Low-ablation-rate clean thermal insulation material and preparation method thereof
By designing a composite of rubber-resin matrix material, ablation-resistant fiber and flame retardant, a condensed phase carbon layer is constructed, which solves the problem of ablation and cleaning of thermal insulation materials, and realizes thermal insulation materials with low ablation rate and cleanliness, ensuring Ensure the normal operation of the attitude control engine.
Patent Information
- Application Number
- CN202410810980.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-01
AI Technical Summary
In the attitude-orbit-controlled solid engine, the ablation residue of the insulation material affects the cleanliness and normal operation of the gas generator. In particular, the high melting point and boiling point of silicon dioxide lead to the loss of the char layer, causing ablation problems, which are difficult to achieve with the existing technology. Effectively solve the problems of cleaning degree and ablation rate.
It is designed using a rubber-resin matrix material, combined with ablation-resistant fibers and flame retardants, and uses composite materials and thermal insulation layer interface bonding technology to design low ablation rate clean insulation materials. The formula does not contain traditional rubber reinforcing agent silica. , using aluminum-magnesium or antimony-based flame retardants and phosphate ester flame retardants to build a condensed phase carbon layer to achieve low ablation properties.
It has realized the low ablation rate and cleanliness of the thermal insulation material in the attitude orbit control engine, ensuring the normal operation of the valve core, reducing the erosion of the ablation carbon layer and the generation of residues, and meeting the thermal protection needs of the solid attitude orbit control engine.
Smart Images

Figure CN118725428A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of thermal protection of attitude and orbit control solid engines, and in particular relates to a clean insulation material with a low ablation rate and a preparation method thereof. Background Art
[0002] Thermal insulation material is a structural functional material used for thermal protection in solid rocket engines. It is a layer of heat-insulating and ablation-resistant material between the engine casing and the solid propellant. Its important role is to protect the integrity of the casing structure during the operation of the engine, and to protect the engine casing from losing strength and burning through in the environment of high temperature and high pressure gas, thereby ensuring the normal operation of the engine.
[0003] When the solid attitude and orbit control engine is working, the engine thrust needs to be continuously adjustable. As the core component of the thrust adjustment of the solid attitude and orbit control engine, the gas valve has different working modes such as single opening, double opening, and multiple opening. The valve throat diameter is generally less than 10mm and there are changes in the valve opening and closing during the working process. Therefore, the cleanliness of the combustion products is very high during the working process. The deposition of ablation residues such as propellants and insulation layers will affect the normal operation of the valve. In the attitude and orbit control gas generator, the ablation residues of the solid components are the main source of residues when the gas generator is working. For example, aluminum powder in the propellant can effectively improve the energy characteristics, but it will bring negative effects such as slag deposition and increased nozzle ablation.
[0004] Although propellant is the main source of combustion products, in recent years, many scientific research institutes at home and abroad have focused on improving the propellant formula, and have achieved breakthroughs in clean gas technology after systematic research. However, there are few studies on the cleanliness of residues produced by insulation materials. The melting point of silicon dioxide in insulation materials is about 1600℃, and the boiling point is 2530℃. The operating temperature of attitude and orbit control solid engines is often between these two temperatures. When the temperature of the carbonized layer is higher than the phase transition temperature of SiO2, SiO2 will migrate and lose to the surface of the gas valve in liquid or gaseous form, and may adhere to the surface of the carbonized layer in the form of a liquid film. Therefore, the cleanliness of the insulation layer is also one of the key points related to whether the attitude and orbit control engine can work normally.
[0005] Therefore, under the working conditions of the insulation materials in the attitude and orbit control gas generator, it is a key technology to develop clean insulation materials that can achieve almost zero ablation and no emissions after ablation, and do not produce agglomerates deposited around the valve core. Summary of the invention
[0006] In order to overcome the deficiencies in the prior art, the inventors conducted intensive research and provided a low ablation rate clean insulation material and a preparation method thereof through the design of rubber-resin matrix materials, ablation-resistant / flame-retardant materials, composite material / insulation layer interface bonding, and adaptive propellant / liner / insulation layer formulations. The material meets various performance indicators of insulation materials for solid attitude and orbit control engines, and has successfully passed the ground test valve working assessment on a certain type of attitude and orbit control engine, thus solving the urgent need for the cleanliness of solid attitude and orbit control insulation materials.
