SiOC ceramic and preparation method thereof

By assembling the ceramic fiber membrane and the honeycomb structure ceramic precursor and performing ultraviolet curing and pyrolysis treatment, SiOC ceramics with ceramic fiber membrane structure are formed, which solves the problem of poor thermal insulation effect of honeycomb SiOC materials and achieves lightweight, high strength and SiOC ceramic with excellent thermal insulation performance.

CN118930306AActive Publication Date: 2024-11-12INST OF METAL RESEARCH - CHINESE ACAD OF SCI

Patent Information

Application Number
CN202411158714.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-12
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The thermal insulation effect of honeycomb SiOC materials is poor, which limits its widespread application.

Method used

By assembling the ceramic fiber membrane precursor with the honeycomb structure ceramic precursor body, the SiOC ceramic with the ceramic fiber membrane structure is formed, and the through-holes of the honeycomb structure are covered with the fiber membrane to reduce heat conduction and convection efficiency .

Benefits of technology

The lightweight, high-strength performance and excellent thermal insulation properties of SiOC ceramics are achieved, with thermal conductivity of 0.04-0.15W/(m·K), back temperature of 500℃-1000℃, and compression strength of 5-15MPa, which significantly improves Thermal insulation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930306A_ABST
    Figure CN118930306A_ABST
Patent Text Reader

Abstract

The invention provides SiOC ceramic and a preparation method thereof, and relates to the technical field of thermal insulation materials, and the preparation method comprises the following steps: respectively preparing a ceramic precursor blank and a ceramic fiber membrane precursor; the ceramic precursor blank is of a honeycomb structure; carrying out assembly treatment on the ceramic fiber membrane precursor and the ceramic precursor blank to enable the ceramic fiber membrane precursor to cover the through holes of the honeycomb structure to obtain an assembly, and then carrying out ultraviolet curing on the assembly; and performing pyrolysis treatment on the assembly subjected to ultraviolet curing to obtain the SiOC ceramic. According to the preparation method, the ceramic precursor blank and the ceramic fiber membrane precursor are assembled and then subjected to ultraviolet curing and pyrolysis treatment, and the obtained SiOC ceramic not only has the light and high-strength performance of a porous ceramic material, but also has the excellent heat insulation performance of a ceramic fiber membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermal insulation materials, and in particular relates to a SiOC ceramic and a preparation method thereof. Background Art

[0002] With the rapid development of mechanical processing technology and the increasing demand for lightweight and efficient materials in aerospace, shipbuilding and other fields, lightweight porous materials have become the focus of material application in these fields. Porous materials have good load-bearing capacity, energy absorption performance and anti-buckling ability, and can still maintain good strength when subjected to strong compressive loads, so they have been widely used.

[0003] Polymer-derived ceramics (PDCs) prepared by pyrolysis of polymer ceramic precursors have significant properties of traditional ceramics, such as high thermal stability, chemical resistance to oxidative corrosion, and mechanical resistance to friction. Among PDCs, SiOC ceramics have enhanced thermal, mechanical, and chemical properties compared to pure silica ceramics, and can operate at a maximum temperature of 1200°C, and are currently used in thermal protection systems. However, SiOC ceramics are prone to breakage during sintering, and the temperature gradient can be mitigated by selecting a suitable porous structure, resulting in a very uniform shrinkage during pyrolysis, thereby reducing cracking.

[0004] Porous materials come in many forms, among which bionic porous materials have the unique advantage that their structural properties can be precisely controlled. Their mechanical properties can be precisely controlled through finite element simulation, prototype trial production, and other methods. Typical bionic porous materials such as honeycomb structures have been widely used in aircraft landing gear doors, panels, and other parts. The natural honeycomb structure is composed of evenly distributed double-layer hexagons, is symmetrical in two dimensions, is lightweight, and is relatively strong in both tension and compression, meeting the requirements of lightweight and high-strength thermal insulation materials. However, since the macroscopic pores of the honeycomb structure cannot block thermal radiation and convection, the thermal insulation effect of the honeycomb SiOC material is poor, which limits the widespread application of the honeycomb SiOC material. Summary of the invention

[0005] Therefore, the present invention provides a SiOC ceramic and a preparation method thereof, which can solve the technical problem of poor thermal insulation effect of honeycomb SiOC materials in the prior art.

[0006] In order to solve the above problems, the present invention provides a method for preparing SiOC ceramics, comprising the following steps:

[0007] Step 1) preparing a ceramic precursor body and a ceramic fiber membrane precursor respectively; wherein the ceramic precursor body is a honeycomb structure;

[0008] Step 2) assembling the ceramic fiber membrane precursor and the ceramic precursor body so that the ceramic fiber membrane precursor covers the through holes of the honeycomb structure to obtain an assembly, and then UV curing the assembly;

[0009] Step 3) The UV-cured assembly is subjected to pyrolysis treatment to obtain SiOC ceramics.

[0010] Furthermore, in step 1), the step of preparing the ceramic precursor body comprises:

[0011] Mixing a polysiloxane solution and a photoinitiator to obtain a photosensitive ceramic precursor slurry; then performing a first photocuring treatment on the photosensitive ceramic precursor slurry to obtain a ceramic precursor body;

[0012] Wherein, the mass of the photoinitiator is 0.5% to 3% of the mass of the polysiloxane solution.

[0013] Furthermore, the polysiloxane solution is an acrylate group siloxane solution; and / or,

[0014] The photoinitiator is one or more of diphenyl-2,4,6-trimethylbenzoyl-phosphine oxide, phenyl bis-2,4,6-trimethylbenzoyl-phosphine oxide, and 2,4,6-trimethylbenzoyl ethyl phosphate; and / or,

[0015] Placing the photosensitive ceramic precursor slurry in a photocuring device to perform a first photocuring treatment;

[0016] Preferably, the parameters of the light curing device are set as follows: layer thickness is 1-300 μm, exposure intensity is 1-100 mW / cm 2 , exposure time is 0.5-30s, speed is 0.1-300mm / min.

[0017] Further, in the step 1): the thickness of the ceramic fiber membrane precursor is 100-500 μm; and / or

[0018] The preparation steps of the ceramic fiber membrane precursor include: dissolving a polysiloxane solution, a spinning aid and a photoinitiator in a volatile solvent to obtain a spinning solution; then electrostatically spinning the spinning solution and simultaneously performing a second photocuring treatment to obtain a ceramic fiber membrane precursor;

[0019] Preferably, the photoinitiator is one or more of TPO free radical initiator, 819 free radical initiator, and TPO-L free radical initiator;

[0020] Preferably, the exposure intensity of the second light curing treatment is 40-100 mW / cm 2 .

[0021] Further, the spinning solution comprises the following components by mass percentage: polysiloxane solution: 15-40%, spinning aid: 5-15%, initiator: 0.1-5%, volatile solvent: 40-70%;

[0022] Preferably, the spinning aid is one of polyvinyl pyrrolidone and polyethylene oxide;

[0023] Preferably, the volatile solvent is one of ethanol and isopropanol.

