Modified graphene / polymer compound as well as preparation method and application thereof

Through polypropylene compatibilizer emulsion-assisted exfoliation and melt blending technology, the dispersion and interfacial interaction problems of graphene/polypropylene composite materials are solved, and high-performance, low-cost graphene/polypropylene composite material preparation is achieved, improving The comprehensive performance and industrial application potential of the material are demonstrated.

CN118725448AActive Publication Date: 2024-10-01FUDAN UNIVERSITY +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310316763.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-01
Estimated Expiration
2043-03-28

AI Technical Summary

Technical Problem

It is difficult to achieve low-cost, large-scale preparation of graphene/polypropylene composite materials with existing technology. Graphene is unevenly dispersed in the polypropylene matrix and easily agglomerates, resulting in poor interface interaction and inability to effectively improve the overall performance of the composite material.

Method used

By using polypropylene compatibilizer emulsion to assist in the exfoliation of low-oxidation expanded graphite, efficient exfoliation and uniform dispersion of graphene are achieved, and melt blending with polypropylene, combined with interface modification, simplifies the process and reduces production costs.

Benefits of technology

It achieves high-performance preparation of graphene/polypropylene composite materials, improves the material's mechanical strength, toughness, conductivity and other properties, simplifies the production process, reduces costs, and has important industrial application value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725448A_ABST
    Figure CN118725448A_ABST
Patent Text Reader

Abstract

The invention provides a modified graphene / polymer compound and a preparation method and application thereof.The preparation method comprises the steps that expanded graphite is subjected to intercalation oxidation in a mixed solution of strong acid and a strong oxidant, and low-oxidation expanded graphite is obtained; the preparation method comprises the following steps: mixing expanded graphite with low oxidation degree and a polymer compatilizer emulsion, and mechanically stripping to obtain a compatilizer modified graphene suspension (A); and drying the suspension (A) to obtain compatibilizer-modified graphene particles (B), and carrying out melt blending on the compatibilizer-modified graphene particles (B) and polyolefin to obtain the modified graphene / polyolefin compound (C). According to the method, expensive graphene or graphene derivatives are not needed as raw materials, and expanded graphite can be stripped into high-quality graphene in the liquid-phase processing process. According to the graphene / polypropylene composite material disclosed by the invention, the complex modification process of graphene is avoided, stripping and modification of graphene are organically combined together, production and application of the material are combined, and integrated preparation of the graphene / polypropylene composite material is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for preparing a modified graphene / polymer composite and the prepared modified graphene / polymer composite, in particular to a method for preparing a modified graphene / polyolefin (such as polypropylene) composite and the obtained modified graphene / polyolefin (such as polypropylene) composite, belonging to the field of polyolefin compositions. Background Art

[0002] As a thermoplastic bulk general-purpose plastic, polypropylene has the advantages of high strength, high wear resistance, chemical resistance, good processing performance, light weight, and high cost performance. It has been widely developed and used in many industries such as machinery, automobiles, rail transportation, construction, electronics and electrical, and packaging. However, polypropylene has a low melting point, poor light and thermal stability, high low-temperature brittleness, and poor antistatic properties. Its rigidity and strength are still far from people's needs, which limits its application in some complex environments and high-end fields. Therefore, achieving high performance and functionalization of polypropylene has very important industrial value. Graphene is a two-dimensional nanomaterial formed by the close stacking of carbon atoms. It has many excellent properties, such as an extremely large specific surface area (2630m 2 / g), ultra-high Young's modulus (1TPa) and fracture strength (130GPa), ultra-large carrier mobility (200,000cm 2 / (V·s)) and ultra-high thermal conductivity (5300W / (m·K)). Therefore, adding graphene as a functional filler to polypropylene can greatly improve its strength, toughness, thermal conductivity, electrical conductivity, gas barrier, flame retardancy, electromagnetic shielding, anti-ultraviolet aging and other properties, providing an ideal solution for achieving the functionalization and high performance of polypropylene.

[0003] When preparing polymer nanocomposites, the thorough exfoliation and good dispersion of graphene are two key factors for polymer enhancement and functionalization, which requires the need to solve the difficulties faced by the large-scale preparation of high-quality graphene and the preparation of high-performance graphene-enhanced polymer nanocomposites respectively. In existing technical means, these two preparation processes are usually completed independently of each other. For graphene preparation, it can be achieved by methods such as micromechanical exfoliation, liquid phase exfoliation, chemical vapor deposition and epitaxial growth. However, the high production cost, low yield, complex production process, serious pollution, serious in-plane defects, and small lateral dimensions of the product of graphene greatly limit the industrial production and application of graphene. On the other hand, in the process of graphene and polymer composite, due to the strong conjugated interaction between sheets, graphene is easy to agglomerate in the polymer matrix. In order to solve the dispersion problem of graphene and obtain high-performance polymer nanocomposites, most technical solutions tend to adopt in-situ polymerization, solution mixing and melt mixing methods. However, the former method has a complex process, a long preparation time, and a large amount of toxic chemical reagents, which is not suitable for industrial and low-cost production. Although the dispersion degree of graphene can be improved to a certain extent by multi-step and long-time melt mixing technology, the improvement effect of this method is limited, and long-time melt shearing may cause the size cutting of graphene, greatly reduce its intrinsic excellent performance, bring adverse effect. In addition, the surface chemical inertness of graphene makes it very weak to interact with the interface between polymer matrix, which can cause the performance of the composite material prepared to be undesirable, and even some performance indicators are seriously deteriorated, greatly reducing its use value. Therefore, it is also necessary to carry out surface modification (CN112064338A and CN112174286A) to promote the dispersion of graphene, strengthen the interfacial force of graphene and polymer matrix to the graphene peeling. But the graphene surface modification process is long, energy consumption is high, and operation is complicated, and extra cost is increased.

[0004] The problems existing in the prior art are:

[0005] 1. Low-cost, large-scale preparation of graphene / polypropylene composites has always been difficult to achieve. In the existing technical solutions, the preparation of high-quality graphene and the production of high-performance polypropylene nanocomposites are independent and separated from each other. The graphene production process is complicated and costly, which seriously restricts the large-scale production and practical application of polypropylene composites.

[0006] 2. The problem of uneven dispersion and easy agglomeration of graphene in the polypropylene matrix has not been solved. Since the production and application of graphene are separated, in order to promote the good dispersion of graphene in the polypropylene matrix and enhance the interfacial interaction between graphene and polypropylene, the existing technical methods generally use chemical modification methods to modify the graphene surface and then compound it with polypropylene, but such surface modification will significantly reduce the functionality of graphene and affect the effect of graphite-modified polypropylene. More importantly, the existing surface chemical modification methods generally have cumbersome processes, poor operability, high costs, and are not environmentally friendly. They are incompatible with existing polypropylene production and processing technologies and cannot meet the needs of large-scale production of polypropylene nanocomposites.

[0007] 3. The compatibility between graphene and polypropylene matrix is ​​poor, the interface interaction is poor, the functionality of graphene cannot be effectively combined with the matrix, and the comprehensive performance of the composite material cannot be significantly improved. Since the quality of the peeled graphene is not high and the dispersion is poor, in order to obtain the expected performance of the polypropylene / graphene composite material, a higher mass fraction of graphene is usually used, which not only greatly increases the cost, but also seriously deteriorates the inherent properties of polypropylene itself, such as fracture toughness, processing performance, light weight, etc., and reduces the comprehensive performance of the polypropylene composite material.