[0007] The technical solution provided by the present invention is as follows:
[0008] In a first aspect, a low ablation rate clean insulation material comprises the following components in parts by weight: 100 parts of nitrile rubber, 10 to 25 parts of a plasticizer, 40 to 60 parts of a benzoxazine resin, 30 to 80 parts of ablation-resistant fiber, 1 to 7 parts of an activator, 0.5 to 2.5 parts of a lubricant, 10 to 30 parts of a flame retardant A, 2 to 10 parts of a flame retardant B, 2 to 5 parts of a vulcanizing agent, 0.2 to 0.5 parts of an accelerator, and 0.5 to 0.8 parts of an antioxidant;
[0009] The flame retardant A is an aluminum-based inorganic flame retardant, a magnesium-based inorganic flame retardant and / or an antimony-based flame retardant; the flame retardant B is a phosphate flame retardant; the thermal insulation material has the characteristics of low ablation and cleanliness, and can meet the requirements for the use of thermal insulation materials for gas generators in attitude and orbit control solid rocket engines.
[0010] In a second aspect, a method for preparing a clean insulation material with a low ablation rate comprises:
[0011] The nitrile rubber and the plasticizer are plasticized on a two-roller machine to obtain the nitrile plasticized rubber;
[0012] Add nitrile plasticized rubber, activator, flame retardant A and flame retardant B into an internal mixer and mix them to 50°C to 60°C; add benzoxazine resin and ablation-resistant fiber into the internal mixer and mix them to 70°C to 80°C; add lubricant into the internal mixer and mix them to 100°C to 110°C before discharging to obtain a section of internal mixer, and use thin pass and triangle bag on a two-roller machine until the components are evenly mixed to form a heat insulation layer sheet, and store it in a warehouse with an ambient temperature of 15°C to 35°C and a relative humidity of no more than 75% for at least 12 hours;
[0013] Add a first-stage internal mixing rubber, a vulcanizing agent, an accelerator and an antioxidant into a mixing chamber, mix to 60°C-80°C and discharge to obtain a second-stage internal mixing rubber. Use a thin pass and a triangle bag on a two-roller machine until the components are evenly mixed to form a heat-insulating layer sheet. Store in a warehouse with an ambient temperature of 15°C-35°C and a relative humidity of no more than 75% for at least 24 hours; finally, vulcanize under pressure on a flat vulcanizer to obtain a heat-insulating material.
[0014] According to the present invention, a low ablation rate clean insulation material and a preparation method thereof have the following characteristics:
[0015] Beneficial effects:
[0016] (1) The present invention provides a low ablation rate clean insulation material and a preparation method thereof, which uses rubber and resin as the base material, and is filled with ablation-resistant fibers and flame retardants to prepare the insulation material, which has the characteristics of low ablation rate and can meet the thermal protection requirements of the new solid attitude and orbit control engine for long-term operation;
[0017] (2) The present invention provides a low ablation rate clean insulation material and a preparation method thereof. The formula does not contain the traditional rubber reinforcing agent silica, and the ablated carbon layer has good bonding strength with the matrix and is not easy to produce residue, which can ensure the normal operation of the valve core of the attitude and orbit control engine during operation;
[0018] (3) The present invention provides a low ablation rate clean insulation material and a preparation method thereof, which selects aluminum-magnesium or antimony flame retardants, phosphate flame retardants and ablation-resistant fibers for compound use, and uses a flame retardant mechanism with the condensed phase as the main and the gas phase as the auxiliary, combined with the three elements of the ablation carbon layer: ablation-resistant fiber skeleton, metal oxide flame retardant filler and phosphorus-containing adhesive matrix, to construct a condensed phase carbon layer. The three have a good ablation-flame retardant synergistic effect, and can obtain a clean insulation material with micro-erosion and low ablation characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The surface morphology of the ablated carbon layer of the oxygen-acetylene sample of Example 4 is compared with the conventional EPDM insulation material for attitude and orbit control engines (based on 100 parts by mass of EPDM rubber, the amount of SiO2 is ≥ 25 parts); (a) the ablation morphology of the conventional EPDM insulation material for attitude and orbit control engines, (b) the ablation morphology of the clean insulation material with low ablation rate;
[0020] Figure 2 The surface SEM and element distribution of the carbon layer ablated by oxygen-acetylene sample in Example 4, (a) carbon layer morphology 100 times; (b) carbon layer selected area 3000 times and total surface element distribution; (c) C element distribution; (d) Cl element distribution; (e) Mg element distribution; (f) P element distribution; (g) O element distribution; (h) Zn element distribution;
[0021] Figure 3 It is the physical model of the condensed phase carbon layer;
[0022] Figure 4The results of the ground test valve assessment of a certain type of attitude and orbit control engine using the clean insulation material with low ablation rate of Example 4 and the EPDM insulation material for conventional attitude and orbit control engines are compared; (a) the test results of the EPDM insulation material for conventional attitude and orbit control engines, (b) the test results of the clean insulation material with low ablation rate. DETAILED DESCRIPTION
[0023] The following detailed description of the present invention will make the features and advantages of the present invention more clear and explicit.
[0024] The word “exemplary” is used exclusively herein to mean “serving as an example, example, or illustration.” Any embodiment described herein as “exemplary” is not necessarily to be construed as preferred or advantageous over other embodiments.