[0024] Furthermore, the wall thickness of the honeycomb structure is 0.5-10 mm;

[0025] Furthermore, the ceramic precursor body is a single-layer honeycomb structure or a double-layer honeycomb structure;

[0026] When the ceramic precursor green body is a single-layer honeycomb structure, the assembly process includes: stacking two ceramic precursor green bodies to obtain a stacked green body, and then respectively applying a ceramic fiber membrane precursor between the two single-layer honeycomb structures of the stacked green body and on the surface where the through holes of the stacked green body are located;

[0027] When the ceramic precursor blank is a double-layer honeycomb structure, the assembly process includes: pasting a ceramic fiber membrane precursor on the surface where the through hole of the ceramic precursor blank is located;

[0028] Preferably, in the double-layer honeycomb structure, the contact area between the upper layer and the lower layer accounts for 50%-100% of the upper surface area of ​​the lower layer;

[0029] Preferably, the number of coating layers of the ceramic fiber membrane precursor is 1-10 layers.

[0030] Furthermore, in step 2), the parameters of UV curing are: the irradiation intensity of the UV lamp is 40-100 mW / cm 2 ; The wavelength of the UV lamp is 365-405nm; the curing time is 5-20min.

[0031] Further, in step 3), the pyrolysis treatment includes:

[0032] In an inert atmosphere, heating the UV-cured assembly to 800-1200° C., keeping the temperature for 0.5-10 hours, and then cooling to room temperature to obtain the SiOC ceramic;

[0033] Preferably, the inert atmosphere is argon;

[0034] Preferably, the heating rate of the UV-cured assembly when heated to 800-1200° C. is 1-10° C. / min.

[0035] On the other hand, the present invention provides a SiOC ceramic, the SiOC ceramic comprising a ceramic fiber membrane structure and a SiOC ceramic honeycomb structure arranged opposite to each other; the ceramic fiber membrane structure covers the through holes of the SiOC ceramic honeycomb structure;

[0036] The thermal conductivity of the SiOC ceramic is 0.04-0.15 W / (m·K); the back temperature of the SiOC ceramic is 500° C.-1000° C.; the compressive strength of the SiOC ceramic is 5-15 MPa;

[0037] Preferably, the SiOC ceramic is obtained by any of the preparation methods described above.

[0038] The SiOC ceramic and the preparation method thereof provided by the present invention have the following beneficial effects:

[0039] 1. The present invention assembles a ceramic precursor body and a ceramic fiber membrane precursor and then performs UV curing and pyrolysis treatment, so that the obtained SiOC ceramic not only has the light weight and high strength properties of porous ceramic materials, but also has the excellent thermal insulation properties of ceramic fiber membranes; wherein, the ceramic precursor body is a honeycomb structure, and the ceramic fiber membrane precursor covers the through holes of the honeycomb structure. When heat is transferred to the above-mentioned SiOC ceramic, it first contacts the ceramic fiber membrane precursor. Since both the ceramic precursor body and the ceramic fiber membrane have high porosity, the probability of phonon collision is reduced, resulting in reduced solid-state heat conduction; at the same time, the staggered fibers will hinder the flow of gas, reduce the probability of gas molecules colliding with each other inside the material, thereby reducing the thermal convection efficiency, and when the heat flow reaches the inside of the SiOC ceramic, the heat transfer efficiency is significantly reduced due to the complex heat transfer path at the overlap; in addition, under high temperature conditions, the surface of the object becomes unstable, resulting in the inability to effectively transfer heat through the surface of the object, which also leads to a reduction in thermal conduction efficiency. The lower the thermal convection efficiency and heat transfer (heat conduction) efficiency, the better the thermal insulation performance.

[0040] 2. Furthermore, when the ceramic precursor body is a single-layer honeycomb structure, two ceramic precursor bodies are stacked to obtain a stacked body, and then ceramic fiber membrane precursors are respectively applied between the two single-layer honeycomb structures of the stacked body and on the surface where the through holes of the stacked body are located; since thermal radiation is the main way of heat transfer in a high-temperature environment, adding a ceramic fiber membrane precursor in the middle can absorb thermal radiation, convert it into heat energy and disperse it into the interior of the material, thereby further improving the thermal insulation performance of SiOC ceramics.

[0041] 3. Furthermore, the present invention limits the UV curing time to 5-20 minutes to ensure that the sample has the most complete morphology and obtains better mechanical properties. If the curing time is too short, it will lead to a low curing depth and poor interlayer bonding between the printed layers, so the layers are prone to falling off, and the falling layers will be partially bonded to the SiOC ceramic sample, causing the final SiOC ceramic to deform after repeated exposure; if the curing time is too long, the penetration depth of the ultraviolet light is much greater than the layer thickness, resulting in more serious excess curing, which will clog the internal structure of the SiOC ceramic sample and fail to form a complete porous structure. Therefore, curing time that is too long or too short will reduce the mechanical properties.

[0042] 4. Furthermore, the present invention sets the number of layers of the ceramic fiber membrane precursor to 1-10 layers. This is because when the number of membrane layers is too large, additional slurry needs to be added to promote the assembly of the fiber membrane and the precursor body, resulting in a poor bonding effect. After heat treatment, the fiber membrane on the outside of the sample is deformed, such as cracking or warping, and the sample preparation fails, thereby affecting the thermal insulation properties of the SiOC ceramic. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. The drawings described below are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.

[0044] Figure 1 is a physical picture of the ceramic precursor body prepared in Example 1;

[0045] Figure 2 is a morphology diagram of the ceramic fiber membrane precursor prepared in Example 1;

[0046] Figure 3 is a physical picture of the SiOC ceramic prepared in Example 1;

[0047] Figure 4 is a physical picture of the layer ceramic precursor body prepared in Example 2;

[0048] Figure 5 is a physical picture of the SiOC ceramic prepared in Example 3;

[0049] Figure 6 This is a thermal test diagram of Examples 1 and 3 of the present invention;

[0050] Figure 7 This is a thermal assessment experiment diagram of Example 2 of the present invention;

[0051] Figure 8It is a mechanical property experimental diagram of Examples 1 and 3 and Comparative Example 1 in the present invention. DETAILED DESCRIPTION

[0052] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. The drawings described below are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.

[0053] A method for preparing SiOC ceramics comprises the following steps:

[0054] Step 1) preparing a ceramic precursor body and a ceramic fiber membrane precursor respectively; wherein the ceramic precursor body is a honeycomb structure;

[0055] Step 2) assembling the ceramic fiber membrane precursor and the ceramic precursor body so that the ceramic fiber membrane precursor covers the through holes of the honeycomb structure to obtain an assembly, and then UV curing the assembly;

[0056] Step 3) The UV-cured assembly is subjected to pyrolysis treatment to obtain SiOC ceramics.

[0057] Based on the above method, the ceramic precursor body with honeycomb structure has relatively higher mechanical strength, and the ceramic fiber membrane has relatively lower thermal conductivity. After combining the two, SiOC ceramics with lighter weight, better thermal insulation performance and sufficient mechanical properties can be obtained.

[0058] In some embodiments, in step 1), the step of preparing a ceramic precursor body comprises:

[0059] Mixing a polysiloxane solution and a photoinitiator to obtain a photosensitive ceramic precursor slurry; then performing a first photocuring treatment on the photosensitive ceramic precursor slurry to obtain a ceramic precursor body;

[0060] The mass of the photoinitiator is 0.5% to 3% of the mass of the polysiloxane solution.