[0008] In view of the above problems, CN113276376A proposes to realize the exfoliation and uniform dispersion of expanded graphite in situ during the polymer melt processing. However, this method is superior to the graphene sheets in the expanded graphite, which are still highly stacked (often dozens of graphene sheets are stacked on each other due to the conjugate attraction between the layers). The moisture contained between the thick layers cannot exfoliate the stacked graphene into a single layer or a few layers of graphene sheets under the action of high temperature. Moreover, the interaction between graphene and polypropylene is weak and they are incompatible with each other. Therefore, it is difficult for the composite material to realize the exfoliation, dispersion, interface load transfer of the graphene sheets and the final effective improvement of the macroscopic performance.

[0009] Currently, there is a lack of a simpler and more efficient method to prepare highly exfoliated and well-dispersed graphene-polypropylene nanocomposites, especially a lack of a green and economically feasible production method that combines graphene exfoliation, interface modification, and compounding to achieve high-performance graphene polypropylene composites. Summary of the invention

[0010] In view of the above problems, the present invention provides a simple method for preparing modified graphene / polymer composites, specifically, using polypropylene compatibilizer emulsion to assist in exfoliation of low-oxidation expanded graphite to obtain compatibilizer-modified graphene, and then blending with polypropylene to obtain modified graphene / polypropylene composites.

[0011] The present invention effectively combines the high-quality exfoliation of expanded graphite, interface modification and preparation of high-performance graphene composite materials, and proposes a simple, low-cost, high-throughput preparation method of modified graphene / polypropylene composites. Low-oxidation expanded graphite (LOEG) is used as a precursor, and the enlarged interlayer spacing (greatly weakening the interlayer force) and the hydrogen bond interaction between compatibilizers such as maleic anhydride grafted polypropylene and oxygen-containing functional groups on the surface of LOEG are utilized. Through simple mechanical mixing, efficient exfoliation, uniform dispersion and interface enhancement of graphene are achieved in one step, and high-performance graphene modified polypropylene masterbatch is obtained. Then, the modified graphene / polypropylene composite material is efficiently prepared by melt blending with a polypropylene matrix. The present invention has a short process flow, simple operation, green economy, and effectively solves the problem of low-cost large-scale preparation of high-quality graphene / polymer nanocomposites.

[0012] The present invention aims to solve the problems existing in the preparation process of existing graphene / polypropylene composites, such as the difficulty in dispersing graphene, the complicated graphene surface modification process, the high cost, and the difficulty in industrial application. The present invention combines the efficient exfoliation of high-quality graphene with the preparation process of high-performance polypropylene nanocomposites to obtain a functionalized modified graphene / polyolefin (e.g., polypropylene) composite.

[0013] To achieve the above object, the present invention modifies a small amount of oxygen-containing functional groups on the surface of expanded graphite by controlling the oxidation process. On the one hand, the process weakens the interaction force between graphite layers, effectively reducing the mechanical treatment time and output energy required for chemical expanded graphite exfoliation. On the other hand, a small amount of oxygen-containing functional groups, under the premise of ensuring that the graphene structure and performance are complete, simultaneously achieve high-quality exfoliation, stable dispersion and surface modification of graphene through interactions such as hydrogen bonds with compatibilizers. This compatibilizer-modified graphene masterbatch can effectively improve the mechanical strength, toughness, electrical conductivity, thermal conductivity and other properties of the polypropylene matrix. The present invention greatly shortens the production process of graphene / polypropylene composite materials, reduces production costs, and has important industrial application value.

[0014] According to a first embodiment of the present invention, there is provided a method for preparing a modified graphene / polyolefin composite, the method comprising the following steps:

[0015] (1) subjecting expanded graphite to intercalation oxidation in a mixed solution of a strong acid and a strong oxidant to obtain expanded graphite with a low degree of oxidation;

[0016] (2) uniformly mixing the low-oxidation expanded graphite obtained in step (1) and the compatibilizer emulsion, and performing mechanical exfoliation to obtain a compatibilizer-modified graphene suspension (A); preferably, the concentration of graphene in the graphene suspension (A) is 0.01-200 mg / ml (preferably 0.1-150 mg / ml, more preferably 1-120 mg / ml, more preferably 5-100 mg / ml, more preferably 10-80 mg / ml, more preferably 15-60 mg / ml, more preferably 10-50 mg / ml, for example 20, 30, 40 mg / ml);

[0017] (3) drying the compatibilizer-modified graphene suspension (A) obtained in step (2) to obtain (dried) compatibilizer-modified graphene particles (B), and

[0018] (4) melt-blending the graphene particles (B) modified by the compatibilizer obtained in step (3) with a polyolefin (e.g., polypropylene, propylene copolymer, polyethylene, ethylene copolymer, etc., as a matrix) to obtain a modified graphene / polyolefin composite (C).

[0019] The above preparation method of the present invention is particularly suitable for preparing modified graphene / polypropylene composites. Therefore, the present invention provides a preparation method of modified graphene / polypropylene composites, which comprises the following steps:

[0020] (1) subjecting expanded graphite to intercalation oxidation in a mixed solution of a strong acid and a strong oxidant to obtain expanded graphite with a low degree of oxidation;

[0021] (2) uniformly mixing the low-oxidation expanded graphite obtained in step (1) and the compatibilizer emulsion, and performing mechanical exfoliation to obtain a compatibilizer-modified graphene suspension (A); preferably, the concentration of graphene in the graphene suspension (A) is 0.01-200 mg / ml (preferably 0.1-150 mg / ml, more preferably 1-120 mg / ml, more preferably 5-100 mg / ml, more preferably 10-80 mg / ml, more preferably 15-60 mg / ml, more preferably 10-50 mg / ml, for example 20, 30, 40 mg / ml);

[0022] (3) drying the compatibilizer-modified graphene suspension (A) obtained in step (2) to obtain (dried) compatibilizer-modified graphene particles (B);

[0023] (4) melt-blending the graphene particles (B) modified by the compatibilizer obtained in step (3) with polypropylene (as a matrix) to obtain a modified graphene / polypropylene composite (C).

[0024] More specifically, the present invention provides a method for preparing a modified graphene / polypropylene composite, the method comprising the following steps:

[0025] (1) subjecting expanded graphite to intercalation oxidation in a mixed solution of a strong acid and a strong oxidant to obtain expanded graphite with a low degree of oxidation;

[0026] (2) mixing the low-oxidation expanded graphite obtained in step (1) and the compatibilizer emulsion at room temperature, and performing mechanical exfoliation to obtain a compatibilizer-modified graphene suspension (A); preferably, the concentration of graphene in the graphene suspension (A) is 0.01-200 mg / ml (preferably 0.1-150 mg / ml, more preferably 1-120 mg / ml, more preferably 5-100 mg / ml, more preferably 10-80 mg / ml, more preferably 15-60 mg / ml, more preferably 10-50 mg / ml, for example 20, 30, 40 mg / ml);

[0027] (3) drying the compatibilizer-modified graphene suspension obtained in step (2) to obtain compatibilizer-modified graphene particles (B);

[0028] (4) melt-blending the graphene particles modified by the compatibilizer with polypropylene (as a matrix) to obtain a modified graphene / polypropylene composite (C).