[0025] The present invention provides a low ablation rate clean type thermal insulation material, comprising the following components in parts by weight:
[0026] 100 parts of nitrile rubber, 10-25 parts of plasticizer, 40-60 parts of benzoxazine resin, 30-80 parts of ablation-resistant fiber, 1-7 parts of activator, 0.5-2.5 parts of lubricant, 10-30 parts of flame retardant A, 2-10 parts of flame retardant B, 2-5 parts of vulcanizing agent, 0.2-0.5 parts of accelerator, 0.5-0.8 parts of antioxidant, does not contain rubber reinforcing agent silica.
[0027] Preferably, the low ablation rate clean type thermal insulation material comprises the following components in parts by weight:
[0028] 100 parts of nitrile rubber, 15-25 parts of plasticizer, 50-60 parts of benzoxazine resin, 30-70 parts of ablation-resistant fiber, 3-7 parts of activator, 1-2.5 parts of lubricant, 15-20 parts of flame retardant A, 5-8 parts of flame retardant B, 2-5 parts of vulcanizing agent, 0.2-0.5 parts of accelerator, 0.5-0.8 parts of antioxidant, does not contain rubber reinforcing agent silica.
[0029] In a preferred embodiment, the plasticizer is at least one of dibutyl phthalate, dioctyl phthalate, diisooctyl phthalate or triphenyl phosphate.
[0030] In a preferred embodiment, the ablation-resistant fiber is at least one of polyimide fiber, asbestos fiber, phenolic fiber, aramid fiber or carbon fiber; and the short cut length of the ablation-resistant fiber is 3 mm to 10 mm.
[0031] In a preferred embodiment, the activator is at least one of zinc oxide, benzoyl peroxide, di-tert-butyryl peroxide or potassium disulfide.
[0032] In a preferred embodiment, the lubricant is at least one of stearic acid or zinc stearate.
[0033] In a preferred embodiment, the flame retardant A is an aluminum-based inorganic flame retardant, a magnesium-based inorganic flame retardant and / or an antimony-based flame retardant, preferably at least one of magnesium hydroxide, aluminum hydroxide or antimony trioxide.
[0034] In a preferred embodiment, the flame retardant B is a phosphate flame retardant, preferably at least one of tri(2-chloroethylene) phosphate, tri(2-chloropropylene) phosphate, triethyl phosphate, triphenyl phosphate or trioctyl phosphate.
[0035] The flame retardant of the present invention selects aluminum-magnesium or antimony flame retardant, phosphate flame retardant and ablation-resistant fiber to form the three elements of ablation carbon layer and construct a condensed phase carbon layer. The three have good ablation-flame retardant synergistic effect. The physical model of the condensed phase carbon layer is shown in Figure 3 .
[0036] In a preferred embodiment, the vulcanizing agent is at least one of sulfur-carrying vulcanizing agents such as sulfur, dibenzothiazole disulfide, and tetramethylthiuram disulfide.
[0037] In a preferred embodiment, the accelerator is at least one of thiazole or sulfenamide accelerators such as 2-mercaptobenzothiazole and N-cyclohexyl-2-benzothiazolesulfenamide.
[0038] In a preferred embodiment, the antioxidant is at least one of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, N-phenyl-β-naphthylamine, N-(2-methoxyethyl)-p-nitroaniline or 2,6-di-tert-butyl-p-cresol.
[0039] The present invention also provides a method for preparing a clean insulation material with a low ablation rate, comprising:
[0040] The nitrile rubber and the plasticizer are plasticized on a two-roller machine to obtain the nitrile plasticized rubber;
[0041] Add nitrile plasticized rubber, activator, flame retardant A and flame retardant B into an internal mixer, mix to 50-60°C, open the top plug of the internal mixer, add benzoxazine resin and ablation-resistant fiber into the internal mixer, mix to 70-80°C, open the top plug of the internal mixer, add lubricant into the internal mixer, mix to 100-110°C and discharge to obtain a section of internal mixer, use thin pass and triangle bag on a two-roller mill until the components are evenly mixed to form a 2.0-3.0 mm insulation layer sheet, and store it in a warehouse with an ambient temperature of 15-35°C and a relative humidity of no more than 75% for at least 12 hours;
[0042] Add a first-stage internal mixing rubber, a vulcanizing agent, an accelerator and an antioxidant into a mixing chamber, mix to 60°C to 80°C and discharge to obtain a second-stage internal mixing rubber. Use a thin pass and a triangular bag on a two-roller machine until the components are evenly mixed to form a 2.0mm to 3.0mm insulation layer sheet, which is stored in a warehouse with an ambient temperature of 15°C to 35°C and a relative humidity of no more than 75% for at least 24 hours; finally, it is pressurized and vulcanized on a flat vulcanizer to obtain an insulation material.