[0061] In some embodiments, the polysiloxane solution is an acrylate group siloxane solution; and / or,

[0062] The photoinitiator is one or more of diphenyl-2,4,6-trimethylbenzoyl-phosphine oxide (TPO free radical initiator), phenyl bis-2,4,6-trimethylbenzoyl-phosphine oxide (819 free radical initiator), and 2,4,6-trimethylbenzoyl ethyl phosphate (TPO-L free radical initiator); and / or,

[0063] Placing the photosensitive ceramic precursor slurry in a photocuring device to perform a first photocuring treatment;

[0064] Preferably, the parameters of the light curing device are set as follows: layer thickness is 1-300 μm, exposure intensity is 1-100 mW / cm 2 , exposure time is 0.5-30s, speed is 0.1-300mm / min.

[0065] In some embodiments, in step 1): the thickness of the ceramic fiber membrane precursor is 100-500 μm; and / or

[0066] The steps for preparing a ceramic fiber membrane precursor include:

[0067] The polysiloxane solution, the spinning aid and the photoinitiator are dissolved in a volatile solvent to obtain a spinning solution; the spinning solution is then subjected to electrostatic spinning and a second photocuring treatment to obtain a ceramic fiber membrane precursor;

[0068] Preferably, the photoinitiator is one or more of TPO free radical initiator, 819 free radical initiator, and TPO-L free radical initiator;

[0069] Preferably, the exposure intensity of the second light curing treatment is 40-100 mW / cm 2 .

[0070] In some embodiments, the spinning solution includes the following components by mass percentage: polysiloxane solution: 15-40%, spinning aid: 5-15%, initiator: 0.1-5%, volatile solvent: 40-70%;

[0071] Preferably, the spinning aid is one of polyvinyl pyrrolidone and polyethylene oxide;

[0072] Preferably, the volatile solvent is one of ethanol and isopropanol.

[0073] In some embodiments, the honeycomb structure has a wall thickness of 0.5-10 mm.

[0074] In some embodiments, the ceramic precursor body is a single-layer honeycomb structure or a double-layer honeycomb structure;

[0075] When the ceramic precursor green body is a single-layer honeycomb structure, the assembly process includes: stacking two ceramic precursor green bodies to obtain a stacked green body, and then respectively applying a ceramic fiber membrane precursor between the two single-layer honeycomb structures of the stacked green body and on the surface where the through holes of the stacked green body are located;

[0076] When the ceramic precursor blank is a double-layer honeycomb structure, the assembly process includes: laminating the ceramic fiber membrane precursor on the surface where the through hole of the ceramic precursor blank is located;

[0077] Preferably, in the double-layer honeycomb structure, the contact area between the upper layer and the lower layer accounts for 50%-100% of the upper surface area of ​​the lower layer; if the contact area between the upper layer and the lower layer accounts for too small a proportion of the upper surface area of ​​the lower layer, the force is easily uneven during the compression test, and the stress concentration is too large, resulting in a decrease in the mechanical properties of the ceramic precursor body;

[0078] Preferably, the number of coating layers of the ceramic fiber membrane precursor is 1-10. When the number of coating layers exceeds 10, the layers after the 10th layer are not bonded to each other, and the outer layer membrane will bulge and crack after heat treatment, resulting in failure in the preparation of SiOC ceramic samples.

[0079] In some embodiments, in step 2), the parameters of UV curing are: the irradiation intensity of the UV lamp is 40-100 mW / cm 2 ; The wavelength of the ultraviolet lamp is 365-405nm; The curing time is 5-20min. When the curing time is less than 5min, the combination effect of the assembly is poor, so that the fiber membrane will warp or crack after heat treatment, resulting in the failure of the preparation of the SiOC ceramic sample; when the curing time is greater than 20min, the time cost will increase.

[0080] In some embodiments, in step 3): pyrolysis treatment comprises:

[0081] In an inert atmosphere, the UV-cured assembly is heated to 800-1200° C., kept at this temperature for 0.5-10 hours, and then cooled to room temperature to obtain SiOC ceramics;

[0082] Preferably, the inert atmosphere is argon;

[0083] Preferably, the heating rate when the UV-cured assembly is heated to 800-1200° C. is 1-10° C. / min.

[0084] On the other hand, SiOC ceramics include a ceramic fiber membrane structure and a SiOC ceramic honeycomb structure that are relatively arranged; the ceramic fiber membrane structure covers the through holes of the SiOC ceramic honeycomb structure; the thermal conductivity of SiOC ceramics is 0.04-0.15W / (m·K); the back temperature of SiOC ceramics is 500℃-1000℃; the compressive strength of SiOC ceramics is 5-15MPa;

[0085] Wherein, the layered honeycomb structure is a single-layer honeycomb structure or a double-layer honeycomb structure. If the layered honeycomb structure is a single-layer honeycomb structure, then the ceramic fiber membrane structures are 2; if the honeycomb structure is a double-layer honeycomb structure, then the ceramic fiber membrane structures are 3; the ceramic fiber membrane structure is 1-10 layers of ceramic fiber membranes bonded together;

[0086] Preferably, the SiOC ceramic is obtained by any of the preparation methods described above.

[0087] The present invention is further described below in conjunction with specific embodiments and comparative examples. Among them, the ceramic precursor blank is formed by photocuring printing (first photocuring treatment) of a polysiloxane solution, and the ceramic precursor blank itself carries a slurry (polysiloxane solution) when it is just printed. The slurry carried by the ceramic precursor blank itself can be used to adhere the ceramic fiber film precursor to the precursor blank, but as the number of fiber film layers increases, the slurry carried by the precursor blank itself is not enough to adhere the outermost fiber film, therefore, the polysiloxane solution can be coated on the ceramic fiber film precursor so that the ceramic fiber film precursor can be attached to the surface of the ceramic precursor blank (honeycomb structure); the polysiloxane solution used is the same as the polysiloxane solution used to prepare the ceramic precursor blank.

[0088] Example 1

[0089] This embodiment provides a method for preparing SiOC ceramics, comprising the following steps:

[0090] Step 1)

[0091] Preparation of ceramic precursor green body:

[0092] Establishing the model: According to the optical photographs and SEM microscopic photographs of the honeycomb cross section of the honeycomb structure, the characteristic dimensions of the ceramic precursor body are obtained, and the model of the SiOC ceramic precursor body is established in the three-dimensional drawing software for subsequent additive manufacturing; wherein the honeycomb structure is double-layered; the contact area between the upper layer and the lower layer accounts for 100% of the upper surface area of ​​the lower layer; the wall thickness of the honeycomb structure is 0.5 mm;

[0093] Preparation of photosensitive ceramic precursor slurry: weigh 0.4g of 819 free radical photoinitiator and dissolve it in 40g of methyl-terminated acrylate polysiloxane (polysiloxane solution), then place it on a magnetic stirrer and stir it at a speed of 500rpm for 30min to obtain a clear and transparent 1wt.% photosensitive polysiloxane solution (photosensitive ceramic precursor slurry); the viscosity of the obtained photosensitive ceramic precursor slurry is 181cps; wherein, the molecular weight Mw of methyl-terminated acrylate polysiloxane is 4000-7000;

[0094] Additive manufacturing: The photosensitive ceramic precursor slurry is placed in a stereolithography 3D printing device for a first light curing process to obtain a ceramic precursor blank with a honeycomb structure; wherein the setting parameters of the stereolithography 3D printing device are: the layer thickness is set to 80μm, and the exposure intensity is set to 20mW / cm 2 , the exposure time was set to 3s, and the speed was set to 5mm / min.