[0029] In the above methods, the compatibilizer emulsion used is a polymer compatibilizer emulsion.

[0030] In the present application, the expanded graphite used in step (1) is one or more (eg, a combination of two or three) of chemically expanded graphene, thermally expanded graphite, and microwave expanded graphite.

[0031] In the present application, the strong acid used in step (1) is one or a combination of concentrated sulfuric acid, concentrated hydrochloric acid, concentrated nitric acid, and concentrated phosphoric acid. Preferably, the volume of the strong acid required per gram of expanded graphite is 80-350 ml, preferably 100-320 ml, preferably 120-300 ml, preferably 150-280 ml.

[0032] In the present application, the strong oxidant described in step (1) is one or more (e.g., a combination of two, three, or four) of potassium permanganate, potassium perchlorate, potassium ferrate, potassium dichromate, potassium nitrate, sodium nitrate, potassium persulfate, sodium persulfate, and ammonium persulfate. The mass ratio (wt) of the strong oxidant to the expanded graphite is (0.1-5):1, preferably (0.2-4.7):1, preferably (0.3-4.5):1, preferably (0.4-4.2):1, preferably (0.5-4.0):1, preferably (0.6-3.7):1, preferably (0.7-3.5):1, preferably (0.8-3.2):1, preferably (1-3):1. Preferably, the oxidation time is 20 minutes to 5 hours, more preferably 30 minutes to 4.5 hours, more preferably 1 hour to 4 hours, for example 2 or 3 hours.

[0033] The "oxidation degree" of expanded graphite is determined by the amount of the strong oxidant and the oxidation time mentioned above. The less the amount of strong oxidant, the shorter the oxidation time and the lower the oxidation degree. The oxidation degree can also be determined by the carbon-oxygen ratio in the material.

[0034] Preferably, in step (1), the "low oxidation" degree in the low-oxidation expanded graphite means that the carbon-oxygen atomic ratio in the oxidized expanded graphite is between 1.5-8: 1, preferably between 2.5-6: 1, preferably between 3-5.5: 1, preferably between 3.2-5: 1, and more preferably between 3.5-4.5: 1. If the oxidation degree is too high, the lattice integrity and conductivity of the exfoliated graphene will be destroyed.

[0035] In the present invention, the carbon-oxygen atomic ratio in the oxidized expanded graphite after oxidation can be obtained by detecting by an X-ray photoelectron spectrometer or elemental analysis (atomic emission spectrometry). The X-ray photoelectron spectrometer can be obtained by using equipment such as the German SPECTRO XRF-x-ray spectrometer, Thermo Scientific ESCALAB Xi+, etc. The elemental analysis can be obtained by detecting by using instruments such as the German SPECTRO emission spectrometer, Agilent 5800ICP-OES, etc.

[0036] Preferably, the compatibilizer emulsion is a (low molecular weight) polyolefin type compatibilizer emulsion (i.e., a polyolefin type compatibilizer emulsion that is not grafted or grafted), or a polyether type compatibilizer emulsion. More preferably, the compatibilizer emulsion is selected from one or more of the following polymer compatibilizer emulsions: polyethylene wax emulsion, polypropylene wax emulsion, ethylene-vinyl acetate copolymer emulsion, isooctylphenyl polyoxyethylene ether (e.g., Triton), polyoxyethylene polyether, polyoxypropylene polyether or polyoxyethylene polyoxypropylene (e.g., poloxamer), maleic anhydride grafted polyethylene emulsion, maleic anhydride grafted polypropylene emulsion, maleic anhydride grafted ethylene-vinyl acetate copolymer emulsion, maleic anhydride grafted ethylene-butylene copolymer emulsion and maleic anhydride grafted ethylene-octene copolymer emulsion.

[0037] Accordingly, the compatibilizer is a (low molecular weight) polyolefin type compatibilizer (ie, a non-graft modified or graft modified polyolefin type compatibilizer), or a polyether type compatibilizer.

[0038] The solid content of the emulsion is 1-50wt%, preferably 3-48wt%, preferably 5-46wt%, preferably 7-45wt%, preferably 9-43wt%, preferably 10-40wt%, preferably 15-37wt%, preferably 18-35wt%, preferably 20-30wt%.

[0039] The mass ratio of the solid component in the compatibilizer emulsion to the low-oxidation expanded graphite is (0.4-9):1, preferably (0.8-8.5):1, preferably (1.2-8):1, preferably (1.5-7):1, preferably (1.7-6):1, preferably (1.8-5):1, preferably (2.0-4.0):1.

[0040] Preferably, in step (2), the low-oxidation expanded graphite obtained in step (1) and the compatibilizer emulsion are uniformly mixed at 5-100°C, more preferably 6-80°C, preferably 7-60°C, preferably 10-50°C, more preferably 15-40°C, more preferably at room temperature (20-30°C).

[0041] Preferably, in step (2), the amount of low-oxidation expanded graphite relative to the compatibilizer emulsion should be such that the concentration of graphene in the resulting compatibilizer-modified graphene suspension (A) (i.e., the concentration of graphene in the graphene suspension (A)) is 0.01-250 mg / ml, preferably 0.05-230 mg / ml, preferably 0.1-200 mg / ml, preferably 0.5-190 mg / ml, preferably 0.8-180 mg / ml. g / ml, preferably 1-170 mg / ml, preferably 1.5-165 mg / ml, preferably 2.0-160 mg / ml, for example 3, 4, 5, 6, 7, 8, 9, 10, 12, 15, 18, 20, 22, 25, 27, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 90, 100, 110, 120, 130, 140, 150 mg / ml.

[0042] The mechanical exfoliation in step (2) includes one or a combination of ball milling, sand milling, water bath ultrasound, probe ultrasound, high-speed shearing, high-pressure homogenization, and Taylor-Couette fluid exfoliation.

[0043] The drying described in step (3) includes one or a combination of vacuum drying, freeze drying, forced air drying, fluidized bed drying, spray drying, infrared drying, and microwave drying.

[0044] In the present invention, the melt blending in step (3) includes one or more of internal mixing, single screw extrusion, and twin screw extrusion. The processing temperature is 180-220° C. and the processing time is 3-20 minutes.

[0045] Preferably, the polyolefin (as a matrix) used in step (4) is: polyolefin plastic and / or polyolefin elastomer. Polyolefin elastomer refers to a thermoplastic elastomer that is polymerized in situ by ethylene and α-olefin using a metallocene catalyst, and exhibits thermoplastic elastomer behavior through physical crosslinking, and has the properties of both plastic and rubber.

[0046] EPDM rubber is formed by chemical cross-linking and is a type of rubber. It can be divided into EPDM rubber and EPDM rubber.

[0047] Preferably, the polyolefin plastic (as the matrix) is selected from one or more of polypropylene, propylene copolymer, polyethylene, ethylene copolymer, ethylene-vinyl acetate copolymer, poly-1-butene, 1-butene copolymer. The polyolefin elastomer (as the matrix) is selected from one or more of ethylene-1-butene elastomer, ethylene-1-octene elastomer, ethylene / propylene elastomer.

