Neodymium-iron-boron magnetic plastic material and preparation method thereof
By using self-developed reinforcing additives in NdFeB magnetic plastic materials to modify the magnetic powder surface and improve the compatibility of chlorinated polyethylene, the problem of poor compatibility between the magnetic powder and the plastic matrix is solved and the magnetic properties and mechanics are improved. The performance improvement broadens the application scope.
Patent Information
- Application Number
- CN202411099008.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The interface compatibility between the magnetic powder and the plastic matrix in traditional NdFeB magnetic plastic materials is poor, resulting in insufficient bonding strength and affecting the mechanical and magnetic properties of the composite material.
Using self-developed strengthening additives, mercaptoethanol is oxidized into disulfide with terminal hydroxyl groups, and vinyl chloroacetate is substituted with the hydroxyl groups in the intermediate molecules to introduce the terminal vinyl ester structure to form chelation and improve the surface modification of magnetic particles. The compatibility with chlorinated polyethylene, combined with the high-temperature initiating effect, forms a bridging effect to enhance the bonding strength between magnetic powder and chlorinated polyethylene.
It significantly improves the mechanical properties and magnetic properties of composite materials, broadens the application conditions of magnetic plastic materials, and achieves two-way improvement in magnetic and mechanical properties.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of magnetic composite materials, and in particular, relates to a NdFeB magnetic plastic material and a preparation method thereof. Background Art
[0002] NdFeB magnets are made of intermetallic compounds Nd2Fe 14 B-based permanent magnetic material has high remanence, coercive force and maximum magnetic energy product, and is one of the materials with the best magnetic properties among known commercial magnets. Traditional NdFeB magnets are hard and brittle materials that are difficult to process and shape, which greatly limits the application of magnets. The magnetic plastic material made by making it into powder and combining it with plastic has certain toughness and processability, and is widely used in electronic equipment, sensors, motors, speakers and other products.
[0003] However, in order to ensure good magnetic properties, the amount of magnetic powder used is usually high, and the interface compatibility between the magnetic powder and the plastic matrix is poor, resulting in insufficient bonding strength, thereby affecting the mechanical properties of the composite material. In the prior art, coupling agents are used to treat the surface of the magnetic powder, which can improve the compatibility of the magnetic powder and the plastic matrix to a certain extent. However, the bonding strength between these coupling agents and the magnetic powder is too high, which increases the viscosity of the magnetic powder during the melt blending process, limits the dispersion effect of the magnetic powder, and makes it difficult to further improve the magnetic properties and mechanical properties of the magnetic plastic material. Summary of the invention
[0004] In order to solve the technical problems mentioned in the background technology, the object of the present invention is to provide a NdFeB magnetic plastic material and a preparation method thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions: A NdFeB magnetic plastic material is made of the following components in terms of weight percentage: 8-15wt% of plastic masterbatch, 0.8-1.2wt% of reinforcing agent and 0.1-0.15wt% of initiator, and the balance is NdFeB magnetic powder; The strengthening aid is prepared by the following method: Step A1: mercaptoethanol and anhydrous ethanol are mixed, heated to 40-50°C, stirred at 60-90 rpm, PTAD is added in batches to react for 6-8 hours, and ethanol is removed by rotary evaporation after the reaction is completed. The mixture is frozen to 5°C, washed with n-hexane, and dried to obtain an intermediate; Furthermore, the usage ratio of mercaptoethanol, PTAD and anhydrous ethanol is 0.1 mol: 15-20 mg: 10-15 mL. Under the oxidation action of PTAD, mercaptoethanol is oxidized into disulfide with terminal hydroxyl groups.
[0006] Step A2: The intermediate, vinyl chloroacetate, triethylamine and anhydrous tetrahydrofuran are mixed, dry nitrogen is introduced for protection, the temperature is raised to 65-75° C., stirring is applied at 120-180 rpm, and reflux reaction is carried out for 2-3 hours. After the reaction is completed, tetrahydrofuran is removed by rotary evaporation, and the mixture is cooled to room temperature, washed with water, and vacuum dried to obtain a strengthening auxiliary agent; Furthermore, the usage ratio of the intermediate, vinyl chloroacetate, triethylamine and anhydrous tetrahydrofuran is 0.1 mol: 0.2 mol: 5-8 mL: 40-60 mL, and under the promotion of triethylamine, vinyl chloroacetate undergoes substitution reaction with the hydroxyl group in the intermediate molecule.