[0043] Example
[0044] Example 1
[0045] A low ablation rate clean insulation material consists of the following components: 100 parts of nitrile rubber, 15 parts of dioctyl phthalate, 50 parts of benzoxazine resin, 30 parts of aramid fiber with a short cut length of 5 mm, 3 parts of zinc oxide, 1 part of stearic acid, 15 parts of antimony trioxide, 5 parts of tri(2-chloroethylene) phosphate, 5 parts of tetramethylthiuram disulfide, 0.3 parts of 2-mercaptobenzothiazole, and 0.5 parts of N-phenyl-β-naphthylamine.
[0046] The preparation method of the low ablation rate clean type thermal insulation material comprises the following steps:
[0047] (1) plasticizing nitrile rubber and dioctyl phthalate on a two-roll mill to obtain nitrile plasticized rubber;
[0048] (2) Add nitrile plasticized rubber, zinc oxide, antimony trioxide, and tri(2-chloroethylene) phosphate into an internal mixer, mix to 60° C., open the top plug of the internal mixer, add benzoxazine resin and aramid fiber into the internal mixer, mix to 75° C., open the top plug of the internal mixer, add stearic acid into the internal mixer, mix to 110° C., and discharge to obtain a section of internal mixer. Use thin pass and triangle bag on a two-roll mill until the components are evenly mixed to form a 2.0 mm insulation layer sheet, which is placed in a warehouse with an ambient temperature of 25° C. and a relative humidity of 30% to 70% for 24 hours;
[0049] (3) Add the first stage internal mixing rubber, tetramethylthiuram disulfide, 2-mercaptobenzothiazole, and N-phenyl-β-naphthylamine into the internal mixing chamber, mix to 70°C, and then discharge to obtain the second stage internal mixing rubber. Use thin pass and triangle bag on a two-roller mill until the components are mixed evenly to form a 2.0 mm insulation layer sheet, which is placed in a warehouse with an ambient temperature of 25°C and a relative humidity of 30% to 70% for 48 hours. Finally, it is pressurized and vulcanized on a flat vulcanizer to obtain an insulation material.
[0050] Table 1 shows the oxygen-acetylene line ablation rate, mass ablation rate, tensile strength and elongation of the insulation material samples tested in Example 1. Comparing the oxygen-acetylene ablation morphology of the insulation material in Example 1 with that of the conventional EPDM insulation material for attitude and orbit control engines, it can be seen that compared with conventional insulation materials, the low ablation rate clean insulation material of the present invention has a more complete and dense ablated carbon layer with basically no erosion, while the ablated carbon layer of the latter is sparse and brittle, and easy to peel off. The micromorphology and elemental analysis of the ablated carbon layer of the oxygen-acetylene sample of Example 1 show that the strip-distributed skeleton structure in the micromorphology contains more carbon elements, the dispersed particle structure contains a small amount of Mg, P and other elements, and the main components of the condensed phase carbon layer are carbon fibers, magnesium oxide and phosphorus-containing substances. From the comparison results of the ground test valve assessment on a certain type of attitude and orbit control engine carried by the clean insulation material with low ablation rate in Example 1 and the EPDM insulation material for conventional attitude and orbit control engines, it can be seen that since the insulation material formula of the present invention does not contain the traditional rubber reinforcement agent silica, and the ablated carbon layer has good bonding strength with the matrix and is not easy to produce residue, it can ensure the normal operation of the valve core of the attitude and orbit control engine during operation.
[0051] Table 1 Example 1 Preparation of thermal insulation material sample performance by masterbatch material
[0052]
[0053] Example 2
[0054] A low ablation rate clean insulation material consists of the following components: 100 parts of nitrile rubber, 20 parts of dibutyl phthalate, 60 parts of benzoxazine resin, 60 parts of carbon fiber with a short cut length of 3 mm, 3 parts of zinc oxide, 1.5 parts of stearic acid, 16 parts of magnesium hydroxide, 5 parts of tri(2-chloroethylene) phosphate, 4 parts of tetramethylthiuram disulfide, 0.2 parts of N-cyclohexyl-2-benzothiazole sulfonamide, and 0.5 parts of 2,2,4-trimethyl-1,2-dihydroquinoline polymer.