[0048] Preferably, in the compatibilizer-modified graphene particles (B), the mass percentage of graphene is in the range of 5-70wt%, preferably 7-65wt%, preferably 8-60wt%, preferably 9-55wt%, preferably 10-50wt%, preferably 15-45wt%, preferably 20-40wt%, preferably 25-35wt%, for example 13, 17, 22, 27, 30, 32wt%, based on the total weight of the compatibilizer-modified graphene particles (B).

[0049] In step (4), the amount of the compatibilizer-modified graphene particles (B) relative to the polyolefin (e.g., polypropylene) should be such that in the resulting modified graphene / polyolefin (e.g., polypropylene) composite (C), the mass percentage or weight percentage of graphene (i.e., the mass fraction or content of graphene in the composite C) is 0.05-25wt%, preferably 0.1-20wt%, preferably 0.15-15wt%, preferably 0.20-13wt%, Preferably 0.25-12wt%, preferably 0.30-10wt%, preferably 0.35-9wt%, preferably 0.40-8wt%, for example 0.50, 0.60, 0.70, 0.80, 0.90, 1.0, 1.2, 1.5, 1.8, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5wt%, based on the total weight of composite (C).

[0050] More specifically, the present invention provides a method for preparing a modified graphene / polyolefin (e.g., polypropylene) composite, characterized in that the specific steps are as follows:

[0051] (1) subjecting expanded graphite to intercalation oxidation in a mixed solution of a strong acid and a strong oxidant to obtain expanded graphite with a low degree of oxidation;

[0052] (2) mixing the low-oxidation expanded graphite obtained in step (1) and the compatibilizer emulsion uniformly at room temperature, and performing mechanical exfoliation to obtain a compatibilizer-modified graphene suspension, wherein the concentration of the graphene is controlled to be 0.01-200 mg / ml;

[0053] (3) drying the compatibilizer-modified graphene suspension obtained in step (2) to obtain compatibilizer-modified graphene particles, and then melt-blending the graphene particles with a polyolefin (such as polypropylene) (as a matrix) to obtain a modified graphene / polyolefin (such as polypropylene) composite.

[0054] Preferably, the expanded graphite in step (1) is one or a combination of chemically expanded graphene, thermally expanded graphite, and microwave expanded graphite.

[0055] Preferably, the strong acid in step (1) is one or a combination of concentrated sulfuric acid, concentrated hydrochloric acid, concentrated nitric acid, and concentrated phosphoric acid, and the volume of the strong acid required per gram of expanded graphite is 100-300 ml.

[0056] Preferably, the strong oxidant in step (1) is one or a combination of potassium permanganate, potassium perchlorate, potassium ferrate, potassium dichromate, potassium nitrate, sodium nitrate, potassium persulfate, sodium persulfate, and ammonium persulfate, the mass ratio of the strong oxidant to the expanded graphite is (0.1-5):1, and the oxidation time is 20 minutes to 5 hours.

[0057] Preferably, the compatibilizer described in step (2) is one or more combinations of polyethylene wax emulsion, polypropylene wax emulsion, ethylene-vinyl acetate copolymer emulsion, isooctylphenyl polyoxyethylene ether (e.g., Triton), various polyethers (e.g., polyethylene oxide or polypropylene oxide) or polyoxyethylene polyoxypropylene (e.g., poloxamer), maleic anhydride grafted polyethylene emulsion, maleic anhydride grafted polypropylene emulsion, maleic anhydride grafted ethylene-vinyl acetate copolymer emulsion, maleic anhydride grafted ethylene-butene copolymer emulsion, and maleic anhydride grafted ethylene-octene copolymer emulsion, the solid content of the emulsion is 1-50%, and the mass ratio of the compatibilizer used to the low-grade graphene oxide is (1-9):1.

[0058] Preferably, the mechanical exfoliation in step (2) comprises one or a combination of ball milling, sand milling, water bath ultrasound, probe ultrasound, high-speed shearing, high-pressure homogenization, and Taylor-Couette fluid exfoliation.

[0059] Preferably, the drying in step (3) comprises one or a combination of vacuum drying, freeze drying, forced air drying, fluidized bed drying, spray drying, infrared drying, and microwave drying.

[0060] Preferably, the melt blending in step (3) includes one or more of internal mixing, single-screw extrusion, and twin-screw extrusion, and the processing temperature is 180-220° C. and the processing time is 3-20 minutes.

[0061] Preferably, the content of graphene in the modified graphene / polyolefin (eg, polypropylene) composite obtained in step (3) is 0.01-20%.

[0062] According to a second embodiment of the present invention, the present invention also provides a (compatibilizer) modified graphene / polyolefin composite obtained by the above method. The mass percentage or weight percentage of graphene (i.e., the mass fraction or content of graphene in composite C) is 0.05-25wt%, preferably 0.1-20wt%, preferably 0.15-15wt%, preferably 0.20-13wt%, preferably 0.25-12wt%, preferably 0.30-10wt%, preferably 0.35-9wt%, preferably 0.40-8wt%, such as 0.50, 0.60, 0.70, 0.80, 0.90, 1.0, 1.2, 1.5, 1.8, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5wt%, based on the total weight of composite (C).

[0063] According to a third embodiment of the present invention, the present invention also provides compatibilizer-modified graphene particles (B). It is prepared by a preparation method comprising the following steps:

[0064] (1) subjecting expanded graphite to intercalation oxidation in a mixed solution of a strong acid and a strong oxidant to obtain expanded graphite with a low degree of oxidation;

[0065] (2) uniformly mixing the low-oxidation expanded graphite obtained in step (1) and the compatibilizer emulsion, and performing mechanical exfoliation to obtain a compatibilizer-modified graphene suspension (A);

[0066] (3) Drying the compatibilizer-modified graphene suspension (A) obtained in step (2) to obtain (dried) compatibilizer-modified graphene particles (B).

[0067] That is, the compatibilizer-modified graphene particles (B) are prepared by steps (1) to (3) of the above method according to the first embodiment.

[0068] The compatibilizer used in the present application is a (low molecular weight) polyolefin type compatibilizer (i.e., a polyolefin type compatibilizer that is not grafted or grafted), or a polyether type compatibilizer. The compatibilizer emulsion is formed by emulsifying the polyolefin type compatibilizer (i.e., a polyolefin type compatibilizer that is not grafted or grafted), or a polyether type compatibilizer in water with an emulsifier or a surfactant. The solid content of the emulsion is as described above, for example, 1-50wt%.

[0069] Preferably, the number average molecular weight of the compatibilizer, that is, the number average molecular weight of the polyolefin type compatibilizer or the polyether type compatibilizer is generally between 1000 and 70000, preferably between 1200-60000, more preferably between 1500-50000, for example, 2000, 3000, 4000, 5000, 6000, 7000, 8000, 9000, 10000, 15000, 20000, 25000, 30000, 35000, 40000. The polyolefin type compatibilizer is, for example, polypropylene wax and / or polyethylene wax (polypropylene wax, polyethylene wax, ethylene propylene copolymer wax, polyethylene copolymer wax, etc.).