[0007] A method for preparing a NdFeB magnetic plastic material comprises the following steps: Step S1: dissolving the strengthening agent and acetone, adding NdFeB magnetic powder and mixing, baking to remove acetone, adding plastic masterbatch and refining, adding initiator and mixing, crushing the material to obtain composite masterbatch; Furthermore, the refining temperature is 145-155° C., and the amount of acetone used is 4-5 times the mass of the strengthening auxiliary agent.
[0008] Step S2: placing the composite masterbatch in a calender for lamination, then molding and shaping, cutting and shaping the material, and magnetizing to obtain a NdFeB magnetic plastic material.
[0009] Furthermore, the lamination temperature is 120-130° C., the number of laminations is 3-5 times, and the reduction amount of a single lamination is 55-70%.
[0010] Furthermore, the molding temperature is 160-170° C. and the pressure is 2.5-3 MPa.
[0011] Preferably, the NdFeB magnetic powder is isotropic magnetic powder with a fineness of not less than 325 mesh.
[0012] Preferably, the plastic masterbatch is chlorinated polyethylene.
[0013] Preferably, the initiator is calcium peroxide.
[0014] Beneficial effects of the present invention: The invention uses NdFeB magnetic powder as magnetic material and chlorinated polyethylene as viscous plastic material, and introduces a self-developed strengthening auxiliary agent for blending to improve the mechanical properties and magnetic properties of the composite material; the strengthening auxiliary agent is oxidized from mercaptoethanol to a disulfide with terminal hydroxyl groups, i.e., an intermediate, and then chloroacetic acid vinyl ester replaces the hydroxyl groups in the intermediate molecule to introduce terminal vinyl ester structure modification; the disulfide structure in the strengthening auxiliary agent molecule forms a chelating effect, and is loaded onto the surface of the NdFeB magnetic powder during the blending process to modify the surface of the magnetic powder; the vinyl ester structure at both ends of the molecule is highly compatible with the chlorinated polyethylene and is easily infiltrated by the chlorinated polyethylene during the blending process, and the strengthening auxiliary agent is different from common titanate and silane coupling agents in that the chelating effect of ...hydroxyl groups in the intermediate molecule are replaced by terminal vinyl ester structure modification; the disulfide structure in the strengthening auxiliary agent molecule forms a chelating effect, and is loaded onto the surface of the NdFeB magnetic powder during the blending process to modify the surface of the magnetic powder; the vinyl ester structure at both ends of the molecule is highly compatible with the chlorinated polyethylene and is easily infiltrated by the chlorinated polyethylene during the blending process, and the strengthening auxiliary agent is different from common titanate and silane coupling agents in that the strengthening auxiliary agent has a chelating effect. The effect is weakened during the blending temperature rise process, and the disulfide structure may be destroyed, which makes the binding force between the magnetic powder and the reinforcing agent weaker. The two can move freely during the blending process. The reinforcing agent forms a sufficient lubricating effect between the magnetic powder and the chlorinated polyethylene, which is beneficial to the uniform dispersion of the magnetic powder and improves the magnetic properties. During the compression molding process, the vinyl ester structure is added to the residual unsaturated structure in the chlorinated polyethylene under the action of high temperature initiation. During the cooling process, the chelation effect is restored again, and the reinforcing agent forms a bridging effect to strengthen the bonding strength between the magnetic powder and the chlorinated polyethylene, so that the composite material has good mechanical properties. Thanks to the two-way improvement of magnetic and mechanical properties, the application conditions of magnetic plastic materials have been greatly broadened. DETAILED DESCRIPTION
[0015] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0016] Example 1, preparation of NdFeB magnetic plastic material, the specific implementation process is as follows: (1) Preparation of strengthening additives Step A1: Mix mercaptoethanol and anhydrous ethanol, heat to 50°C, stir at 90rpm, add PTAD (4-phenyl-1,2,4-triazolin-3,5-dione) in two batches, add two-thirds of the first batch, add the remaining PTAD after an interval of 1.5h, continue to stir at a constant temperature after complete addition, and control the total reaction time of PTAD addition to be 6h, wherein the amount ratio of mercaptoethanol, PTAD and anhydrous ethanol is 0.1mol:20mg:15mL. After the reaction is completed, remove ethanol by rotary evaporation, freeze to 5°C, wash with n-hexane, and dry to obtain an intermediate.
[0017] Step A2: Take the intermediate, vinyl chloroacetate, triethylamine and anhydrous tetrahydrofuran, mix them, introduce dry nitrogen protection, heat to 75°C, stir at 180rpm, and reflux for 2h, wherein the amount ratio of the intermediate, vinyl chloroacetate, triethylamine and anhydrous tetrahydrofuran is 0.1mol:0.2mol:8mL:60mL. After the reaction, remove tetrahydrofuran by rotary evaporation, cool to room temperature, wash with water, and vacuum dry to obtain a strengthening auxiliary agent.