[0055] The preparation method of the low ablation rate clean type thermal insulation material comprises the following steps:
[0056] (1) plasticating nitrile rubber and dibutyl phthalate on a two-roll mill to obtain nitrile plasticized rubber;
[0057] (2) Add nitrile plasticized rubber, zinc oxide, magnesium hydroxide, and tri(2-chloroethylene) phosphate to an internal mixer, mix to 50° C., open the top plug on the internal mixer, add benzoxazine resin and carbon fiber to the internal mixer, mix to 70° C., open the top plug on the internal mixer, add stearic acid to the internal mixer, mix to 110° C., and discharge to obtain a section of internal mixer. Use thin pass and triangle bag on a two-roll mill until the components are evenly mixed to form a 2.5 mm insulation layer sheet, which is placed in a warehouse with an ambient temperature of 25° C. and a relative humidity of 20% to 60% for 20 hours;
[0058] (3) Add the first-stage internal mixing rubber, tetramethylthiuram disulfide, N-cyclohexyl-2-benzothiazole sulfenamide, and 2,2,4-trimethyl-1,2-dihydroquinoline polymer into the internal mixing chamber, mix to 75°C, and discharge to obtain the second-stage internal mixing rubber. Use thin pass and triangle bag on a two-roller mill until the components are mixed evenly to form a 2.5 mm insulation layer sheet, which is placed in a warehouse with an ambient temperature of 25°C and a relative humidity of 20% to 60% for 48 hours. Finally, the insulation material is obtained by pressure vulcanization on a flat vulcanizer.
[0059] Table 2 shows the oxygen-acetylene line ablation rate, mass ablation rate, tensile strength and elongation of the insulation material samples tested in Example 2. Comparing the oxygen-acetylene ablation morphology of the insulation material of Example 2 with that of the conventional EPDM insulation material for attitude and orbit control engines, it can be seen that compared with conventional insulation materials, the low ablation rate clean insulation material of the present invention has a more complete and dense ablated carbon layer with basically no erosion, while the ablated carbon layer of the latter is sparse and brittle, and easy to peel off. The microscopic morphology and elemental analysis of the ablated carbon layer of the oxygen-acetylene sample of Example 2 show that the strip-shaped skeleton structure in the microscopic morphology contains more carbon elements, the dispersed particle structure contains a small amount of Mg, P and other elements, and the main components of the condensed phase carbon layer are carbon fibers, magnesium oxide and phosphorus-containing substances. From the comparison results of the ground test valve assessment on a certain type of attitude and orbit control engine carried by the clean insulation material with low ablation rate in Example 2 and the EPDM insulation material for conventional attitude and orbit control engines, it can be seen that since the insulation material formula of the present invention does not contain the traditional rubber reinforcement agent silica, and the ablated carbon layer has good bonding strength with the matrix and is not easy to produce residue, it can ensure the normal operation of the valve core of the attitude and orbit control engine during operation.
[0060] Table 2 Performance of thermal insulation material samples prepared from masterbatch materials in Example 2
[0061]
[0062]
[0063] Example 3
[0064] A low ablation rate clean insulation material consists of the following components: 100 parts of nitrile rubber, 12.5 parts of dibutyl phthalate, 50 parts of benzoxazine resin, 50 parts of polyimide fiber with a short cut length of 5 mm, 6.25 parts of potassium disulfide, 2.5 parts of stearic acid, 18.75 parts of aluminum hydroxide, 6.25 parts of tri(2-chlorovinyl) phosphate, 4.4 parts of dibenzothiazole disulfide, 0.4 parts of N-cyclohexyl-2-benzothiazole sulfonamide, and 0.6 parts of 2,2,4-trimethyl-1,2-dihydroquinoline polymer.
[0065] The preparation method of the low ablation rate clean type thermal insulation material comprises the following steps:
[0066] (1) plasticating nitrile rubber and dibutyl phthalate on a two-roll mill to obtain nitrile plasticized rubber;
[0067] (2) Add nitrile plasticized rubber, potassium disulfide, aluminum hydroxide, and tri(2-chloroethylene) phosphate to an internal mixer, mix to 50° C., open the top plug of the internal mixer, add benzoxazine resin and polyimide fiber to the internal mixer, mix to 75° C., open the top plug of the internal mixer, add stearic acid to the internal mixer, mix to 100° C., and discharge to obtain a section of internal mixer. Use thin pass and triangle bag on a two-roll mill until the components are evenly mixed to form a 2.5 mm insulation layer sheet, which is placed in a warehouse with an ambient temperature of 25° C. and a relative humidity of 30% to 60% for 18 hours;
[0068] (3) Add the first-stage internal mixing rubber, dibenzothiazole disulfide, N-cyclohexyl-2-benzothiazole sulfonamide, and 2,2,4-trimethyl-1,2-dihydroquinoline polymer into the internal mixing chamber, mix to 80°C, and then discharge to obtain the second-stage internal mixing rubber. Use thin pass and triangle bag on a two-roller mill until the components are mixed evenly to form a 3.0 mm insulation layer sheet, which is placed in a warehouse with an ambient temperature of 25°C and a relative humidity of 30% to 60% for 48 hours. Finally, the insulation material is obtained by pressure vulcanization on a flat vulcanizer.
