Carbon black-based electromagnetic shielding composite material and preparation method thereof
By using carbon black-based electromagnetic shielding composite materials with components such as modified carbon black and nitrile rubber in cables, the problems of insufficient electromagnetic shielding capabilities and insufficient mechanical properties in traditional cables are solved, and efficient electromagnetic shielding and mechanical properties are achieved. promote.
Patent Information
- Application Number
- CN202410942309.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional metal shielding layers in cables are limited by weight, flexibility and cost issues, and pure NBR has insufficient electromagnetic shielding capabilities. New composite materials with both excellent electromagnetic shielding and good mechanical properties need to be developed.
Carbon black-based electromagnetic shielding composite materials are used. The modified carbon black is dried in concentrated hydrochloric acid, mixed with pretreated nitrile rubber, zinc oxide and other components and vulcanized. The carbon black is oxidized, sensitized and nickel plated. Processed to improve its dispersion and conductive properties in the material, forming a hydrogen bond cross-linked network to enhance the mechanical properties of the material.
It significantly improves the electromagnetic shielding performance and mechanical properties, ensures the uniform dispersion of carbon black particles and the continuity of the conductive network, and meets the needs of high-performance cables.
Smart Images

Figure BDA0004944539660000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electromagnetic shielding materials, and in particular to a carbon black-based electromagnetic shielding composite material and a preparation method thereof. Background Art
[0002] In the field of modern electronics and communications, electromagnetic interference (EMI) is becoming increasingly severe, affecting equipment operation and signal quality, and even threatening human health. Cables are key connectors, and their electromagnetic shielding performance is crucial to system stability. Although traditional metal shielding layers are effective, they are limited in applications that pursue lightness and flexibility due to weight, flexibility and cost issues. For this reason, the research and development of new composite materials that have both excellent electromagnetic shielding and good mechanical properties has become a research focus.
[0003] Nitrile rubber (NBR) is widely used in cable materials for its excellent oil resistance, wear resistance and heat resistance. However, pure NBR has insufficient electromagnetic shielding ability. Its shielding effectiveness can be enhanced by adding conductive fillers, such as carbon black. Carbon black has high specific surface area, low resistance and good dispersibility, which can form a conductive network and greatly improve the electromagnetic shielding performance of the material. However, the uniform dispersion of carbon black is the key. Poor dispersion will weaken the shielding effect and damage the mechanical properties of the material, such as tensile strength and elongation at break.
[0004] Therefore, it is of great significance to conduct in-depth research on the uniform dispersion technology of carbon black in nitrile rubber and optimize the material mechanics and electromagnetic shielding performance at the same time. This can not only promote the innovation of electromagnetic shielding materials, but also promote the technological upgrading of the cable industry and meet the market's urgent demand for high-performance cables. Therefore, the applicant prepared a carbon black-based electromagnetic shielding composite material to solve the above problems. Summary of the invention
[0005] In order to solve the existing technical problems, the present invention provides a carbon black-based electromagnetic shielding composite material, which comprises the following raw material components in parts by weight: 100 parts by weight of pretreated nitrile rubber, 5 parts by weight of zinc oxide, 1 part by weight of stearic acid, 2 parts by weight of antioxidant MB, 1 part by weight of antioxidant RD, 1.5 parts by weight of accelerator DTDM, 1 part by weight of accelerator TMTD, 2.5 parts by weight of accelerator DM, and 18 to 22 parts by weight of acid-treated modified carbon black.
[0006] Furthermore, the pretreated nitrile rubber is obtained by dissolving the nitrile rubber in tetrahydrofuran, adding a methanol solution of hydroxylamine hydrochloride and a methanol solution of potassium hydroxide, and then washing, flocculating and drying.
[0007] Furthermore, the acid-treated modified carbon black is obtained by mixing the modified carbon black in concentrated hydrochloric acid and then drying it.
[0008] Furthermore, the modified carbon black is obtained by oxidizing carbon black and then performing two sensitizations and nickel plating.