[0095] Preparation of ceramic fiber membrane precursor:

[0096] Prepare a photosensitive mixed spinning solution: weigh 20g of methyl-terminated acrylate polysiloxane (polysiloxane solution) into a beaker, then add 0.2g of 819 (initiator) into the beaker, shake gently and disperse ultrasonically until the solution is clear to obtain a clear and transparent photosensitive polysiloxane solution; then dissolve 2g of PVP powder (spinning aid) in 10g of anhydrous ethanol (volatile solvent), stir for 4h, and prepare a PVP solution with a mass fraction of 20wt%; then, take 1wt.% of the photosensitive polysiloxane solution and an appropriate amount of PVP solution and place them on a magnetic stirrer for 5h to mix, and obtain a stable spinning solution. The mass ratio of PVP solution to photosensitive polysiloxane solution is 3:1. In terms of mass percentage, the spinning solution includes 25% of polysiloxane solution, 12.5% ​​of spinning aid, and 62.5% of volatile solvent;

[0097] Solidification spinning: The above-mentioned photosensitive mixed spinning solution was placed in a 5 ml disposable syringe, which was installed on the electrospinning machine platform at a pushing speed of 1 ml / h. During the process, a high voltage of 15 kV was applied, and a high-power ultraviolet lamp (80 mW / cm 2 ) is subjected to a second photocuring treatment, and a ceramic fiber membrane precursor is obtained by stretching and curing under a high-voltage electrostatic field, and cross-linking is induced under high-power ultraviolet irradiation, and the spinning time is 60 minutes.

[0098] Step 2) Cut the ceramic fiber membrane precursor into 30×30 mm 2 The size of the ceramic precursor body is applied layer by layer to the upper and lower surfaces of the ceramic precursor body through a polysiloxane solution, so that the ceramic fiber membrane precursor covers the through holes of the honeycomb structure to obtain an assembly, which is a structure of "fiber membrane-body-fiber membrane (i.e., ceramic fiber membrane precursor-ceramic precursor body-ceramic fiber membrane precursor)", and then the assembly is UV-cured; wherein, the upper and lower surfaces of the ceramic precursor body are respectively covered with 5 layers of membrane, and the average thickness of each layer of membrane is 500 μm; the power of the UV lamp during UV curing is 50 mW / cm 2 , wavelength is 365nm, and curing time is 5min.

[0099] Step 3) placing the UV-cured assembly into a pyrolysis treatment furnace, heating it to 1000° C., and then keeping it at 1000° C. for 1 hour to obtain SiOC ceramics; wherein the heating rate is 1° C. / min.

[0100] The ceramic precursor body structure, the microscopic morphology of the silicon oxygen carbon ceramic fiber membrane (ceramic fiber membrane precursor) and the SiOC ceramic object prepared in this embodiment are shown in FIG. Figure 1 , 2 and 3. From Figure 2It can be seen that the silicon oxygen carbon ceramic fiber membrane of this embodiment has uniform fiber diameter and smooth surface. The thermal conductivity of the SiOC ceramic prepared in this embodiment is 0.09W / (m·K), and the surface temperature is 210.1°C after 800°C back temperature test for 20 minutes.

[0101] Example 2

[0102] This embodiment provides a method for preparing SiOC ceramics, comprising the following steps:

[0103] Step 1)

[0104] Preparation of ceramic precursor body:

[0105] Establishing the model: According to the optical photographs and SEM microscopic photographs of the honeycomb cross section of the honeycomb structure, the characteristic dimensions of the ceramic precursor body are obtained, and the model of the SiOC ceramic precursor body is established in the 3D drawing software for subsequent additive manufacturing; the honeycomb structure is double-layered, and the contact area between the upper layer and the lower layer accounts for 90% of the upper surface area of ​​the lower layer; the wall thickness of the honeycomb structure is 0.5 mm;

[0106] Preparation of photosensitive ceramic precursor slurry: Weigh 0.4 g of 819 free radical photoinitiator and dissolve it in 40 g of methyl-terminated acrylate polysiloxane (same as in Example 1), then place it on a magnetic stirrer and stir it at 500 rpm for 30 minutes to obtain a clear and transparent 1 wt.% photosensitive polysiloxane solution (photosensitive ceramic precursor slurry); the viscosity of the obtained photosensitive ceramic precursor slurry is 181 cps;

[0107] Additive manufacturing: The photosensitive ceramic precursor slurry is placed in a stereolithography 3D printing device for a first light curing process to obtain a ceramic precursor blank with a honeycomb structure; wherein the setting parameters of the stereolithography 3D printing device are: the layer thickness is set to 80μm, and the exposure intensity is set to 20mW / cm 2 , the exposure time was set to 3s, and the speed was set to 5mm / min.

[0108] Preparation of ceramic fiber membrane precursor:

[0109] Prepare a photosensitive mixed spinning solution: weigh 20g of methyl-terminated acrylate polysiloxane (polysiloxane solution) into a beaker, then add 0.2g of 819 (initiator) into the beaker, shake gently and disperse ultrasonically until the solution is clear to obtain a clear and transparent photosensitive polysiloxane solution; then dissolve 2g of PVP powder (spinning aid) in 10g of anhydrous ethanol (volatile solvent), stir for 4h, and prepare a PVP solution with a mass fraction of 20wt%; then, take 1wt.% of the photosensitive polysiloxane solution and an appropriate amount of PVP solution and place them on a magnetic stirrer for 5h to mix, and obtain a stable spinning solution. The mass ratio of PVP solution to photosensitive polysiloxane solution is 3:1. In terms of mass percentage, the spinning solution includes 25% of polysiloxane solution, 12.5% ​​of spinning aid, and 62.5% of volatile solvent;

[0110] Solidification spinning: The above-mentioned photosensitive mixed spinning solution was placed in a 5 ml disposable syringe, which was installed on the electrospinning machine platform at a pushing speed of 1 ml / h. During the process, a high voltage of 15 kV was applied, and a high-power ultraviolet lamp (80 mW / cm 2 ) is subjected to a second photocuring treatment, and a ceramic fiber membrane precursor is obtained by stretching and curing under a high-voltage electrostatic field, and cross-linking is induced under high-power ultraviolet irradiation, and the spinning time is 60 minutes.

[0111] Step 2) Cut the ceramic fiber membrane precursor into 30×30 mm 2 The size of the ceramic precursor body is applied layer by layer to the upper and lower surfaces of the ceramic precursor body through a polysiloxane solution, so that the ceramic fiber membrane precursor covers the through holes of the honeycomb structure to obtain an assembly, which is a "fiber membrane-body-fiber membrane" structure, and then the assembly is UV-cured; wherein, the upper and lower surfaces of the ceramic precursor body are respectively covered with 5 layers of membrane, and the average thickness of each layer of membrane is 500μm; the power of the UV lamp during UV curing is 50mW / cm 2 , wavelength is 365nm, and curing time is 5min.