[0069] Table 3 shows the oxygen-acetylene line ablation rate, mass ablation rate, tensile strength and elongation of the insulation material samples tested in Example 3. Comparing the oxygen-acetylene ablation morphology of the insulation material of Example 3 with that of the conventional EPDM insulation material for attitude and orbit control engines, it can be seen that compared with conventional insulation materials, the low ablation rate clean insulation material of the present invention has a more complete and dense ablated carbon layer with basically no erosion, while the ablated carbon layer of the latter is sparse and brittle, and easy to peel off. The microscopic morphology and elemental analysis of the ablated carbon layer of the oxygen-acetylene sample of Example 3 show that the strip-distributed skeleton structure in the microscopic morphology contains more carbon elements, the dispersed particle structure contains a small amount of Mg, P and other elements, and the main components of the condensed phase carbon layer are carbon fibers, magnesium oxide and phosphorus-containing substances. From the comparison results of the ground test valve assessment on a certain type of attitude and orbit control engine carried by the clean insulation material with low ablation rate in Example 3 and the EPDM insulation material for conventional attitude and orbit control engines, it can be seen that since the insulation material formula of the present invention does not contain the traditional rubber reinforcement agent silica, and the ablated carbon layer has good bonding strength with the matrix and is not easy to produce residue, it can ensure the normal operation of the valve core of the attitude and orbit control engine during operation.
[0070] Table 3 Performance of thermal insulation material samples prepared from masterbatch materials in Example 3
[0071] Serial number Test items Test value 1 Linear ablation rate (mm / s) 0.0425 2 Mass ablation rate (g / s) 0.0315 3 Thermal conductivity (Wmk) 0.2156 4 Tensile strength(kPa) 5079 5 Elongation(%) 239 6 <![CDATA[Density (g / cm 3 )]]> 1.20 7 Shore hardness 80
[0072] Example 4
[0073] A low ablation rate clean insulation material consists of the following components: 100 parts of nitrile rubber, 22 parts of diethyl phthalate, 55 parts of benzoxazine resin, 66 parts of carbon fiber with a short cut length of 5 mm, 5.5 parts of zinc oxide, 1.6 parts of stearic acid, 20 parts of magnesium hydroxide, 6.6 parts of triphenyl phosphate, 5 parts of tetramethylthiuram disulfide, 0.3 parts of N-cyclohexyl-2-benzothiazole sulfonamide, and 0.5 parts of 2,6-di-tert-butyl-p-cresol.
[0074] The preparation method of the low ablation rate clean type thermal insulation material comprises the following steps:
[0075] (1) plasticizing nitrile rubber and diisooctyl phthalate on a two-roll mill to obtain nitrile plasticized rubber;
[0076] (2) Add nitrile plasticized rubber, zinc oxide, magnesium hydroxide, and triphenyl phosphate into an internal mixer, mix to 55° C., open the top plug of the internal mixer, add benzoxazine resin and carbon fiber into the internal mixer, mix to 80° C., open the top plug of the internal mixer, add stearic acid into the internal mixer, mix to 110° C., and discharge to obtain a section of internal mixer. Use thin pass and triangle bag on a two-roll mill until the components are evenly mixed to form a 2.5 mm insulation layer sheet, which is placed in a warehouse with an ambient temperature of 25° C. and a relative humidity of 30% to 60% for 24 hours;
[0077] (3) Add the first-stage internal mixing rubber, tetramethylthiuram disulfide, N-cyclohexyl-2-benzothiazole sulfonamide, and 2,6-di-tert-butyl-p-cresol into the internal mixing chamber, mix to 70°C, and discharge to obtain the second-stage internal mixing rubber. Use thin pass and triangle bag on a two-roller mill until the components are mixed evenly to form a 2.5 mm insulation layer sheet, which is placed in a warehouse with an ambient temperature of 25°C and a relative humidity of 30% to 60% for 48 hours. Finally, the insulation material is obtained by pressure vulcanization on a flat vulcanizer.
[0078] Table 4 shows the oxygen-acetylene wire ablation rate, mass ablation rate, tensile strength and elongation of the insulation material samples tested in Example 4. Figure 1 By comparing the oxygen-acetylene ablation morphology of the insulation material of Example 4 with the conventional EPDM insulation material for attitude and orbit control engines, it can be seen that compared with conventional insulation materials, the low ablation rate clean insulation material of the present invention has a more complete and dense ablated carbon layer with basically no peeling, while the latter has a sparse, brittle ablated carbon layer that is easy to peel off. Figure 2 The microscopic morphology and elemental analysis of the carbon layer ablated by the oxygen-acetylene sample of Example 4 show that the strip-shaped skeleton structure in the microscopic morphology contains more carbon elements, the diffusely distributed particle structure contains a small amount of Mg, P and other elements, and the main components of the condensed phase carbon layer are carbon fibers, magnesium oxide and phosphorus-containing substances. Figure 4The comparison results of the clean insulation material with low ablation rate in Example 4 and the EPDM insulation material for conventional attitude and orbit control engines on the ground test valves of a certain type of attitude and orbit control engine are shown; (a) the test results of the EPDM insulation material for conventional attitude and orbit control engines, (b) the test results of the clean insulation material with low ablation rate; since the insulation material formula does not contain the traditional rubber reinforcement agent silica, and the ablated carbon layer has good bonding strength with the matrix and is not easy to produce residue, it can ensure the normal operation of the valve core of the attitude and orbit control engine during operation.