[0009] The present invention also provides a method for preparing a carbon black-based electromagnetic shielding composite material, comprising the following preparation steps:
[0010] (1) The modified carbon black and 20% concentrated hydrochloric acid were mixed in a volume ratio of 1:1 and stirred for 20 to 30 minutes, and then placed in an oven at 100 to 120° C. for 40 to 80 minutes to obtain acid-treated modified carbon black;
[0011] (2) 100 parts by mass of pretreated nitrile rubber, 5 parts by mass of zinc oxide, 1 part by mass of stearic acid, 2 parts by mass of antioxidant MB, 1 part by mass of antioxidant RD, 1.5 parts by mass of accelerator DTDM, 1 part by mass of accelerator TMTD, and 2.5 parts by mass of accelerator DM were mixed for 20 to 30 minutes, and then 18 to 22 parts by mass of acid-treated modified carbon black were added and mixed for another 20 to 30 minutes. Then, the mixture was vulcanized at 160°C and 15 MPa for 30 minutes to obtain a 2 mm thick carbon black-based electromagnetic shielding composite material.
[0012] Furthermore, the preparation method of the modified carbon black is as follows: 1 part by mass of carbon black is added to 140 parts by mass of a 68% nitric acid solution, ultrasonically oscillated at 80°C for 10 hours, filtered, washed with deionized water until the washing liquid is neutral, then dried at 80°C to constant weight, naturally cooled to room temperature, then added to 140 parts by mass of a sensitizing solution A and ultrasonically oscillated at 25°C for 1 hour, continued to filter, washed with deionized water until the washing liquid is neutral, then dried at 80°C to constant weight, naturally cooled to room temperature, then added to 140 parts by mass of a sensitizing solution B and ultrasonically oscillated at 25°C for 1 hour, continued to filter, washed with deionized water until the washing liquid is neutral, then dried at 80°C to constant weight, naturally cooled to room temperature, and finally added to 1000 parts by mass of a nickel plating solution, ultrasonically oscillated at 35°C for 5 minutes, filtered after completion, washed with deionized water 5 to 7 times, then dried at 80°C to constant weight, and naturally cooled to room temperature to obtain modified carbon black.
[0013] Furthermore, the sensitizing solution A includes tin chloride and hydrogen chloride; wherein the tin chloride content is 20 g / L and the hydrogen chloride concentration is 1 M; the sensitizing solution B includes palladium chloride and hydrogen chloride; wherein the palladium chloride concentration is 1 g / L and the hydrogen chloride concentration is 0.25 M.
[0014] Furthermore, the preparation method of the nickel plating solution is as follows: 5 parts by mass of sodium citrate, 25 parts by mass of nickel (II) sulfate hexahydrate, 15 parts by mass of sodium dihydrogen hypophosphite, 60 parts by mass of ammonium chloride and 1000 parts by mass of deionized water are mixed, and then 28% ammonia water is added to adjust the pH to 9 to obtain a nickel plating solution.
[0015] Furthermore, the preparation method of the pretreated nitrile rubber is as follows: 30 parts by mass of nitrile rubber and 240 to 250 parts by mass of tetrahydrofuran are mixed, stirred until the solution is uniform and transparent, then 47 parts by mass of a methanol solution of hydroxylamine hydrochloride and 16 parts by mass of a methanol solution of potassium hydroxide are added, and mixing is continued for 10 to 15 minutes, then the water bath is heated to 40 to 60°C, and the condensation reaction is carried out at a speed of 300r / min for 12 to 24 hours. During the reaction, 47 parts by mass of a methanol solution of hydroxylamine hydrochloride and 16.16 parts by mass of a methanol solution of potassium hydroxide are added every 6 hours, and then 40°C deionized water is added at a rate of 5s / drop to wash until neutral, and then added to 480 to 500 parts by mass of ethanol for flocculation and precipitation, filtered, and placed in a 60°C oven to dry to constant weight to obtain the pretreated nitrile rubber.