[0112] Step 3) placing the UV-cured assembly into a pyrolysis treatment furnace, heating it to 1000° C., and then keeping it at 1000° C. for 1 hour to obtain SiOC ceramics; wherein the heating rate is 1° C. / min.

[0113] The structure of the ceramic precursor body prepared in this embodiment is as follows Figure 4 The thermal conductivity of the SiOC ceramic prepared in this embodiment is 0.1 W / (m·K), and the surface temperature is 199.7°C after 800°C back temperature test for 20 minutes.

[0114] Example 3

[0115] This embodiment provides a method for preparing SiOC ceramics, comprising the following steps:

[0116] Step 1)

[0117] Preparation of ceramic precursor green body:

[0118] Model building: According to the optical photographs of the honeycomb cross section and the SEM microscopic photographs of the honeycomb structure, the characteristic dimensions of the ceramic precursor body are obtained, and the model of the SiOC ceramic precursor body is built in the three-dimensional drawing software for subsequent additive manufacturing. Among them, the honeycomb structure is a single layer, so two ceramic precursor bodies are prepared; the wall thickness of the honeycomb structure is 0.5 mm;

[0119] Preparation of photosensitive ceramic precursor slurry: Weigh 0.4g of 819 free radical photoinitiator and dissolve it in 40g of methyl-terminated acrylate polysiloxane (same as Example 1), then place it on a magnetic stirrer and stir it at 500rpm for 30min to obtain a clear and transparent 1wt.% photosensitive polysiloxane solution (photosensitive ceramic precursor slurry); the viscosity of the obtained photosensitive ceramic precursor slurry is 181cps;

[0120] Additive manufacturing: The photosensitive ceramic precursor slurry is placed in a stereolithography 3D printing device for a first light curing process to obtain a ceramic precursor blank with a honeycomb structure; wherein the setting parameters of the stereolithography 3D printing device are: the layer thickness is set to 80μm, and the exposure intensity is set to 20mW / cm 2 , the exposure time was set to 3s, and the speed was set to 5mm / min.

[0121] Preparation of ceramic fiber membrane precursor:

[0122] Prepare a photosensitive mixed spinning solution: weigh 20g of methyl-terminated acrylate polysiloxane (polysiloxane solution) into a beaker, then add 0.2g of 819 (initiator) into the beaker, shake gently and disperse ultrasonically until the solution is clear to obtain a clear and transparent photosensitive polysiloxane solution; then dissolve 2g of PVP powder (spinning aid) in 10g of anhydrous ethanol (volatile solvent), stir for 4h, and prepare a PVP solution with a mass fraction of 20wt%; then, take 1wt.% of the photosensitive polysiloxane solution and an appropriate amount of PVP solution and place them on a magnetic stirrer for 5h to mix, and obtain a stable spinning solution. The mass ratio of PVP solution to photosensitive polysiloxane solution is 3:1. In terms of mass percentage, the spinning solution includes 25% of polysiloxane solution, 12.5% ​​of spinning aid, and 62.5% of volatile solvent;

[0123] Solidification spinning: The above-mentioned photosensitive mixed spinning solution was placed in a 5 ml disposable syringe, which was installed on the electrospinning machine platform at a pushing speed of 1 ml / h. During the process, a high voltage of 15 kV was applied, and a high-power ultraviolet lamp (80 mW / cm 2 ) is subjected to a second photocuring treatment, and a ceramic fiber membrane precursor is obtained by stretching and curing under a high-voltage electrostatic field, and cross-linking is induced under high-power ultraviolet irradiation, and the spinning time is 60 minutes.

[0124] Step 2) Cut the ceramic fiber membrane precursor into 30×30 mm 2 The size of the two ceramic precursor green bodies is stacked. When stacking, the two green bodies are completely aligned, that is, the contact area between the upper layer and the lower layer accounts for 100% of the upper surface area of ​​the lower layer, and 5 layers of ceramic fiber membrane precursor are successively pasted between the two, and then 5 layers of ceramic fiber membrane precursor are respectively pasted on the upper and lower surfaces of the stacked green bodies, so that the ceramic fiber membrane precursor covers the through holes of the honeycomb structure, and an assembly is obtained. The assembly is a "fiber membrane-green body-fiber membrane-green body-fiber membrane" structure, and then the assembly is UV-cured; wherein the average thickness of each film layer is 500μm; the power of the UV lamp during UV curing is 50mW / cm 2 , wavelength is 365nm, and curing time is 5min.

[0125] Step 3) placing the UV-cured assembly into a pyrolysis treatment furnace, heating it to 1000° C., and then keeping it at 1000° C. for 1 hour to obtain SiOC ceramics; wherein the heating rate is 1° C. / min.

[0126] The SiOC ceramics prepared in this embodiment are shown in FIG. Figure 5 The thermal conductivity of the SiOC ceramic prepared in this embodiment is 0.11 W / (m·K), and the surface temperature is 184°C after 800°C back temperature test for 20 minutes.

[0127] Example 4

[0128] This embodiment provides a method for preparing SiOC ceramics, comprising the following steps:

[0129] Step 1)

[0130] Preparation of ceramic precursor body:

[0131] Establishing the model: According to the optical photographs and SEM microscopic photographs of the honeycomb cross section of the honeycomb structure, the characteristic dimensions of the ceramic precursor body are obtained, and the model of the SiOC ceramic precursor body is established in the three-dimensional drawing software for subsequent additive manufacturing; wherein, the honeycomb structure is a single layer, so two ceramic precursor bodies are prepared;

[0132] Preparation of photosensitive ceramic precursor slurry: Weigh 0.4g of 819 free radical photoinitiator and dissolve it in 40g of methyl-terminated acrylate polysiloxane (same as Example 1), then place it on a magnetic stirrer and stir it at 500rpm for 30min to obtain a clear and transparent 1wt.% photosensitive polysiloxane solution (photosensitive ceramic precursor slurry); the viscosity of the obtained photosensitive ceramic precursor slurry is 181cps;

[0133] Additive manufacturing: The photosensitive ceramic precursor slurry is placed in a stereolithography 3D printing device for a first light curing process to obtain a ceramic precursor blank with a honeycomb structure; wherein the setting parameters of the stereolithography 3D printing device are: the layer thickness is set to 80μm, and the exposure intensity is set to 20mW / cm 2 , the exposure time was set to 3s, and the speed was set to 5mm / min.