[0070] The emulsifier or surfactant used to prepare the above-mentioned compatibilizer emulsion is one or a combination of ionic surfactants (including sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, sodium cholate, hexadecyltrimethylammonium bromide, etc.) and non-ionic surfactants (isomeric decanol polyoxyethylene ether, octadecyl alcohol polyoxyethylene ether, isooctylphenyl polyoxyethylene ether, isooctylphenyl polyoxyethylene ether, etc.).

[0071] The technical solution of the present invention can be directly used to enhance polyolefins (such as polymer matrices or substrates such as polypropylene or polyethylene), for the preparation of polymer nanocomposites, and can also be directly used in the field of functional inks and coatings, or the products of this solution can be used as raw materials to produce high-performance modified polyolefin fibers (such as polypropylene fibers) through spinning technology, or to produce anti-pathogen (bacterial, antiviral) non-woven fabrics through melt-blowing technology, or can be used in other related fields through other technical means.

[0072] The preparation method of the present invention has the following advantages compared with the prior art:

[0073] By combining the exfoliation of graphene with the preparation of graphene-modified polyolefin (such as polypropylene) masterbatch, the use of expensive graphene or graphene derivatives is avoided, the process flow is greatly simplified, and the production cost of polymer nanocomposites is reduced.

[0074] Different from the cumbersome modification process of traditional graphene surface, this scheme realizes the efficient exfoliation and dispersion of expanded graphite through simple structural design of the precursor expanded graphite, enhances the interaction between graphene and polyolefin (such as polypropylene) matrix, and effectively solves the difficulty of preparing polymer nanocomposites.

[0075] The preparation method proposed in this scheme is simple, efficient, green, environmentally friendly, low-cost, and has strong industrial application potential. The polymer nanocomposite material obtained by this scheme has excellent comprehensive performance and a wide range of applications.

[0076] For the exfoliation and dispersion of expanded graphite by mechanical exfoliation using polypropylene compatibilizer emulsion mentioned in the embodiments of the present invention, in addition, direct mechanical treatment using polypropylene solution (or suspension) can achieve a similar effect, but it is not preferred. In addition, for the method of exfoliation by liquid phase mechanical processing mentioned in the embodiments of the present invention, it can also be achieved by polymer melt processing.

[0077] Here, the "polypropylene solution" (or suspension) refers to a solution formed by dissolving polypropylene in toluene and / or xylene under heating conditions. The "polypropylene suspension" refers to a suspension formed by adding polypropylene to toluene or xylene.

[0078] Advantages of the present invention

[0079] 1. The present invention does not require expensive graphene or graphene derivatives as raw materials, and can peel expanded graphite into high-quality graphene during liquid phase processing;

[0080] 2. The present invention avoids the cumbersome modification process of graphene, but organically combines the exfoliation and modification of graphene, combines the production and application of materials, and realizes the integrated preparation of graphene / polypropylene composite materials;

[0081] 3. The preparation method proposed by the present invention is simple, efficient, green, environmentally friendly, low-cost, and has important industrial application value;

[0082] 4. The composite obtained by the present invention has uniform dispersion of graphene, strong interface interaction, superior comprehensive material performance and wide application range.

[0083] All raw materials involved in the present invention can be purchased on the market. For example: expanded graphite (Qingdao Jinke Graphite Co., Ltd.); strong acids such as sulfuric acid and oxidants such as potassium permanganate (Sinopharm Chemical Reagent Co., Ltd.); maleic anhydride grafted polypropylene emulsion (Shanghai Joule Wax Co., Ltd.); isotactic polypropylene (Sinopec Zhenhai Refining and Chemical Co., Ltd.). BRIEF DESCRIPTION OF THE DRAWINGS

[0084] Figure 1 (a) TEM image of the MOG sheet and (b) HRTEM image of the edge of the MOG sheet in Example 1.

[0085] Figure 2 These are the selected area electron diffraction pattern corresponding to (c) of Example 1 and (d) the (1010) and (2110) diffraction peak intensity patterns.

[0086] Figure 3 (a) TGA curves of PP-g nanocomposites with different MOG contents.

[0087] Figure 4 (b) DTG curves of PP-g nanocomposites with different MOG contents.

[0088] Figure 5 (c) Tonset, T-50, and Tmax comparison chart of PP-g nanocomposites with different MOG contents.

[0089] Figure 6 (a) Stress-strain curves of PP-g nanocomposites with different MOG contents.

[0090] Figure 7 (b) Tensile strength and Young’s modulus of PP-g nanocomposites with different MOG contents. DETAILED DESCRIPTION

[0091] The present invention further describes the technical scheme in detail through the following examples, but the present invention is not limited to these examples.

[0092] Unless otherwise specified, the devices used in the examples are all devices commonly used in the art and commercially available on the market.

[0093] Raw materials in the embodiment:

[0094] Expanded graphite can be prepared by conventional methods, wherein chemical expanded graphite can be prepared by the method disclosed in the Chinese patent publication (CN105253878A) of our research group. An exemplary preparation method is as follows: 20 ml of hydrogen peroxide solution (Sinopharm Chemical Reagent Co., Ltd., 30% concentration) is added to 180 ml of concentrated sulfuric acid (Sinopharm Chemical Reagent Co., Ltd., 98% concentration) and mixed evenly, then 2 g of flake graphite (Sigma-Aldrich reagent, brand 808113) is added, and the mixture is allowed to stand for expansion for 24 hours, and chemical expanded graphite is obtained after separation.

[0095] The heat-expandable graphite was obtained by heating expandable graphite (purchased from Qingdao Jintao Graphite Co., Ltd.) at 800°C for 60s.

[0096] Microwave expanded graphite is obtained by expanding expandable graphite (purchased from Qingdao Jintao Graphite Co., Ltd.) in a 60 Hz microwave oven for 5 seconds.

[0097] Sulfuric acid and potassium permanganate: Sinopharm Chemical Reagent Co., Ltd.

[0098] Maleic anhydride grafted polypropylene (MAPP) emulsion with a solid content of 5%: Shanghai Joule Wax Co., Ltd., brand EP15.

[0099] Isotactic polypropylene: China Petrochemical Corporation Zhenhai Refining and Chemical Co., Ltd., brand name T30S.

[0100] Maleic anhydride grafted polyethylene (MAPE) emulsion with a solid content of 10%: Shanghai Joule Wax Co., Ltd., EM21335, solid content 35%, diluted to 10% before use.

[0101] Ethylene vinyl acetate (EVA) emulsion with a solid content of 20%: Shandong Yueyang New Materials Co., Ltd., BJ-806H, solid content 60%, diluted to 20% before use.

[0102] Example 1

[0103] 1) 2g potassium permanganate was dissolved in 400ml of concentrated sulfuric acid (98wt%), then 2g chemical expanded graphite (prepared by the above method) was added and mixed evenly, the temperature of the reaction system was controlled to be 35°C, and after continuous stirring for 1 hour, it was slowly added to ice water for quenching, and then 10ml hydrogen peroxide (30% concentration) was added and stirred for 5 minutes, and a low-oxidation expanded graphite (MOCEG) product was obtained after filtering and washing. The degree of oxidation was controlled by the amount of potassium permanganate and the reaction time. As the degree of oxidation, the carbon-oxygen atomic ratio of the product (obtained by detection by a German SPECTRO emission spectrometer) was 3.9:1.