[0016] Furthermore, the preparation steps of the methanol solution of hydroxylamine hydrochloride are as follows: dissolving hydroxylamine hydrochloride in anhydrous methanol to obtain the methanol solution of hydroxylamine hydrochloride, wherein the mass ratio of hydroxylamine hydrochloride to anhydrous methanol is 7:40; the mass ratio of potassium hydroxide in the methanol solution is 6.16:10.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The carbon black-based electromagnetic shielding composite material prepared by the invention comprises the following steps: firstly, modifying carbon black is mixed in concentrated hydrochloric acid and then dried to obtain acid-treated modifying carbon black; then, pre-treated nitrile rubber, zinc oxide, stearic acid, antioxidant MB, antioxidant RD, accelerator DTDM, accelerator TMTD, accelerator DM and the acid-treated modifying carbon black are mixed and vulcanized to obtain the modified carbon black; wherein the modified carbon black is obtained by oxidizing the carbon black and then performing sensitization twice and nickel plating; and the pre-treated nitrile rubber is obtained by dissolving the nitrile rubber in tetrahydrofuran, adding a methanol solution of hydroxylamine hydrochloride and a methanol solution of potassium hydroxide to react, and then washing, flocculating and drying.
[0019] First, the carbon black is oxidized, followed by two sensitizations and nickel plating to obtain a modified carbon black with a surface covered with metallic nickel. This process aims to overcome the high cohesive energy problem caused by the presence of a large number of polar groups between carbon black particles, as well as the challenges of difficult dispersion and easy flocculation in the matrix material, thereby improving its compatibility with the matrix material. Traditionally, in order to achieve low volume resistivity, a large amount of carbon black filler needs to be added, which will significantly reduce the mechanical properties of the rubber. To resolve this contradiction, we chose to adhere the non-oxidizable and low-cost metallic nickel to the surface of the carbon black by chemical plating, which can significantly improve the conductivity of the rubber even at a lower addition amount.
[0020] Secondly, the present application pre-treats the nitrile rubber and introduces amine oxime bonds into the molecular chain of the rubber. The amine oxime bonds can undergo self-condensation at high temperature to produce a "covalent" cross-linked network; at the same time, the nitrile rubber functionalized with amine oxime and the acid-treated modified carbon black are mixed and vulcanized, and the nickel chloride attached to the surface of the acid-treated modified carbon black can coordinate with the ligand amine oxime bonds on the rubber to obtain metal coordination bonds. The acid-treated modified carbon black is uniformly dispersed in the nitrile rubber, and the uniformly dispersed nickel-plated carbon black particles can ensure the continuity and integrity of the conductive network, and the "hydrogen bonds" between the molecules of the amine oxime functionalized nitrile rubber can form a hydrogen bond cross-linked network, so that the molecular chain of the self-crosslinking and self-reinforcing rubber of the present invention contains a hydrogen bond cross-linked network, a metal coordination bond cross-linked network and a covalent bond cross-linked network, thereby enhancing the mechanical properties and electromagnetic shielding properties of the carbon black-based electromagnetic shielding composite material. DETAILED DESCRIPTION
[0021] The present invention is further described in detail below in conjunction with examples, but the following examples should not be construed as limiting the present invention.
[0022] Some of the raw materials of the embodiments of the present invention and the comparative examples are as follows:
[0023] The primary structure particle size of carbon black is about 20nm, and the DBP absorption value is 6*10 -3 m 3 *kg -1 , pH is 6, and volume resistivity is 0.2Ω*cm.
[0024] The nitrile rubber used is NBR220S from Japan JSR Company.
[0025] Example 1
[0026] A method for preparing a carbon black-based electromagnetic shielding composite material, the preparation steps are as follows:
[0027] (1) The modified carbon black and 20% concentrated hydrochloric acid were mixed in a volume ratio of 1:1 and stirred for 20 minutes, and then placed in an oven at 100° C. for 40 minutes to obtain acid-treated modified carbon black;
[0028] (2) 100 parts by mass of pretreated nitrile rubber, 5 parts by mass of zinc oxide, 1 part by mass of stearic acid, 2 parts by mass of antioxidant MB, 1 part by mass of antioxidant RD, 1.5 parts by mass of accelerator DTDM, 1 part by mass of accelerator TMTD, and 2.5 parts by mass of accelerator DM were mixed for 20 minutes, and then 18 parts by mass of acid-treated modified carbon black were added and mixed for another 20 minutes. Then, the mixture was vulcanized at 160°C and 15 MPa for 30 minutes to obtain a 2 mm thick carbon black-based electromagnetic shielding composite material.