[0079] Table 4 Performance of thermal insulation material samples prepared from masterbatch materials in Example 4
[0080]
[0081]
[0082] Example 5
[0083] A low ablation rate clean insulation material consists of the following components: 100 parts of nitrile rubber, 20 parts of dibutyl phthalate, 55 parts of benzoxazine resin, 40 parts of aramid fiber with a short cut length of 5 mm, 4 parts of zinc oxide, 2 parts of stearic acid, 20 parts of antimony trioxide, 5 parts of triphenyl phosphate, 5 parts of tetramethylthiuram disulfide, 0.2 parts of 2-mercaptobenzothiazole, and 0.6 parts of N-phenyl-β-naphthylamine.
[0084] The preparation method of the low ablation rate clean type thermal insulation material comprises the following steps:
[0085] (1) plasticating nitrile rubber and dibutyl phthalate on a two-roll mill to obtain nitrile plasticized rubber;
[0086] (2) Adding nitrile plasticized rubber, zinc oxide, antimony trioxide, and triphenyl phosphate to an internal mixer, mixing to 50° C., opening the top plug on the internal mixer, adding benzoxazine resin and aramid fiber to the internal mixer, mixing to 75° C., opening the top plug on the internal mixer, adding stearic acid to the internal mixer, mixing to 105° C., and discharging to obtain a section of internal mixer rubber. Using a thin pass and a triangle bag on a two-roll mill until the components are evenly mixed, a 2.5 mm insulation layer sheet is prepared, and the sheet is placed in a warehouse with an ambient temperature of 25° C. and a relative humidity of 35% to 70% for 20 hours;
[0087] (3) Add the first stage internal mixing rubber, tetramethylthiuram disulfide, 2-mercaptobenzothiazole, and N-phenyl-β-naphthylamine into the internal mixing chamber, mix to 80°C, and then discharge to obtain the second stage internal mixing rubber. Use thin pass and triangle bag on a two-roller mill until the components are mixed evenly to form a 3.0 mm insulation layer sheet, which is placed in a warehouse with an ambient temperature of 25°C and a relative humidity of 35% to 70% for 48 hours. Finally, the insulation material is obtained by pressure vulcanization on a flat vulcanizer.
[0088] Table 5 shows the oxygen-acetylene line ablation rate, mass ablation rate, tensile strength and elongation of the insulation material samples tested in Example 5. Comparing the oxygen-acetylene ablation morphology of the insulation material in Example 5 with that of the conventional EPDM insulation material for attitude and orbit control engines, it can be seen that compared with conventional insulation materials, the low ablation rate clean insulation material of the present invention has a more complete and dense ablated carbon layer with basically no erosion, while the ablated carbon layer of the latter is sparse and brittle, and easy to peel off. The microscopic morphology and elemental analysis of the ablated carbon layer of the oxygen-acetylene sample of Example 5 show that the strip-shaped skeleton structure in the microscopic morphology contains more carbon elements, the dispersed particle structure contains a small amount of Mg, P and other elements, and the main components of the condensed phase carbon layer are carbon fibers, magnesium oxide and phosphorus-containing substances. From the comparison results of the ground test valve assessment on a certain type of attitude and orbit control engine carried by the clean insulation material with low ablation rate in Example 5 and the EPDM insulation material for conventional attitude and orbit control engines, it can be seen that since the insulation material formula of the present invention does not contain the traditional rubber reinforcement agent silica, and the ablated carbon layer has good bonding strength with the matrix and is not easy to produce residue, it can ensure the normal operation of the valve core of the attitude and orbit control engine during operation.
[0089] Table 5 Performance of thermal insulation material samples prepared from masterbatch materials in Example 5
[0090]
[0091] Comparative Example
[0092] Comparative Example 1
[0093] This comparative example 1 is consistent with example 4, except that it does not contain magnesium hydroxide and triphenyl phosphate, and contains 25 parts of silicon dioxide.
[0094] Comparative Example 2
[0095] This comparative example 1 is consistent with example 4, except that it does not contain triphenyl phosphate.
[0096] Comparative Example 3
[0097] This comparative example 1 is consistent with embodiment 4, and the only difference is that it does not contain magnesium hydroxide.