[0104] 2) The above MOCEG was added to 40 g of maleic anhydride grafted polypropylene (MAPP) emulsion (Shanghai Joule Wax Co., Ltd., brand P15) with a solid content of 5%, and stirred evenly. The mixed system was then treated with probe ultrasound (350 W) for 2 h to obtain a MAPP / graphene dispersion, and the dispersion was placed in an 80° C. forced air oven and dried for 48 hours to obtain MAPP-modified graphene particles, in which the mass of graphene accounted for about 50 wt%.

[0105] 3) 4 g of modified graphene particles and 36 g of polypropylene (isotactic polypropylene: China Petrochemical Corporation Zhenhai Refining and Chemical Co., Ltd., brand T30S) were premixed at high speed at room temperature for 5 min, and then banburying at 200° C. for 8 min to obtain a modified graphene / polypropylene composite, and the final mass fraction of graphene in the composite was 5 wt%. The code name is PP-g-MOG-5.0.

[0106] Example 2

[0107] 1) Dissolve 15g potassium dichromate in 450ml concentrated sulfuric acid, then add 3g thermal expansion graphite (prepared by the above method) and mix well, control the temperature of the reaction system to 35°C, stir and react for 20 minutes, then slowly add it into ice water to quench, then add 75ml hydrogen peroxide (30%) and stir for 5 minutes, filter and wash to obtain a low oxidation degree expansion graphite (MOCEG) product. The oxidation degree is controlled by the amount of potassium dichromate and the reaction time. The carbon oxygen atomic ratio of the product is 4.7:1.

[0108] 2) The above MOCEG was added to 70 g of maleic anhydride grafted polyethylene (MAPE) emulsion (Shanghai Joule Wax Co., Ltd., EM21335) with a solid content of 10%, and stirred evenly. The mixed system was then treated with water bath ultrasound (600 W) for 5 h to obtain a MAPE / graphene dispersion. The dispersion was freeze-dried for 72 hours to obtain MAPE-modified graphene particles, in which the mass of graphene accounted for about 30 wt%.

[0109] 3) 10 g of modified graphene particles were premixed with 290 g of polypropylene at room temperature for 5 min at high speed, and then blended in a twin-screw extruder at 190° C. for 5 min to obtain a modified graphene / polypropylene composite, wherein the mass fraction of graphene in the composite was 1 wt %. The code name is PP-g-MOG-1.0.

[0110] Example 3

[0111] 1) Dissolve 5g potassium perchlorate in 1000ml concentrated sulfuric acid, then add 10g microwave expanded graphite (prepared by the above method) and mix well, control the temperature of the reaction system to 35°C, stir and react for 2 hours, then slowly add it into ice water to quench, then add 2ml hydrogen peroxide (30%) and stir for 5 minutes, filter and wash to obtain a low-oxidation expanded graphite (MOCEG) product. The oxidation degree is controlled by the amount of potassium perchlorate and the reaction time. The carbon-oxygen atomic ratio of the product is 3.7:1.

[0112] 2) The above MOCEG was added to 450 g of ethylene-vinyl acetate (EVA) emulsion (Shandong Yueyang New Materials Co., Ltd., brand BJ-707) with a solid content of 20%, stirred evenly, and then the mixed system was treated in a sand mill at 2500 rpm for 10 h to obtain an EVA / graphene dispersion, and the dispersion was microwave-dried to obtain EVA-modified graphene particles, in which the mass of graphene accounted for about 10 wt%.

[0113] 3) 20 g of modified graphene particles and 18 g of polypropylene were premixed at high speed at room temperature for 5 min, and then banburying was performed at 210° C. for 10 min to obtain a modified graphene / polypropylene composite, and the final mass fraction of graphene in the composite was 10 wt %.

[0114] Example 4

[0115] 1) Dissolve 0.5g potassium ferrate in 250ml concentrated sulfuric acid, then add 2g chemical expanded graphite (prepared by the above method) and mix well, control the temperature of the reaction system to 35°C, stir and react for 3 hours, then slowly add it into ice water to quench, then add 2.5ml hydrogen peroxide (30%) and stir for 5 minutes, filter and wash to obtain a low-oxidation expanded graphite (MOCEG) product. The oxidation degree is controlled by the amount of potassium ferrate and the reaction time. The carbon-oxygen atomic ratio of the product is 3.8:1.

[0116] 2) The above MOCEG was added to 20 g of maleic anhydride grafted ethylene-vinyl acetate copolymer (MA-g-EVA) emulsion (Shandong Yueyang New Materials Co., Ltd., BJ-806H) with a solid content of 15%, and stirred evenly. The mixed system was then sheared with a high-speed shearing device at 11000 rpm for 3 h to obtain a MA-g-EVA / graphene dispersion. The dispersion was freeze-dried for 48 hours to obtain MA-g-EVA modified graphene particles, wherein the mass proportion of graphene was about 40%.

[0117] 3) 5 g of modified graphene particles were premixed with 395 g of polypropylene at room temperature for 5 min at high speed, and then blended in a twin-screw extruder at 195° C. for 5 min to obtain a modified graphene / polypropylene composite, wherein the mass fraction of graphene in the composite was 0.5%, codenamed PP-g-MOG-0.5.

[0118] Example 5

[0119] 1) Dissolve 4g potassium permanganate in 500ml concentrated sulfuric acid, then add 2g thermochemical expanded graphite (prepared by the above method) and mix well, control the temperature of the reaction system to 35°C, stir continuously for 40 minutes, then slowly add it into ice water to quench, then add 20ml hydrogen peroxide (30%) and stir for 5 minutes, filter and wash to obtain a low-oxidation expanded graphite (MOCEG) product. The oxidation degree is controlled by the amount of potassium permanganate and the reaction time. The carbon-oxygen atomic ratio of the product is 3.3:1.

[0120] 2) The above MOCEG was added to 100 g of 8% isooctylphenyl polyoxyethylene ether (X-100) emulsion (Sinopharm Chemical Reagent Co., Ltd., brand 30188928) with a solid content of 8%, and stirred evenly. The mixed system was then treated in a ball mill at 400 rpm for 24 h to obtain X-100 / graphene slurry, and the slurry was placed in an 80° C. blast oven and dried for 48 hours to obtain X-100-modified graphene particles, in which the mass of graphene accounted for about 20%.

[0121] 3) 4 g of modified graphene particles were premixed with 36 g of polypropylene at high speed at room temperature for 5 min, and then kneaded at 185° C. for 10 min to obtain a modified graphene / polypropylene composite, and the final mass fraction of graphene in the composite was 2%.

[0122] Example 6

[0123] 1) 6g potassium perchlorate is dissolved in 550ml concentrated sulfuric acid, and then 2g chemical expanded graphite (prepared by the above method) is added and mixed evenly, the temperature of the reaction system is controlled to 35°C, and after continuous stirring for 30 minutes, it is slowly added into ice water for quenching, and then 30ml hydrogen peroxide (30%) is added and stirred for 5 minutes, and after filtering and washing, a low-oxidation expanded graphite (MOCEG) product is obtained. The oxidation degree is determined by the amount of potassium perchlorate and the reaction time. The carbon-oxygen atomic ratio of the product is 3.9:1.