[0029] The preparation method of the modified carbon black is as follows: 1 part by mass of carbon black is added to 140 parts by mass of nitric acid solution with a mass fraction of 68%, ultrasonically oscillated at 80° C. for 10 hours, filtered, washed with deionized water until the washing liquid is neutral, then dried at 80° C. to constant weight, naturally cooled to room temperature, then added to 140 parts by mass of sensitizing solution A and ultrasonically oscillated at 25° C. for 1 hour, continued to filter, washed with deionized water until the washing liquid is neutral, then dried at 80° C. to constant weight, naturally cooled to room temperature, then added to 140 parts by mass of sensitizing solution B and ultrasonically oscillated at 25° C. for 1 hour, continued to filter, washed with deionized water until the washing liquid is neutral, then dried at 80° C. to constant weight, naturally cooled to room temperature, and finally added to 1000 parts by mass of nickel plating solution, ultrasonically oscillated at 35° C. for 5 minutes, filtered after completion, washed with deionized water 5 times, then dried at 80° C. to constant weight, and naturally cooled to room temperature to obtain the modified carbon black.
[0030] The sensitizing solution A includes tin chloride and hydrogen chloride; wherein the tin chloride content is 20 g / L and the hydrogen chloride concentration is 1 M; the sensitizing solution B includes palladium chloride and hydrogen chloride; wherein the palladium chloride concentration is 1 g / L and the hydrogen chloride concentration is 0.25 M.
[0031] The nickel plating solution is prepared as follows: 5 parts by mass of sodium citrate, 25 parts by mass of nickel (II) sulfate hexahydrate, 15 parts by mass of sodium dihydrogen hypophosphite, 60 parts by mass of ammonium chloride and 1000 parts by mass of deionized water are mixed, and then 28% ammonia water is added to adjust the pH to 9 to obtain a nickel plating solution.
[0032] The preparation method of the pretreated nitrile rubber is as follows: 30 parts by mass of nitrile rubber and 240 parts by mass of tetrahydrofuran are mixed, stirred until the solution is uniform and transparent, then 47 parts by mass of hydroxylamine hydrochloride methanol solution and 16 parts by mass of potassium hydroxide methanol solution are added, and the mixing is continued for 10 minutes, then the water bath is heated to 40°C, and condensation reaction is carried out at a speed of 300r / min for 12 hours. During the reaction, 47 parts by mass of hydroxylamine hydrochloride methanol solution and 16.16 parts by mass of potassium hydroxide methanol solution are added every 6 hours, and then 40°C deionized water is added at a rate of 5s / drop to wash until neutral, and then added to 480 parts by mass of ethanol for flocculation and precipitation, and after filtering, it is placed in a 60°C oven and dried to constant weight to obtain the pretreated nitrile rubber.
[0033] The preparation steps of the methanol solution of hydroxylamine hydrochloride are as follows: dissolving hydroxylamine hydrochloride in anhydrous methanol to obtain the methanol solution of hydroxylamine hydrochloride, wherein the mass ratio of hydroxylamine hydrochloride to anhydrous methanol is 7:40; and the mass ratio of potassium hydroxide in the methanol solution is 6.16:10.
[0034] Example 2
[0035] A method for preparing a carbon black-based electromagnetic shielding composite material, the preparation steps are as follows:
[0036] (1) The modified carbon black and 20% concentrated hydrochloric acid were mixed in a volume ratio of 1:1 and stirred for 25 minutes, and then placed in an oven at 110° C. for 60 minutes to obtain acid-treated modified carbon black;
[0037] (2) 100 parts by mass of pretreated nitrile rubber, 5 parts by mass of zinc oxide, 1 part by mass of stearic acid, 2 parts by mass of antioxidant MB, 1 part by mass of antioxidant RD, 1.5 parts by mass of accelerator DTDM, 1 part by mass of accelerator TMTD, and 2.5 parts by mass of accelerator DM were mixed for 25 minutes, and then 20 parts by mass of acid-treated modified carbon black were added and the mixing was continued for 25 minutes. Then, the mixture was vulcanized at 160°C and 15 MPa for 30 minutes to obtain a 2 mm thick carbon black-based electromagnetic shielding composite material.