[0134] Preparation of ceramic fiber membrane precursor:

[0135] Prepare a photosensitive mixed spinning solution: weigh 20g of methyl-terminated acrylate polysiloxane (polysiloxane solution) into a beaker, then add 0.2g of 819 (initiator) into the beaker, shake gently and disperse ultrasonically until the solution is clear to obtain a clear and transparent photosensitive polysiloxane solution; then dissolve 2g of PVP powder (spinning aid) in 10g of anhydrous ethanol (volatile solvent), stir for 4h, and prepare a PVP solution with a mass fraction of 20wt%; then, take 1wt.% of the photosensitive polysiloxane solution and an appropriate amount of PVP solution and place them on a magnetic stirrer for 5h to mix, and obtain a stable spinning solution. The mass ratio of PVP solution to photosensitive polysiloxane solution is 3:1. In terms of mass percentage, the spinning solution includes 25% of polysiloxane solution, 12.5% ​​of spinning aid, and 62.5% of volatile solvent;

[0136] Solidification spinning: The above-mentioned photosensitive mixed spinning solution was placed in a 5 ml disposable syringe, which was installed on the electrospinning machine platform at a pushing speed of 1 ml / h. During the process, a high voltage of 15 kV was applied, and a high-power ultraviolet lamp (80 mW / cm 2 ) is subjected to a second photocuring treatment, and a ceramic fiber membrane precursor is obtained by stretching and curing under a high-voltage electrostatic field, and cross-linking is induced under high-power ultraviolet irradiation, and the spinning time is 60 minutes.

[0137] Step 2) Cut the ceramic fiber membrane precursor into 30×30 mm 2The size of the two ceramic precursor green bodies is stacked. When stacking, there is a misalignment between the two green bodies, that is, the contact area between the upper layer and the lower layer accounts for 90% of the upper surface area of ​​the lower layer, and 5 layers of ceramic fiber membrane precursor are successively pasted between the two, and then 5 layers of ceramic fiber membrane precursor are respectively pasted on the upper and lower surfaces of the stacked green bodies, so that the ceramic fiber membrane precursor covers the through holes of the honeycomb structure, and an assembly is obtained. The assembly is a "fiber membrane-green body-fiber membrane-green body-fiber membrane" structure, and then the assembly is UV-cured; wherein the average thickness of each film layer is 500μm; the power of the UV lamp during UV curing is 50mW / cm 2 , wavelength is 365nm, and curing time is 10min.

[0138] Step 3) placing the UV-cured assembly into a pyrolysis treatment furnace, heating it to 1000° C., and then keeping it at 1000° C. for 1 hour to obtain SiOC ceramics; wherein the heating rate is 1° C. / min.

[0139] The thermal conductivity of the SiOC ceramic prepared in this embodiment is 0.11 W / (m·K), and the surface temperature is 168.6° C. after being tested at 800° C. for 20 minutes.

[0140] Example 5

[0141] This embodiment provides a method for preparing SiOC ceramics, comprising the following steps:

[0142] Step 1)

[0143] Preparation of ceramic precursor body:

[0144] Establishing the model: According to the optical photographs and SEM microscopic photographs of the honeycomb cross section of the honeycomb structure, the characteristic dimensions of the ceramic precursor body are obtained, and the model of the SiOC ceramic precursor body is established in the three-dimensional drawing software for subsequent additive manufacturing; wherein the honeycomb structure is double-layered; the contact area between the upper layer and the lower layer accounts for 100% of the upper surface area of ​​the lower layer; the wall thickness of the honeycomb structure is 0.5 mm;

[0145] Preparation of photosensitive ceramic precursor slurry: Weigh 0.4g of 819 free radical photoinitiator and dissolve it in 40g of methyl-terminated acrylate polysiloxane (same as Example 1), then place it on a magnetic stirrer and stir it at 500rpm for 30min to obtain a clear and transparent 1wt.% photosensitive polysiloxane solution (photosensitive ceramic precursor slurry); the viscosity of the obtained photosensitive ceramic precursor slurry is 181cps;

[0146] Additive manufacturing: The photosensitive ceramic precursor slurry is placed in a stereolithography 3D printing device for a first light curing process to obtain a ceramic precursor blank with a honeycomb structure; wherein the setting parameters of the stereolithography 3D printing device are: the layer thickness is set to 80μm, and the exposure intensity is set to 20mW / cm 2 , the exposure time was set to 3s, and the speed was set to 5mm / min.

[0147] Preparation of ceramic fiber membrane precursor:

[0148] Prepare a photosensitive mixed spinning solution: weigh 20g of methyl-terminated acrylate polysiloxane (polysiloxane solution) into a beaker, then add 0.2g of 819 (initiator) into the beaker, shake gently and disperse ultrasonically until the solution is clear to obtain a clear and transparent photosensitive polysiloxane solution; then dissolve 2g of PVP powder (spinning aid) in 10g of anhydrous ethanol (volatile solvent), stir for 4h, and prepare a PVP solution with a mass fraction of 20wt%; then, take 1wt.% of the photosensitive polysiloxane solution and an appropriate amount of PVP solution and place them on a magnetic stirrer for 5h to mix, and obtain a stable spinning solution. The mass ratio of PVP solution to photosensitive polysiloxane solution is 3:1. In terms of mass percentage, the spinning solution includes 25% of polysiloxane solution, 12.5% ​​of spinning aid, and 62.5% of volatile solvent;

[0149] Solidification spinning: The above-mentioned photosensitive mixed spinning solution was placed in a 5 ml disposable syringe, which was installed on the electrospinning machine platform at a pushing speed of 1 ml / h. During the process, a high voltage of 15 kV was applied, and a high-power ultraviolet lamp (80 mW / cm 2 ) is subjected to a second photocuring treatment, and a ceramic fiber membrane precursor is obtained by stretching and curing under a high-voltage electrostatic field, and cross-linking is induced under high-power ultraviolet irradiation, and the spinning time is 60 minutes.

[0150] Step 2) Cut the ceramic fiber membrane precursor into 30×30 mm 2 The size of the ceramic precursor body is applied layer by layer to the upper and lower surfaces of the ceramic precursor body through a polysiloxane solution, so that the ceramic fiber membrane precursor covers the through holes of the honeycomb structure to obtain an assembly, which is a "fiber membrane-body-fiber membrane" structure, and then the assembly is UV-cured; wherein, 10 layers of membrane are respectively applied to the upper and lower surfaces of the ceramic precursor body, and the average thickness of each layer of membrane is 500 μm; the power of the UV lamp during UV curing is 50 mW / cm 2 , wavelength is 365nm, and curing time is 5min.

[0151] Step 3) placing the UV-cured assembly into a pyrolysis treatment furnace, heating it to 1000° C., and then keeping it at 1000° C. for 1 hour to obtain SiOC ceramics; wherein the heating rate is 1° C. / min.

[0152] Example 6

[0153] This embodiment provides a method for preparing SiOC ceramics, comprising the following steps:

[0154] Step 1)

[0155] Preparation of ceramic precursor body:

[0156] Establishing the model: According to the optical photographs and SEM microscopic photographs of the honeycomb cross section of the honeycomb structure, the characteristic dimensions of the ceramic precursor body are obtained, and the model of the SiOC ceramic precursor body is established in the three-dimensional drawing software for subsequent additive manufacturing; wherein the honeycomb structure is double-layered; the contact area between the upper layer and the lower layer accounts for 100% of the upper surface area of ​​the lower layer; the wall thickness of the honeycomb structure is 0.5 mm;

[0157] Preparation of photosensitive ceramic precursor slurry: Weigh 0.4g of 819 free radical photoinitiator and dissolve it in 40g of methyl-terminated acrylate polysiloxane (same as Example 1), then place it on a magnetic stirrer and stir it at 500rpm for 30min to obtain a clear and transparent 1wt.% photosensitive polysiloxane solution (photosensitive ceramic precursor slurry); the viscosity of the obtained photosensitive ceramic precursor slurry is 181cps;

[0158] Additive manufacturing: The photosensitive ceramic precursor slurry is placed in a stereolithography 3D printing device for a first light curing process to obtain a ceramic precursor blank with a honeycomb structure; wherein the setting parameters of the stereolithography 3D printing device are: the layer thickness is set to 80μm, and the exposure intensity is set to 20mW / cm 2 , the exposure time was set to 3s, and the speed was set to 5mm / min.