[0124] 2) The above MOCEG was added to 25 g of a polypropylene wax (PPW) emulsion (Shanghai Tongyi Chemical, brand Lakewax 78) with a solid content of 24%, stirred evenly, and then the mixed system was treated in a ball mill at 400 rpm for 24 h to obtain a PPW / graphene slurry, and the slurry was vacuum dried for 36 hours to obtain PPW-modified graphene particles, in which the mass of graphene accounted for about 25%.

[0125] 3) 4.8 g of modified graphene particles and 35.2 g of polypropylene were premixed at high speed at room temperature for 5 min, and then banburying was performed at 200° C. for 8 min to obtain a modified graphene / polypropylene composite, wherein the mass fraction of graphene in the composite was 3 wt %. The composite was named PP-g-MOG-3.0.

[0126] Example 7

[0127] 1) Dissolve 2g potassium ferrate in 300ml concentrated sulfuric acid, then add 2g thermal expansion graphite (prepared by the above method) and mix well, control the temperature of the reaction system to 35°C, stir and react for 1 hour, then slowly add it into ice water to quench, then add 10ml hydrogen peroxide (30%) and stir for 5 minutes, filter and wash to obtain low oxidation degree expansion graphite (MOCEG) product. The oxidation degree is determined by the amount of potassium ferrate and the reaction time. The carbon oxygen atomic ratio of the product is 3.8:1.

[0128] 2) The above MOCEG was added to 50 g of polyethylene wax (PEW) emulsion (BASF, Poligen WE6) with a solid content of 8%, stirred evenly, and then the mixed system was treated with probe ultrasound (350 W) for 2 h to obtain a PEW / graphene dispersion, and the dispersion was fluidized and dried for 10 hours to obtain PEW-modified graphene particles, in which the mass proportion of graphene was about 33%.

[0129] 3) 6 g of modified graphene particles were premixed with 44 g of polypropylene at high speed at room temperature for 5 min, and then kneaded at 210° C. for 7 min to obtain a modified graphene / polypropylene composite, and the final mass fraction of graphene in the composite was 4%.

[0130] Example 8

[0131] 1) Dissolve 3g potassium dichromate in 400ml concentrated sulfuric acid, then add 2g microwave expanded graphite (prepared by the above method) and mix well, control the temperature of the reaction system to 35°C, stir and react for 50 minutes, then slowly add it into ice water to quench, then add 15ml hydrogen peroxide (30%) and stir for 5 minutes, filter and wash to obtain a low-oxidation expanded graphite (MOCEG) product. The oxidation degree is determined by the amount of potassium dichromate and the reaction time. The carbon-oxygen atomic ratio of the product is 3.2:1.

[0132] 2) The above MOCEG was added to 400 g of a poloxamer (F-127) emulsion (Sigma-Aldrich, brand P2443) with a solid content of 2%, stirred evenly, and then the mixed system was subjected to high-pressure spraying at a flow rate of 1 L / h and a fluid pressure of 20 MPa to obtain an F-127 / graphene dispersion, and the dispersion was spray-dried to obtain F-127-modified graphene particles, in which the mass of graphene accounted for about 20%.

[0133] 3) 10 g of modified graphene particles were premixed with 190 g of polypropylene at high speed at room temperature for 5 min, and then blended in a twin-screw extruder at 200° C. for 6 min to obtain a modified graphene / polypropylene composite, wherein the mass fraction of graphene in the composite was 1%.

[0134] Example 9

[0135] 1) Dissolve 2g potassium permanganate in 400ml concentrated sulfuric acid, then add 2g chemical expanded graphite (prepared by the above method) and mix well, control the temperature of the reaction system to 35°C, stir and react for 1 hour, then slowly add it into ice water to quench, then add 10ml hydrogen peroxide (30%) and stir for 5 minutes, filter and wash to obtain a low-oxidation expanded graphite (MOCEG) product. The oxidation degree is controlled by the amount of potassium permanganate and the reaction time. The carbon-oxygen atomic ratio of the product is 4.0:1.

[0136] 2) The above MOCEG is added to 1000 g of maleic anhydride grafted polyethylene (MAPE) emulsion (Shanghai Joule Wax Co., Ltd., EM21335) with a solid content of 1.8%, and stirred evenly. The mixed system is then subjected to high-pressure spraying at a flow rate of 10 L / h and a fluid pressure of 200 MPa to obtain a MAPE / graphene dispersion. The dispersion is fluidized and dried to obtain MAPE-modified graphene particles, in which the mass of graphene accounts for about 10%.

[0137] 3) 20 g of modified graphene particles were premixed with 980 g of polypropylene at room temperature for 10 min at high speed, and then banburying was performed at 200° C. for 10 min to obtain a modified graphene / polypropylene composite, wherein the final mass fraction of graphene in the composite was 0.2%.

[0138] Example 10

[0139] 1) Dissolve 2g of potassium permanganate in 400ml of concentrated sulfuric acid, then add 2g of chemical expanded graphite (prepared by the above method) and mix well, control the temperature of the reaction system to 35°C, stir and react for 1 hour, then slowly add it into ice water to quench, then add 10ml of hydrogen peroxide (30%) and stir for 5 minutes, filter and wash to obtain a low-oxidation expanded graphite (MOCEG) product. The oxidation degree is controlled by the amount of potassium permanganate and the reaction time. The carbon-oxygen atomic ratio of the product is 3.9:1.

[0140] 2) The above MOCEG was added to 100 g of maleic anhydride grafted ethylene-octene copolymer (MA-g-POE) emulsion (Shanghai Tongyi Chemical, Novaseal 2225) with a solid content of 2%, and stirred evenly. The mixed system was then treated with probe ultrasound (350 W) for 2 h to obtain a MA-g-POE / graphene dispersion, and the dispersion was freeze-dried for 72 hours to obtain MA-g-POE-modified graphene particles, in which the mass of graphene accounted for about 50%.

[0141] 3) 4 g of modified graphene particles were premixed with 46 g of polypropylene at room temperature for 5 min at high speed, and then kneaded at 200° C. for 8 min to obtain a modified graphene / polypropylene composite, and the final mass fraction of graphene in the composite was 8%.

[0142] The performance test results of the products of various codes obtained in the above embodiments are shown in the accompanying drawings.

Claims

1. A method for preparing a modified graphene / polyolefin composite, the method comprising the following steps: (1) subjecting expanded graphite to intercalation oxidation in a mixed solution of a strong acid and a strong oxidant to obtain expanded graphite with a low degree of oxidation; (2) uniformly mixing the low-oxidation expanded graphite obtained in step (1) and a compatibilizer emulsion, and subjecting the mixture to mechanical exfoliation to obtain a compatibilizer-modified graphene suspension (A), wherein the compatibilizer emulsion is formed by emulsifying a polyolefin-type compatibilizer or a polyether-type compatibilizer in water with an emulsifier or a surfactant; (3) drying the compatibilizer-modified graphene suspension (A) obtained in step (2) to obtain a compatibilizer-modified graphene particle (B), and (4) melt-blending the graphene particles (B) modified by the compatibilizer obtained in step (3) with a polyolefin as a matrix to obtain a modified graphene / polyolefin composite (C).