[0038] The preparation method of the modified carbon black is as follows: 1 part by mass of carbon black is added to 140 parts by mass of nitric acid solution with a mass fraction of 68%, ultrasonically oscillated at 80° C. for 10 hours, filtered, washed with deionized water until the washing liquid is neutral, then dried at 80° C. to constant weight, naturally cooled to room temperature, then added to 140 parts by mass of sensitizing solution A and ultrasonically oscillated at 25° C. for 1 hour, continued to filter, washed with deionized water until the washing liquid is neutral, then dried at 80° C. to constant weight, naturally cooled to room temperature, then added to 140 parts by mass of sensitizing solution B and ultrasonically oscillated at 25° C. for 1 hour, continued to filter, washed with deionized water until the washing liquid is neutral, then dried at 80° C. to constant weight, naturally cooled to room temperature, and finally added to 1000 parts by mass of nickel plating solution, ultrasonically oscillated at 35° C. for 5 minutes, filtered after completion, washed with deionized water 6 times, then dried at 80° C. to constant weight, and naturally cooled to room temperature to obtain the modified carbon black.
[0039] The sensitizing solution A includes tin chloride and hydrogen chloride; wherein the tin chloride content is 20 g / L and the hydrogen chloride concentration is 1 M; the sensitizing solution B includes palladium chloride and hydrogen chloride; wherein the palladium chloride concentration is 1 g / L and the hydrogen chloride concentration is 0.25 M.
[0040] The nickel plating solution is prepared as follows: 5 parts by mass of sodium citrate, 25 parts by mass of nickel (II) sulfate hexahydrate, 15 parts by mass of sodium dihydrogen hypophosphite, 60 parts by mass of ammonium chloride and 1000 parts by mass of deionized water are mixed, and then 28% ammonia water is added to adjust the pH to 9 to obtain a nickel plating solution.
[0041] The preparation method of the pretreated nitrile rubber is as follows: 30 parts by mass of nitrile rubber and 245 parts by mass of tetrahydrofuran are mixed, stirred until the solution is uniform and transparent, then 47 parts by mass of a methanol solution of hydroxylamine hydrochloride and 16 parts by mass of a methanol solution of potassium hydroxide are added, and the mixing is continued for 13 minutes, then the water bath is heated to 50°C, and a condensation reaction is carried out at a speed of 300r / min for 18 hours. During the reaction, 47 parts by mass of a methanol solution of hydroxylamine hydrochloride and 16.16 parts by mass of a methanol solution of potassium hydroxide are added every 6 hours, and then the mixture is washed with water at 40°C deionized water at a rate of 5s / drop to neutrality, and then the mixture is added to 490 parts by mass of ethanol for flocculation and precipitation, and after filtering, the mixture is placed in a 60°C oven and dried to constant weight to obtain the pretreated nitrile rubber.
[0042] The preparation steps of the methanol solution of hydroxylamine hydrochloride are as follows: dissolving hydroxylamine hydrochloride in anhydrous methanol to obtain the methanol solution of hydroxylamine hydrochloride, wherein the mass ratio of hydroxylamine hydrochloride to anhydrous methanol is 7:40; and the mass ratio of potassium hydroxide in the methanol solution is 6.16:10.
[0043] Example 3
[0044] A method for preparing a carbon black-based electromagnetic shielding composite material, the preparation steps are as follows:
[0045] (1) The modified carbon black and 20% concentrated hydrochloric acid were mixed in a volume ratio of 1:1 and stirred for 30 minutes, and then placed in an oven at 120° C. for 80 minutes to obtain acid-treated modified carbon black;
[0046] (2) 100 parts by mass of pretreated nitrile rubber, 5 parts by mass of zinc oxide, 1 part by mass of stearic acid, 2 parts by mass of antioxidant MB, 1 part by mass of antioxidant RD, 1.5 parts by mass of accelerator DTDM, 1 part by mass of accelerator TMTD, and 2.5 parts by mass of accelerator DM were mixed for 30 minutes, and then 22 parts by mass of acid-treated modified carbon black were added and mixed for another 30 minutes. Then, the mixture was vulcanized at 160°C and 15 MPa for 30 minutes to obtain a 2 mm thick carbon black-based electromagnetic shielding composite material.