[0018] (2) Preparation of NdFeB magnetic plastic materials The raw materials are taken according to weight percentage: 15wt% plastic masterbatch, CPE135A raw material of Shandong Bangtai Petrochemical (Group) Co., Ltd. is used in the implementation process; 0.8wt% strengthening agent, which is self-made in this embodiment; 0.1wt% initiator, high-temperature initiator calcium peroxide is used in the implementation process; 84.1wt% neodymium iron boron magnetic powder, 400 mesh isotropic magnetic powder of Guangzhou Xinnod Transmission Parts Co., Ltd. is used in the implementation process.
[0019] Step S1: Dissolve the strengthening agent and acetone 5 times its mass, add NdFeB magnetic powder and stir to mix for 1 hour, bake to remove acetone, add plastic masterbatch and mix and start refining, control the refining temperature to 155°C, start rolling after 15 minutes of refining, add initiator and mix, crush the material to obtain composite masterbatch.
[0020] Step S2: placing the composite masterbatch in a calender for lamination, controlling the lamination temperature to 130°C, the lamination times to 3 times, the single lamination reduction amount to 70%, and then molding, controlling the molding temperature to 170°C, the pressure to 2.5MPa, making a sheet with a thickness of 5mm, cutting and shaping the material, placing it in a magnetizer for magnetization, and obtaining a NdFeB magnetic plastic material.
[0021] Example 2, preparation of NdFeB magnetic plastic material, the specific implementation process is as follows: (1) Preparation of strengthening additives Step A1: Mix mercaptoethanol and anhydrous ethanol, heat to 40°C, stir at 60rpm, add PTAD in two batches, add two-thirds of the first batch, add the remaining PTAD after an interval of 2h, continue to stir at a constant temperature after complete addition, and control the total reaction time of PTAD to be 8h, wherein the amount ratio of mercaptoethanol, PTAD and anhydrous ethanol is 0.1mol:15mg:10mL. After the reaction is completed, remove ethanol by rotary evaporation, freeze to 5°C, wash with n-hexane and dry to obtain an intermediate.
[0022] Step A2: Take the intermediate, vinyl chloroacetate, triethylamine and anhydrous tetrahydrofuran, mix them, introduce dry nitrogen protection, heat to 65°C, stir at 120rpm, and reflux for 3h, wherein the amount ratio of the intermediate, vinyl chloroacetate, triethylamine and anhydrous tetrahydrofuran is 0.1mol:0.2mol:5mL:40mL. After the reaction, remove tetrahydrofuran by rotary evaporation, cool to room temperature, wash with water, and vacuum dry to obtain a strengthening auxiliary agent.
[0023] (2) Preparation of NdFeB magnetic plastic materials The raw materials are taken according to weight percentage: 8wt% plastic masterbatch, CPE135A raw material of Shandong Bangtai Petrochemical (Group) Co., Ltd. is used in the implementation process; 1.2wt% strengthening agent, which is self-made in this embodiment; 0.15wt% initiator, high-temperature initiator calcium peroxide is used in the implementation process; 90.65wt% neodymium iron boron magnetic powder, 400 mesh isotropic magnetic powder of Guangzhou Xinnod Transmission Parts Co., Ltd. is used in the implementation process.
[0024] Step S1: Dissolve the strengthening agent and acetone of 4 times its mass, add NdFeB magnetic powder and stir to mix for 1 hour, bake to remove acetone, add plastic masterbatch and mix and start refining, control the refining temperature to 145°C, start rolling after 18 minutes of refining, add initiator and mix, crush the material to obtain composite masterbatch.
[0025] Step S2: placing the composite masterbatch in a calender for lamination, controlling the lamination temperature to 120°C, the number of laminations to 5 times, the single lamination reduction amount to 55%, and then molding, controlling the molding temperature to 160°C, the pressure to 3MPa, making a sheet with a thickness of 5mm, cutting and shaping the material, placing it in a magnetizer for magnetization, and obtaining a NdFeB magnetic plastic material.
[0026] Example 3, preparation of NdFeB magnetic plastic material, the specific implementation process is as follows: (1) Preparation of strengthening additives Step A1: Mix mercaptoethanol and anhydrous ethanol, heat to 45°C, stir at 90rpm, add PTAD in two batches, add two-thirds of the first batch, add the remaining PTAD after an interval of 1.8h, continue to stir at a constant temperature after complete addition, and control the total reaction time of PTAD to be 7h, wherein the amount ratio of mercaptoethanol, PTAD and anhydrous ethanol is 0.1mol:18mg:12mL. After the reaction is completed, remove ethanol by rotary evaporation, freeze to 5°C, wash with n-hexane and dry to obtain an intermediate.