[0098] Table 6 Performance table of samples of comparative examples 1-3
[0099]
[0100]
[0101] Table 6 shows the performance test results of the insulation material samples tested in Comparative Examples 1-3 and Example 4. In Comparative Example 1, magnesium hydroxide and diphenyl phosphate were replaced by silicon dioxide, and both the linear ablation rate and the mass ablation rate were improved. In Comparative Example 2, triphenyl phosphate was not contained, and both the linear ablation rate and the mass ablation rate were improved. In Comparative Example 3, magnesium hydroxide was not contained, and the linear ablation rate and the mass ablation rate were significantly improved. This shows that magnesium hydroxide and triphenyl phosphate flame retardants have a significant and irreplaceable role in the formula, and can form an ablation-flame retardant system with ablation-resistant fibers, thereby improving the ablation resistance of the material and meeting the requirements of a low ablation rate clean type.
[0102] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.
[0103] The contents not described in detail in the specification of the present invention belong to the common knowledge of those skilled in the art.
Claims
1. A low ablation rate clean insulation material, characterized in that: The invention comprises the following components in parts by weight: 100 parts of nitrile rubber, 10 to 25 parts of plasticizer, 40 to 60 parts of benzoxazine resin, 30 to 80 parts of ablation-resistant fiber, 1 to 7 parts of activator, 0.5 to 2.5 parts of lubricant, 10 to 30 parts of flame retardant A, 2 to 10 parts of flame retardant B, 2 to 5 parts of vulcanizing agent, 0.2 to 0.5 parts of accelerator, and 0.5 to 0.8 parts of antioxidant; The flame retardant A is an aluminum-based inorganic flame retardant, a magnesium-based inorganic flame retardant and / or an antimony-based flame retardant; the flame retardant B is a phosphate flame retardant.
2. The low ablation rate clean insulation material according to claim 1, characterized in that: The plasticizer is at least one of dibutyl phthalate, dioctyl phthalate, diisooctyl phthalate or triphenyl phosphate.
3. The low ablation rate clean insulation material according to claim 1, characterized in that: The ablation-resistant fiber is at least one of polyimide fiber, asbestos fiber, phenolic fiber, aramid fiber or carbon fiber.
4. The low ablation rate clean type thermal insulation material according to claim 1, characterized in that: The activator is at least one of zinc oxide, benzoyl peroxide, di-tert-butyryl peroxide or potassium disulfide.
5. The low ablation rate clean type thermal insulation material according to claim 1, characterized in that: The lubricant is at least one of stearic acid or zinc stearate.
6. The low ablation rate clean type thermal insulation material according to claim 1, characterized in that: The flame retardant A is at least one of magnesium hydroxide, aluminum hydroxide or antimony trioxide.
7. The low ablation rate clean type thermal insulation material according to claim 1, characterized in that: The flame retardant B is at least one of tri(2-chloroethylene) phosphate, tri(2-chloropropylene) phosphate, triethyl phosphate, triphenyl phosphate or trioctyl phosphate.
8. The low ablation rate clean type thermal insulation material according to claim 1, characterized in that: The vulcanizing agent is at least one of sulfur, dibenzothiazole disulfide or tetramethylthiuram disulfide; and / or The accelerator is at least one of 2-mercaptobenzothiazole and N-cyclohexyl-2-benzothiazole sulfenamide; and / or The antioxidant is at least one of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, N-phenyl-β-naphthylamine, N-(2-methoxyethyl)-p-nitroaniline or 2,6-di-tert-butyl-p-cresol.
9. The low ablation rate clean type thermal insulation material according to claim 1, characterized in that: The thermal insulation material does not contain silicon dioxide.
10. A method for preparing a clean insulation material with low ablation rate according to any one of claims 1 to 9, characterized in that: include: The nitrile rubber and the plasticizer are plasticized on a two-roller machine to obtain the nitrile plasticized rubber; Add nitrile plasticized rubber, activator, flame retardant A and flame retardant B into an internal mixer and mix them to 50°C to 60°C; add benzoxazine resin and ablation-resistant fiber into the internal mixer and mix them to 70°C to 80°C; add lubricant into the internal mixer and mix them to 100°C to 110°C before discharging to obtain a section of internal mixer, and use thin pass and triangle bag on a two-roller machine until the components are evenly mixed to form a heat insulation layer sheet, and store it in a warehouse with an ambient temperature of 15°C to 35°C and a relative humidity of no more than 75% for at least 12 hours; Add a first-stage internal mixing rubber, a vulcanizing agent, an accelerator and an antioxidant into a mixing chamber, mix to 60°C-80°C and discharge to obtain a second-stage internal mixing rubber. Use a thin pass and a triangle bag on a two-roller machine until the components are evenly mixed to form a heat-insulating layer sheet. Store in a warehouse with an ambient temperature of 15°C-35°C and a relative humidity of no more than 75% for at least 24 hours; finally, vulcanize under pressure on a flat vulcanizer to obtain a heat-insulating material.