[0047] The preparation method of the modified carbon black is as follows: 1 part by mass of carbon black is added to 140 parts by mass of nitric acid solution with a mass fraction of 68%, ultrasonically oscillated at 80° C. for 10 hours, filtered, washed with deionized water until the washing liquid is neutral, then dried at 80° C. to constant weight, naturally cooled to room temperature, then added to 140 parts by mass of sensitizing solution A and ultrasonically oscillated at 25° C. for 1 hour, continued to filter, washed with deionized water until the washing liquid is neutral, then dried at 80° C. to constant weight, naturally cooled to room temperature, then added to 140 parts by mass of sensitizing solution B and ultrasonically oscillated at 25° C. for 1 hour, continued to filter, washed with deionized water until the washing liquid is neutral, then dried at 80° C. to constant weight, naturally cooled to room temperature, and finally added to 1000 parts by mass of nickel plating solution, ultrasonically oscillated at 35° C. for 5 minutes, filtered after completion, washed with deionized water 7 times, then dried at 80° C. to constant weight, and naturally cooled to room temperature to obtain the modified carbon black.
[0048] The sensitizing solution A includes tin chloride and hydrogen chloride; wherein the tin chloride content is 20 g / L and the hydrogen chloride concentration is 1 M; the sensitizing solution B includes palladium chloride and hydrogen chloride; wherein the palladium chloride concentration is 1 g / L and the hydrogen chloride concentration is 0.25 M.
[0049] The nickel plating solution is prepared as follows: 5 parts by mass of sodium citrate, 25 parts by mass of nickel (II) sulfate hexahydrate, 15 parts by mass of sodium dihydrogen hypophosphite, 60 parts by mass of ammonium chloride and 1000 parts by mass of deionized water are mixed, and then 28% ammonia water is added to adjust the pH to 9 to obtain a nickel plating solution.
[0050] The preparation method of the pretreated nitrile rubber is as follows: 30 parts by mass of nitrile rubber and 250 parts by mass of tetrahydrofuran are mixed, stirred until the solution is uniform and transparent, then 47 parts by mass of hydroxylamine hydrochloride methanol solution and 16 parts by mass of potassium hydroxide methanol solution are added, and the mixing is continued for 15 minutes, then the water bath is heated to 60°C, and condensation reaction is carried out at a speed of 300r / min for 24 hours. During the reaction, 47 parts by mass of hydroxylamine hydrochloride methanol solution and 16.16 parts by mass of potassium hydroxide methanol solution are added every 6 hours, and then 40°C deionized water is added at a rate of 5s / drop to wash until neutral, and then added to 500 parts by mass of ethanol for flocculation and precipitation, and after filtering, it is placed in a 60°C oven and dried to constant weight to obtain the pretreated nitrile rubber.
[0051] The preparation steps of the methanol solution of hydroxylamine hydrochloride are as follows: dissolving hydroxylamine hydrochloride in anhydrous methanol to obtain the methanol solution of hydroxylamine hydrochloride, wherein the mass ratio of hydroxylamine hydrochloride to anhydrous methanol is 7:40; and the mass ratio of potassium hydroxide in the methanol solution is 6.16:10.
[0052] Comparative Example 1
[0053] The difference between Comparative Example 1 and Example 2 is that only carbon black is used to prepare the carbon black-based electromagnetic shielding composite material, and the remaining steps and components are the same as those of Example 2.
[0054] Comparative Example 2
[0055] The only difference between Comparative Example 2 and Example 2 is that carbon black acidified with hydrochloric acid is used to prepare the carbon black-based electromagnetic shielding composite material; the remaining steps and components are the same as those in Example 2.
[0056] Comparative Example 3
[0057] The only difference between Comparative Example 3 and Example 2 is that the modified carbon black is prepared by using carbon black modified with silane coupling agent KH550, wherein the amount of silane coupling agent added is 0.3 times the mass of carbon black, and the remaining steps and ingredients are the same as those in Example 2.
[0058] Comparative Example 4
[0059] The difference between Comparative Example 4 and Example 2 is that only modified carbon black obtained by nickel plating carbon black is used to prepare the carbon black-based electromagnetic shielding composite material; the remaining steps and ingredients are the same as those in Example 2.
[0060] Comparative Example 5
[0061] The difference between Comparative Example 5 and Example 2 is that only nitrile rubber is used to prepare the carbon black-based electromagnetic shielding composite material; the remaining steps and components are the same as those in Example 2.