2. The preparation method according to claim 1, wherein In step (1), the "low oxidation degree" in the low oxidation degree expanded graphite means that the carbon-oxygen atomic ratio in the oxidized expanded graphite is between 1.5-8:1, preferably between 2.5-6:1, preferably between 3-5.5:1, preferably between 3.2-5:1, and more preferably between 3.5-4.5:1; and / or In step (2), the concentration of graphene in the graphene suspension (A) is 0.01-200 mg / ml, preferably 0.1-150 mg / ml, more preferably 1-120 mg / ml, more preferably 5-100 mg / ml, more preferably 10-80 mg / ml, more preferably 15-60 mg / ml, more preferably 10-50 mg / ml; and / or In step (4), the polyolefin is a polyolefin plastic, a polyolefin elastomer, or a mixture of the two.

3. The preparation method according to claim 1 or 2, wherein The expanded graphite used in step (1) is one or more selected from chemically expanded graphene, thermally expanded graphite, and microwave expanded graphite; and / or The strong oxidant in step (1) is one or more selected from potassium permanganate, potassium perchlorate, potassium ferrate, potassium dichromate, potassium nitrate, sodium nitrate, potassium persulfate, sodium persulfate, and ammonium persulfate; and / or The strong acid used in step (1) is one or more selected from concentrated sulfuric acid, concentrated hydrochloric acid, concentrated nitric acid, and concentrated phosphoric acid; and / or The number average molecular weight of the polyolefin type compatibilizer or the polyether type compatibilizer is between 1000 and 70000, preferably between 1200 and 60000, and more preferably between 1500 and 50000.

4. The preparation method according to claim 2, wherein The polyolefin plastic is one or more selected from polypropylene, propylene copolymer, polyethylene, ethylene copolymer, ethylene-vinyl acetate copolymer, poly-1-butene, 1-butene copolymer; and / or The polyolefin elastomer is one or more selected from ethylene-1-butene elastomer, ethylene-1-octene elastomer, and ethylene / propylene elastomer.

5. The preparation method according to any one of claims 1 to 4, wherein: The compatibilizer emulsion is one or more selected from the following polymer compatibilizer emulsions: polyethylene wax emulsion, polypropylene wax emulsion, ethylene-vinyl acetate copolymer emulsion, isooctylphenyl polyoxyethylene ether (e.g., Triton), polyoxyethylene polyether, polyoxypropylene polyether, polyoxyethylene polyoxypropylene (e.g., poloxamer), maleic anhydride grafted polyethylene emulsion, maleic anhydride grafted polypropylene emulsion, maleic anhydride grafted ethylene-vinyl acetate copolymer emulsion, maleic anhydride grafted ethylene-butene copolymer emulsion and maleic anhydride grafted ethylene-octene copolymer emulsion.

6. The preparation method according to any one of claims 1 to 5, wherein: The solid content of the compatibilizer emulsion used in step (2) is 1-50wt%, preferably 3-48wt%, preferably 5-46wt%, preferably 7-45wt%, preferably 9-43wt%, preferably 10-40wt%, preferably 15-37wt%, preferably 18-35wt%, preferably 20-30wt%; and / or In step (2), the mass ratio of the solid component in the compatibilizer emulsion to the low-oxidation expanded graphite is (0.4-9):1, preferably (0.8-8.5):1, preferably (1.2-8):1, preferably (1.5-7):1, preferably (1.7-6):1, preferably (1.8-5):1, preferably (2.0-4.0):1; and / or In step (2), the amount of low oxidation expanded graphite relative to the compatibilizer emulsion should be such that the concentration of graphene in the resulting compatibilizer-modified graphene suspension (A) is 0.01-250 mg / ml, preferably 0.05-230 mg / ml, preferably 0.1-200 mg / ml, preferably 0.5-190 mg / ml, preferably 0.8-180 mg / ml, preferably 1-170 mg / ml, preferably 1.5-165 mg / ml, preferably 2.0-160 mg / ml; and / or In step (3), in the compatibilizer-modified graphene particles (B), the mass percentage of graphene is in the range of 5-70wt%, preferably 7-65wt%, preferably 8-60wt%, preferably 9-55wt%, preferably 10-50wt%, preferably 15-45wt%, preferably 20-40wt%, preferably 25-35wt%, based on the total weight of the compatibilizer-modified graphene particles (B); and / or In step (4), the amount of compatibilizer-modified graphene particles (B) relative to polyolefin should be such that in the resulting modified graphene / polyolefin composite (C), the mass percentage or weight percentage of graphene is 0.05-25wt%, preferably 0.1-20wt%, preferably 0.15-15wt%, preferably 0.20-13wt%, preferably 0.25-12wt%, preferably 0.30-10wt%, preferably 0.35-9wt%, preferably 0.40-8wt%, based on the total weight of the composite (C).

7. The preparation method according to any one of claims 1 to 6, wherein: The mechanical exfoliation in step (2) includes one or more combinations of ball milling, sand milling, water bath ultrasound, probe ultrasound, high-speed shearing, high-pressure homogenization, and Taylor-Couette fluid exfoliation; and / or The melt blending in step (3) includes internal mixing, single-screw extrusion or twin-screw extrusion.

8. A modified graphene / polyolefin composite obtained by the method of any one of claims 1 to 7, wherein the mass percentage of graphene, i.e. the mass fraction of graphene in composite C, is 0.05-25wt%, preferably 0.1-20wt%, preferably 0.15-15wt%, preferably 0.20-13wt%, preferably 0.25-12wt%, preferably 0.30-10wt%, preferably 0.35-9wt%, preferably 0.40-8wt%, for example 0.50, 0.60, 0.70, 0.80, 0.90, 1.0, 1.2, 1.5, 1.8, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5wt%, based on the total weight of composite (C).

9. Compatibilizer-modified graphene particles (B), wherein: It is prepared by a preparation method comprising the following steps: (1) subjecting expanded graphite to intercalation oxidation in a mixed solution of a strong acid and a strong oxidant to obtain expanded graphite with a low degree of oxidation; (2) uniformly mixing the low-oxidation expanded graphite obtained in step (1) and a compatibilizer emulsion, and subjecting the mixture to mechanical exfoliation to obtain a compatibilizer-modified graphene suspension (A), wherein the compatibilizer emulsion is formed by emulsifying a polyolefin-type compatibilizer or a polyether-type compatibilizer in water with an emulsifier or a surfactant; (3) Drying the compatibilizer-modified graphene suspension (A) obtained in step (2) to obtain a compatibilizer-modified graphene particle (B).

10. The use of the modified graphene / polyolefin composite according to claim 8, characterized in that: It is used to reinforce polyolefins, it is used to prepare polymer nanocomposites, it is used in the production of functional inks and coatings, it is used as a raw material to produce high-performance modified polyolefin fibers through spinning technology, or, it is used as a raw material to produce non-woven fabrics that are resistant to pathogens (bacteria, viruses) through melt-blown technology.

Citation Information

Patent Citations

  • Preparation method of polymer / graphene composite material through in situ reduction

    CN101864098A

  • Method for preparing low oxidation degree graphene-modified polymethyl methacrylate (PMMA) composite material

    CN105273114A

  • Graphene-polypropylene composite master batch as well as preparation method and application thereof

    CN112175286A