, the epoxysiloxane is added in an amount of 0.1% to 10% relative to the total weight of the feed. The ionizing radiation resistant aromatic polyester material can withstand a processing temperature below 300 degrees and an ionizing radiation dose of at least 300 kGy.
[0010] The present invention provides a method for preparing the above-mentioned ionizing radiation resistant aromatic polyester material, comprising the following steps:
[0011] 1) Pre-drying the aromatic polyester raw material for standby use;
[0012] 2) adding epoxysiloxane to the dried pure aromatic polyester raw material and stirring to mix well;
[0013] 3) adding the mixed material to a melting device such as an internal mixer or a screw extruder, and mixing it at the internal mixing temperature of the pure raw material of the aromatic polyester to be processed until it is uniform;
[0014] 4) The material after the banburying in step 3) is crushed and then re-granulated to obtain an aromatic polyester modified masterbatch.
[0015] As a possible implementation, further, in step 2), the epoxysiloxane is added separately to the pure raw material of the aromatic polyester, or the epoxysiloxane is added to the aromatic polyester masterbatch in batches during the mixing process of step 3).
[0016] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0017] 1) The additive provided by the present invention is substantially non-toxic or low-toxic after cross-linking reaction, and the molecular structure of the additive itself does not contain aromatic hydrocarbon groups, thereby fundamentally avoiding the problems of traditional aromatic hydrocarbon anti-radiation agents that aggravate radiation yellowing and have high toxicity.
[0018] 2) The formula of the present invention is an organosilicon compound with a high boiling point and low volatility, which can reduce air pollution during the processing. At the same time, the additive molecular chain is soft, which can significantly alleviate the radiation curing brittleness of aromatic polyester caused by excessive radiation self-crosslinking and benzene ring rigidity, and can keep the mechanical tensile strength of the material basically unchanged at a radiation dose of several hundred kGy, while significantly improving the radiation resistance toughness of the aromatic polyester material, and has excellent industrial application prospects. DETAILED DESCRIPTION
[0019] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] The polyester masterbatch used in the following examples is polybutylene terephthalate adipate (PBAT), and the additive is 3-(2,3-epoxypropoxy)propyltrimethoxysilane.
[0021] The method for preparing an aromatic polyester material resistant to ionizing radiation specifically comprises the following steps:
[0022] 1) The aromatic polyester raw material is first dried in a drying equipment such as a blast dryer at 60-90°C for 1-4 hours for use. If it is not used immediately after drying, the polyester raw material is sealed in a dry state at 30-40°C. If it is stored openly, it needs to be dried again before use;
[0023] 2) Adding the additives in weight percentage relative to the total feed, wherein the epoxysiloxane addition amount is 0.1% to 10%; mixing the additives with the polyester pellets dried in the above step 1) and stirring evenly, the epoxysiloxane can be added separately to the pure raw material of the aromatic polyester, or added gradually during the subsequent mixing and kneading process.
[0024] 3) The mixed material in the above step 2) is put into a mixing equipment such as an internal mixer for internal mixing. The internal mixing temperature is set to the melting temperature of the aromatic pure raw material. The internal mixing time is 5 to 30 minutes, during which the remaining additives can be added successively.
[0025] 4) The raw materials after mixing are taken out and crushed by a plastic crusher and other equipment, and then re-granulated to obtain the final granular radiation-resistant composite material, which can be used as the masterbatch of various plastic products for anti-ionizing radiation purposes. It has good anti-ionizing radiation performance and can be used alone or blended with other plastics.
[0026] Example 1
[0027] Take 99% of polyester masterbatch (PBAT) (relative to the weight percentage of the total feed, the following percentages of ingredients have the same meaning), dry it in a blast dryer at 80 degrees for 2 hours, cool it to 30-40 degrees and take it out. Mix 1% of the additive 3-(2,3-epoxypropoxy)propyltrimethoxysilane with the dried PBAT masterbatch. Then put the mixture into a mixer and mix it at 150 degrees for 8 minutes. After the mixing is completed, take it out and put it into a plastic crusher for crushing. Put the crushed mixture into a twin-screw extruder for re-granulation. The temperature of each zone of the extruder is 130-180 degrees Celsius and the speed is 40-80r / min.
[0028] The radiation-resistant composite masterbatch finally obtained in this embodiment was injected into a dumbbell-shaped mechanical test sample to test the change of the formula on the radiation resistance of the polyester masterbatch. The test conditions were: the electron accelerator energy was 10 MeV, the temperature was room temperature (25°C), and the ambient atmosphere was exposed to ordinary air. The radiation resistance of the sample is as follows:
[0029] When the electron beam radiation dose increases from 0 kGy to 100 kGy, the tensile strength of the pure PBAT sample in the non-added group increases from about 22 MPa before irradiation to 23.5 MPa after irradiation (self-crosslinking by bulk radiation); but the tensile elongation at break decreases from about 700% before irradiation to about 630% after irradiation (radiation embrittlement); the tensile strength of the composite sample of the present embodiment increases from 21.5 MPa before irradiation to 22 MPa after irradiation, and the elongation at break increases from about 650% before irradiation to about 670% after irradiation (radiation toughening).