[0062] Effect example
[0063] Dispersibility: The dispersion performance of carbon black in the carbon black-based electromagnetic shielding composite materials prepared in the examples and comparative examples was tested using an RCD-II rubber carbon black dispersion tester;
[0064] Electromagnetic shielding effectiveness: Agilent 4396B vector network impedance spectrum analyzer and far-field shielding effectiveness test device were used to test the shielding effectiveness of carbon black-based electromagnetic shielding composite materials. The test frequency was 1.8 GHz.
[0065] Table 1 below lists the performance test analysis results of the carbon black-based electromagnetic shielding composite materials prepared by Examples 1 to 3 and Comparative Examples 1 to 5 of the present invention.
[0066] Table 1
[0067]
[0068] It can be found from Table 1 that the carbon black-based electromagnetic shielding composite material prepared in the embodiment has good electromagnetic shielding performance, carbon black dispersibility, conductivity and mechanical properties; Example 2 is compared with Comparative Examples 1, 2, 3 and 4 to find that the carbon black-based electromagnetic shielding composite material prepared by acid-treated modified carbon black nickel-plated carbon black has good electromagnetic shielding performance, carbon black dispersibility, conductivity and mechanical properties; compared with the traditional coupling agent-modified carbon black, although the dispersibility of carbon black is increased, its conductivity and electromagnetic shielding performance are reduced, and the carbon black-based electromagnetic shielding composite material prepared by the acid-treated modified carbon black nickel-plated carbon black of the present invention has good electromagnetic shielding performance, conductivity and mechanical properties; Example 2 is compared with Comparative Example 5 to find that the nitrile rubber is dissolved in tetrahydrofuran, a methanol solution of hydroxylamine hydrochloride and a methanol solution of potassium hydroxide are added, and then washed, flocculated and dried to obtain the pretreated nitrile rubber, and the carbon black-based electromagnetic shielding composite material has good electromagnetic shielding performance, carbon black dispersibility, conductivity and mechanical properties.
[0069] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
Claims
1. A carbon black-based electromagnetic shielding composite material, It is characterized in that The carbon black-based electromagnetic shielding composite material includes the following raw material components in parts by weight: 100 parts by weight of pretreated nitrile rubber, 5 parts by weight of zinc oxide, 1 part by weight of stearic acid, 2 parts by weight of antioxidant MB, 1 part by weight of antioxidant RD, 1.5 parts by weight of accelerator DTDM, 1 part by weight of accelerator TMTD, 2.5 parts by weight of accelerator DM, and 18 to 22 parts by weight of acid-treated modified carbon black.
2. The carbon black-based electromagnetic shielding composite material according to claim 1, It is characterized in that The pretreated nitrile rubber is obtained by dissolving the nitrile rubber in tetrahydrofuran, adding a methanol solution of hydroxylamine hydrochloride and a methanol solution of potassium hydroxide, and then washing, flocculating and drying.
3. The carbon black-based electromagnetic shielding composite material according to claim 1, It is characterized in that The acid-treated modified carbon black is obtained by mixing the modified carbon black in concentrated hydrochloric acid and then drying it.
4. The carbon black-based electromagnetic shielding composite material according to claim 1, It is characterized in that The modified carbon black is obtained by oxidizing carbon black, then performing sensitization twice and nickel plating.
5. A method for preparing the carbon black-based electromagnetic shielding composite material according to any one of claims 1 to 4, It is characterized in that The method comprises the following preparation steps: (1) The modified carbon black and 20% concentrated hydrochloric acid were mixed in a volume ratio of 1:1 and stirred for 20 to 30 minutes, and then placed in an oven at 100 to 120° C. for 40 to 80 minutes to obtain acid-treated modified carbon black; (2) 100 parts by mass of pretreated nitrile rubber, 5 parts by mass of zinc oxide, 1 part by mass of stearic acid, 2 parts by mass of antioxidant MB, 1 part by mass of antioxidant RD, 1.5 parts by mass of accelerator DTDM, 1 part by mass of accelerator TMTD, and 2.5 parts by mass of accelerator DM were mixed for 20 to 30 minutes, and then 18 to 22 parts by mass of acid-treated modified carbon black were added and mixed for another 20 to 30 minutes. Then, the mixture was vulcanized at 160°C and 15 MPa for 30 minutes to obtain a 2 mm thick carbon black-based electromagnetic shielding composite material.