[0159] Preparation of ceramic fiber membrane precursor:

[0160] Prepare a photosensitive mixed spinning solution: weigh 20g of methyl-terminated acrylate polysiloxane (polysiloxane solution) into a beaker, then add 0.2g of 819 (initiator) into the beaker, shake gently and disperse ultrasonically until the solution is clear to obtain a clear and transparent photosensitive polysiloxane solution; then dissolve 2g of PVP powder (spinning aid) in 10g of anhydrous ethanol (volatile solvent), stir for 4h, and prepare a PVP solution with a mass fraction of 20wt%; then, take 1wt.% of the photosensitive polysiloxane solution and an appropriate amount of PVP solution and place them on a magnetic stirrer for 5h to mix, and obtain a stable spinning solution. The mass ratio of PVP solution to photosensitive polysiloxane solution is 3:1. In terms of mass percentage, the spinning solution includes 25% of polysiloxane solution, 12.5% ​​of spinning aid, and 62.5% of volatile solvent;

[0161] Solidification spinning: The above-mentioned photosensitive mixed spinning solution was placed in a 5 ml disposable syringe, which was installed on the electrospinning machine platform at a pushing speed of 1 ml / h. During the process, a high voltage of 15 kV was applied, and a high-power ultraviolet lamp (80 mW / cm 2 ) is subjected to a second photocuring treatment, and a ceramic fiber membrane precursor is obtained by stretching and curing under a high-voltage electrostatic field, and cross-linking is induced under high-power ultraviolet irradiation, and the spinning time is 60 minutes.

[0162] Step 2) Cut the ceramic fiber membrane precursor into 30×30 mm 2 The size of the ceramic precursor body is applied layer by layer to the upper and lower surfaces of the ceramic precursor body through a polysiloxane solution, so that the ceramic fiber membrane precursor covers the through holes of the honeycomb structure to obtain an assembly, which is a "fiber membrane-body-fiber membrane" structure, and then the assembly is UV-cured; wherein, 10 layers of membrane are respectively applied to the upper and lower surfaces of the ceramic precursor body, and the average thickness of each layer of membrane is 100 μm; the power of the UV lamp during UV curing is 50 mW / cm 2 , wavelength is 365nm, and curing time is 5min.

[0163] Step 3) placing the UV-cured assembly into a pyrolysis treatment furnace, heating it to 1000° C., and then keeping it at 1000° C. for 1 hour to obtain SiOC ceramics; wherein the heating rate is 1° C. / min.

[0164] Comparative Example 1

[0165] This comparative example provides a method for preparing a SiOC porous thermal insulation material, comprising the following steps:

[0166] Step 1) preparing a ceramic precursor body:

[0167] Model building: Based on the optical photos of the honeycomb cross section and the SEM microscopic photos of the honeycomb structure, the characteristic dimensions of the ceramic precursor body are obtained, and a model of the SiOC ceramic precursor body is built in a three-dimensional drawing software for subsequent additive manufacturing;

[0168] Preparation of photosensitive ceramic precursor slurry: Weigh 0.4g of 819 free radical photoinitiator and dissolve it in 40g of methyl-terminated acrylate polysiloxane (same as Example 1), then place it on a magnetic stirrer and stir it at 500rpm for 30min to obtain a clear and transparent 1wt.% photosensitive polysiloxane solution (photosensitive ceramic precursor slurry); the viscosity of the obtained photosensitive ceramic precursor slurry is 181cps;

[0169] Additive manufacturing: The photosensitive ceramic precursor slurry was placed in a stereolithography 3D printing device for the first light curing treatment, and then the residual solution on the surface was blown dry with an air gun, and then ultrasonically cleaned in isopropanol for 5 minutes. After drying, a honeycomb structured ceramic precursor blank was obtained; wherein, the setting parameters of the stereolithography 3D printing device were: the layer thickness was set to 80μm, and the exposure intensity was set to 20mW / cm 2 , the exposure time was set to 3s, and the speed was set to 5mm / min.

[0170] Step 2) UV curing the prepared ceramic precursor body, the power of the UV lamp during UV curing is 50mW / cm 2 , wavelength is 365nm, and curing time is 5min.

[0171] Step 3) placing the UV-cured ceramic precursor body into a pyrolysis treatment furnace, heating it to 1000° C., and then keeping it at 1000° C. for 1 hour to obtain a SiOC porous thermal insulation material; wherein the heating rate is 1° C. / min.

[0172] The thermal insulation performance of the SiOC ceramics prepared in Examples 1, 2 and 3 of the present invention was tested respectively, and the corresponding thermal insulation performance curves are shown in FIG. Figure 6 and 7 shown. Figure 6 and Figure 7 The honeycomb porous thermal insulation structure is the SiOC porous thermal insulation material in the comparative example of the present invention; Figure 6 The sandwich assembly structure is a SiOC ceramic comprising two single-layer honeycomb structures; Figure 7The 10% misaligned honeycomb porous structure is a SiOC ceramic including a double-layer honeycomb structure, and in the double-layer honeycomb structure, the contact area between the upper layer and the lower layer accounts for 90% of the upper surface area of ​​the lower layer. The test steps of thermal insulation performance are as follows: the sample to be tested (SiOC ceramic) is placed in a refractory brick with a through hole, and the gap is strictly filled with thermal insulation cotton. Then the refractory brick is placed in a muffle furnace with a furnace temperature of 800°C, and one side of the sample to be tested faces the inside of the muffle furnace and the other side faces the outside of the muffle furnace. Then, an infrared temperature gun is used to measure the temperature of the outside of the sample, and a curve is drawn to calculate its thermal conductivity. There is no change in the surface morphology of the sample before and after the thermal insulation performance test.

[0173] from Figure 6 and Figure 7 It can be seen that the SiOC ceramics prepared by the present invention have excellent thermal insulation performance. Among them, the thermal conductivity of the SiOC ceramic is 0.11±0.009W / (m·K); at a preset temperature of 800℃, after 20 minutes, the back temperature of the SiOC ceramics of the honeycomb porous insulation structure, Example 1 and Example 3 are 480.8℃, 210.1℃ and 184℃ respectively (see Figure 6 As shown), the back temperature of the honeycomb porous structure with a displacement of 10% and Example 2 is 473.2°C and 199.7°C respectively (see Figure 7 As shown). According to the test, the thermal insulation efficiency of the honeycomb porous structure (ceramic precursor body) is 40.38%, the thermal insulation efficiency of the SiOC ceramic including two single-layer honeycomb structures is 74.38%, and the thermal insulation efficiency of the SiOC ceramic including a double-layer honeycomb structure (sandwich type) is further increased to 77.96%.