[0030] When the electron beam radiation dose increases from 0 kGy to 300 kGy, the tensile strength of the pure PBAT sample in the non-additive group increases from 22 MPa to 23 MPa (bulk radiation self-crosslinking), but the tensile elongation at break decreases from about 700% to about 560% (radiation embrittlement); while the sample of the composite material of this embodiment increases from 21.5 MPa to about 22 MPa, and the elongation at break increases from about 650% to about 700% (significant radiation toughening).
[0031] This compounding ratio enables the PBAT polyester material prepared in this embodiment to maintain the radiation-resistant tensile strength of the sample throughout the process within the range of high radiation dose below 300 kGy, and significantly enhances the radiation-resistant toughness of the material (the elongation at break increases significantly with the increase in radiation dosage).
[0032] Example 2
[0033] The preparation process of the radiation-resistant composite material is the same as that in Example 1, and PBAT polyester is still used as the main masterbatch, but the ratio is different. PBAT is taken at 97%, and the additive 3-(2,3-epoxypropoxy)propyltrimethoxysilane is increased to 3%. The same electron beam irradiation conditions and sample testing conditions as in Example 1 are adopted.
[0034] When the electron beam radiation dose increases from 0 kGy to 100 kGy, the tensile strength of the composite sample with this ratio increases from 25 MPa to 27 MPa, and the tensile elongation at break increases from 720% to about 740%;
[0035] When the electron beam radiation dose increases from 0 kGy to 300 kGy, the tensile strength of the composite sample with this ratio increases from 25 MPa to 28 MPa, and the tensile elongation at break increases from 720% to about 780%;
[0036] This compounding ratio did not significantly improve the tensile strength of the aromatic polyester during the radiation process, and basically maintained the mechanical strength of the compound material at all experimental radiation doses without significant change, but significantly improved the radiation toughness (elongation at break) of the compounded sample at high radiation doses.
[0037] In summary, the epoxysiloxane additives of the present invention have a significant radiation toughening effect on aromatic polyesters with similar structures to PBAT, effectively solving the embrittlement problem caused by radiation self-crosslinking of aromatic polyesters. The additive feed ratio can be adjusted for different aromatic polyester masterbatches according to actual needs.
[0038] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. An additive, It is characterized in that The invention is applicable to the formulation system of aromatic polyester for resisting ionizing radiation, and the additive is mainly composed of epoxysiloxane.
2. The polyester raw material according to claim 1, It is characterized in that The aromatic polyester is a polyester material whose molecular chain repeating unit contains a benzene ring functional group structure.
3. The additive according to claim 1, It is characterized in that The epoxysiloxane is an organic silicon compound having an epoxy group at one end of the molecular chain and an alkoxysilicon structure at the other end, and the intermediate molecular structure connecting the two ends is a saturated CC or CO chain.
4. An aromatic polyester material resistant to ionizing radiation, It is characterized in that The invention comprises an aromatic polyester and the additives according to claims 1 to 3.
5. The ionizing radiation-resistant aromatic polyester material according to claim 4, It is characterized in that The aromatic polyester masterbatch accounts for 90% to 99.9% of the total weight of the raw materials; the added amount of the epoxysiloxane is 10% to 0.1% relative to the total weight of the raw materials.
6. The ionizing radiation-resistant aromatic polyester material according to claim 5, It is characterized in that The composite material resistant to ionizing radiation can withstand processing temperatures below 300 degrees.
7. A method for preparing the ionizing radiation resistant aromatic polyester material according to any one of claims 4 to 6, It is characterized in that The steps include: 1) Pre-drying the aromatic polyester raw material for standby use; 2) adding epoxysiloxane to the dried pure aromatic polyester raw material and stirring to mix well; 3) adding the mixed material into a melting device and mixing it at the mixing temperature of the pure raw material of the aromatic polyester to be processed until it is uniform; 4) The material after the banburying in step 3) is crushed and then re-granulated to obtain an aromatic polyester modified masterbatch.
8. The method for preparing the ionizing radiation resistant aromatic polyester material according to claim 7, It is characterized in that In step 2), the epoxysiloxane is added once and mixed with the pure raw material of the aromatic polyester, or the epoxysiloxane is added several times during the mixing process of step 3).