6. The method for preparing the carbon black-based electromagnetic shielding composite material according to claim 5, It is characterized in that The preparation method of the modified carbon black is as follows: 1 part by mass of carbon black is added to 140 parts by mass of nitric acid solution with a mass fraction of 68%, ultrasonically oscillated at 80° C. for 10 hours, filtered, washed with deionized water until the washing liquid is neutral, then dried at 80° C. to constant weight, naturally cooled to room temperature, then added to 140 parts by mass of sensitizing solution A and ultrasonically oscillated at 25° C. for 1 hour, continued to filter, washed with deionized water until the washing liquid is neutral, then dried at 80° C. to constant weight, naturally cooled to room temperature, then added to 140 parts by mass of sensitizing solution B and ultrasonically oscillated at 25° C. for 1 hour, continued to filter, washed with deionized water until the washing liquid is neutral, then dried at 80° C. to constant weight, naturally cooled to room temperature, finally added to 1000 parts by mass of nickel plating solution, ultrasonically oscillated at 35° C. for 5 minutes, filtered after completion, washed with deionized water for 5 to 7 times, then dried at 80° C. to constant weight, and naturally cooled to room temperature to obtain the modified carbon black.
7. The method for preparing the carbon black-based electromagnetic shielding composite material according to claim 6, It is characterized in that The sensitizing solution A includes tin chloride and hydrogen chloride; wherein the tin chloride content is 20 g / L and the hydrogen chloride concentration is 1 M; the sensitizing solution B includes palladium chloride and hydrogen chloride; wherein the palladium chloride concentration is 1 g / L and the hydrogen chloride concentration is 0.25 M.
8. The method for preparing the carbon black-based electromagnetic shielding composite material according to claim 6, It is characterized in that The nickel plating solution is prepared as follows: 5 parts by mass of sodium citrate, 25 parts by mass of nickel (II) sulfate hexahydrate, 15 parts by mass of sodium dihydrogen hypophosphite, 60 parts by mass of ammonium chloride and 1000 parts by mass of deionized water are mixed, and then 28% ammonia water is added to adjust the pH to 9 to obtain a nickel plating solution.
9. The method for preparing the carbon black-based electromagnetic shielding composite material according to claim 5, It is characterized in that The preparation method of the pretreated nitrile rubber is as follows: 30 parts by mass of nitrile rubber and 240-250 parts by mass of tetrahydrofuran are mixed, stirred until the solution is uniform and transparent, then 47 parts by mass of hydroxylamine hydrochloride methanol solution and 16 parts by mass of potassium hydroxide methanol solution are added, and the mixing is continued for 10-15 minutes, then the water bath is heated to 40-60°C, and the condensation reaction is carried out at a speed of 300r / min for 12-24 hours. During the reaction, 47 parts by mass of hydroxylamine hydrochloride methanol solution and 16.16 parts by mass of potassium hydroxide methanol solution are added every 6 hours, and then the nitrile rubber is washed with water at 40°C at a rate of 5s / drop to neutrality, and then added to 480-500 parts by mass of ethanol for flocculation and precipitation, filtered, and then placed in a 60°C oven to dry to constant weight to obtain the pretreated nitrile rubber.
10. The method for preparing the carbon black-based electromagnetic shielding composite material according to claim 9, It is characterized in that The preparation steps of the methanol solution of hydroxylamine hydrochloride are as follows: dissolving hydroxylamine hydrochloride in anhydrous methanol to obtain the methanol solution of hydroxylamine hydrochloride, wherein the mass ratio of hydroxylamine hydrochloride to anhydrous methanol is 7:40; and the mass ratio of potassium hydroxide in the methanol solution is 6.16:10.
Citation Information
Patent Citations
Electromagnetic shielding rubber with high thermal conductivity, preparation method and application thereof
CN107236161A
Preparation method of wear-resistant aging-resistant rubber compound filled with coupling modified wood fiber
CN109054119A
Silicone rubber lightweight ablation-resistant electromagnetic shielding coating material and application thereof
CN115537117A
Aminoxime functionalized nitrile rubber as well as preparation method and application thereof
CN117659228A
Cited By
Rapidly vulcanized amidoxime modified nitrile rubber as well as preparation method and application thereof
CN120040851A