[0174] In Comparative Example 1, the absence of ceramic fiber membrane precursor will significantly reduce the thermal insulation performance. Although the honeycomb structure itself has certain thermal insulation performance, the pores of the honeycomb structure are arranged in one direction to form a continuous channel. The porosity is usually above 80%, allowing internal fluid transportation, which is conducive to active cooling and forced convection, so that its thermal insulation effect is not good. In the ceramic fiber membrane, its staggered fibers will hinder the flow of gas, reduce the probability of gas molecules colliding with each other inside the material, thereby reducing the efficiency of thermal convection, and when the heat flow reaches the inside of the material, the heat transfer efficiency is significantly reduced due to the complex heat transfer path at the overlap. Under high temperature conditions, the surface of the object becomes unstable, resulting in the inability to effectively transfer heat through the surface of the object, which also leads to a decrease in the efficiency of thermal conduction. Thermal radiation is the main way of heat transfer in a high temperature environment. The presence of fibers can absorb thermal radiation, convert it into heat energy and disperse it into the material, thereby further improving its thermal insulation performance.

[0175] The mechanical properties of the SiOC ceramics prepared in Examples 1 and 3 of the present invention and the SiOC porous material prepared in Comparative Example 1 were tested. The stress-strain curves are shown in FIG. Figure 8 shown. Figure 8 The porous honeycomb structure in is the SiOC porous material prepared in Comparative Example 1. The mechanical properties test data are as follows: the sample is placed in a universal testing machine, a displacement load is applied at a rate of 0.5 mm / min, and a stress-strain curve is obtained.

[0176] It is easy for those skilled in the art to understand that, without conflict, the advantageous technical features of the above-mentioned methods can be freely combined and superimposed.

[0177] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention shall be included in the protection scope of the present invention. The above description is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present invention. These improvements and variations should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing SiOC ceramics, characterized in that: The following steps are involved: Step 1) preparing a ceramic precursor body and a ceramic fiber membrane precursor respectively; wherein the ceramic precursor body is a honeycomb structure; Step 2) Assembling the ceramic fiber membrane precursor and the ceramic precursor green body so that the ceramic fiber membrane precursor covers the through holes of the honeycomb structure to obtain an assembly, and then UV curing the assembly; Step 3) The UV-cured assembly is subjected to pyrolysis treatment to obtain SiOC ceramics.

2. The method for preparing SiOC ceramics according to claim 1, wherein: In step 1), the step of preparing the ceramic precursor body comprises: Mixing a polysiloxane solution and a photoinitiator to obtain a photosensitive ceramic precursor slurry; then performing a first photocuring treatment on the photosensitive ceramic precursor slurry to obtain a ceramic precursor body; Wherein, the mass of the photoinitiator is 0.5% to 3% of the mass of the polysiloxane solution.

3. The method for preparing SiOC ceramics according to claim 2, wherein: The polysiloxane solution is an acrylate group siloxane solution; and / or, The photoinitiator is one or more of diphenyl-2,4,6-trimethylbenzoyl-phosphine oxide, phenyl bis-2,4,6-trimethylbenzoyl-phosphine oxide, and 2,4,6-trimethylbenzoyl ethyl phosphate; and / or, placing the photosensitive ceramic precursor slurry in a light-curing device to perform a first light-curing treatment; Preferably, the parameters of the light curing device are set as follows: layer thickness is 1-300 μm, exposure intensity is 1-100 mW / cm 2 , exposure time is 0.5-30s, speed is 0.1-300mm / min.

4. The method for preparing SiOC ceramics according to claim 1, wherein: In the step 1), the thickness of the ceramic fiber membrane precursor is 100-500 μm; and / or The steps of preparing the ceramic fiber membrane precursor include: dissolving a polysiloxane solution, a spinning aid, and a photoinitiator in a volatile solvent to obtain a spinning solution; Then, the spinning solution is subjected to electrospinning and a second light curing treatment to obtain a ceramic fiber membrane precursor; Preferably, the photoinitiator is one or more of TPO free radical initiator, 819 free radical initiator, and TPO-L free radical initiator; Preferably, the exposure intensity of the second light curing process is 40-100 mW / cm 2 .

5. The method for preparing SiOC ceramics according to claim 4, characterized in that: The spinning solution comprises the following components by mass percentage: polysiloxane solution: 15-40%, spinning aid: 5-15%, initiator: 0.1-5%, volatile solvent: 40-70%; Preferably, the spinning aid is one of polyvinyl pyrrolidone and polyethylene oxide; Preferably, the volatile solvent is one of ethanol and isopropanol.

6. The method for preparing SiOC ceramics according to any one of claims 1 to 5, characterized in that: The wall thickness of the honeycomb structure is 0.5-10 mm.

7. The method for preparing SiOC ceramics according to claim 6, characterized in that: The ceramic precursor body is a single-layer honeycomb structure or a double-layer honeycomb structure; When the ceramic precursor green body is a single-layer honeycomb structure, the assembly process includes: stacking two ceramic precursor green bodies to obtain a stacked green body, and then applying a ceramic fiber membrane precursor between the two single-layer honeycomb structures of the stacked green body and on the surface where the through holes of the stacked green body are located; When the ceramic precursor body is a double-layer honeycomb structure, the assembly process includes: laminating a ceramic fiber membrane precursor on the surface where the through holes of the ceramic precursor body are located; Preferably, in the double-layer honeycomb structure, the contact area between the upper layer and the lower layer accounts for 50%-100% of the upper surface area of ​​the lower layer; Preferably, the number of coating layers of the ceramic fiber membrane precursor is 1-10 layers.

8. The method for preparing SiOC ceramics according to claim 1 or 7, characterized in that: In step 2), the UV curing parameters are: the irradiation intensity of the UV lamp is 40-100 mW / cm 2 ; The wavelength of the UV lamp is 365-405nm; the curing time is 5-20min.

9. The method for preparing SiOC ceramics according to claim 1, wherein: In the step 3), the pyrolysis treatment includes: Under an inert atmosphere, heating the UV-cured assembly to 800-1200° C., maintaining the temperature for 0.5-10 hours, and then cooling to room temperature to obtain the SiOC ceramic; Preferably, the inert atmosphere is argon; Preferably, the UV-cured assembly is heated to 800-1200° C. at a heating rate of 1-10° C. / min.

10. A SiOC ceramic, characterized in that: The SiOC ceramic comprises a ceramic fiber membrane structure and a SiOC ceramic honeycomb structure arranged opposite to each other; the ceramic fiber membrane structure covers the through holes of the SiOC ceramic honeycomb structure; The thermal conductivity of the SiOC ceramic is 0.04-0.15 W / (m·K); the back temperature of the SiOC ceramic is 500° C.-1000° C.; and the compressive strength of the SiOC ceramic is 5-15 MPa. Preferably, the SiOC ceramic is obtained by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Flexible polysiloxane fiber membrane and their preparation method and application thereof

    CN109868559A

  • Composite ceramic with honeycomb fiber structure and preparation method of composite ceramic

    CN113149688A

  • Non-ablative heat protection / heat insulation / bearing integrated material and preparation method thereof

    CN113246563A

  • Bionic light heat insulation sandwich structure and preparation method thereof

    CN113800940A

  • Manufacturing method of lithium metal battery and lithium metal battery manufactured using the same

    KR1020250171042A