[0027] Step A2: Take the intermediate, vinyl chloroacetate, triethylamine and anhydrous tetrahydrofuran, mix them, pass dry nitrogen protection, heat to 70°C, stir at 120rpm, and reflux for 2.2h, wherein the amount ratio of the intermediate, vinyl chloroacetate, triethylamine and anhydrous tetrahydrofuran is 0.1mol:0.2mol:7mL:45mL. After the reaction, remove tetrahydrofuran by rotary evaporation, cool to room temperature, wash with water, and vacuum dry to obtain a strengthening auxiliary agent.
[0028] (2) Preparation of NdFeB magnetic plastic materials The raw materials are taken according to weight percentage: 13wt% plastic masterbatch, CPE135A raw material of Shandong Bangtai Petrochemical (Group) Co., Ltd. is used in the implementation process; 0.9wt% strengthening agent, which is self-made in this embodiment; 0.12wt% initiator, high-temperature initiator calcium peroxide is used in the implementation process; 85.98wt% neodymium iron boron magnetic powder, 400 mesh isotropic magnetic powder of Guangzhou Xinnod Transmission Parts Co., Ltd. is used in the implementation process.
[0029] Step S1: Dissolve the strengthening agent and acetone 5 times its mass, add NdFeB magnetic powder and stir to mix for 1 hour, bake to remove acetone, add plastic masterbatch and mix and start refining, control the refining temperature to 150°C, start rolling after 16 minutes of refining, add initiator and mix, crush the material to obtain composite masterbatch.
[0030] Step S2: placing the composite masterbatch in a calender for lamination, controlling the lamination temperature to 120°C, the lamination times to 4 times, the single lamination reduction amount to 60%, and then molding, controlling the molding temperature to 165°C, the pressure to 2.5MPa, making a sheet with a thickness of 5mm, cutting and shaping the material, placing it in a magnetizer for magnetization, and obtaining a NdFeB magnetic plastic material.
[0031] Example 4, preparation of NdFeB magnetic plastic material, the specific implementation process is as follows: (1) Preparation of strengthening additives Step A1: Mix mercaptoethanol and anhydrous ethanol, heat to 50°C, stir at 60rpm, add PTAD in two batches, add two-thirds of the first batch, add the remaining PTAD after an interval of 1.7h, continue to stir at a constant temperature after complete addition, and control the total reaction time of PTAD addition to be 6.5h, wherein the amount ratio of mercaptoethanol, PTAD and anhydrous ethanol is 0.1mol:15mg:15mL. After the reaction is completed, remove ethanol by rotary evaporation, freeze to 5°C, wash with n-hexane and dry to obtain an intermediate.
[0032] Step A2: Take the intermediate, vinyl chloroacetate, triethylamine and anhydrous tetrahydrofuran, mix them, introduce dry nitrogen protection, heat to 70°C, stir at 180rpm, and reflux for 2.8h, wherein the amount ratio of the intermediate, vinyl chloroacetate, triethylamine and anhydrous tetrahydrofuran is 0.1mol:0.2mol:6mL:55mL. After the reaction, remove tetrahydrofuran by rotary evaporation, cool to room temperature, wash with water, and vacuum dry to obtain a strengthening auxiliary agent.
[0033] (2) Preparation of NdFeB magnetic plastic materials The raw materials are taken according to weight percentage: 11wt% of plastic masterbatch, CPE135A type raw material of Shandong Bangtai Petrochemical (Group) Co., Ltd. is used in the implementation process; 1wt% of strengthening auxiliary agent is self-made in this embodiment; 0.13wt% of initiator, high-temperature initiator calcium peroxide is used in the implementation process; 87.87wt% of neodymium iron boron magnetic powder, 400 mesh isotropic magnetic powder of Guangzhou Xinnod Transmission Parts Co., Ltd. is used in the implementation process.
[0034] Step S1: Dissolve the strengthening agent and acetone of 4 times its mass, add NdFeB magnetic powder and stir to mix for 1 hour, bake to remove acetone, add plastic masterbatch and mix and start refining, control the refining temperature to 150°C, start rolling after 17 minutes of refining, add initiator and mix, crush the material to obtain composite masterbatch.
[0035] Step S2: placing the composite masterbatch in a calender for lamination, controlling the lamination temperature to 125°C, the number of laminations to 4 times, the single lamination reduction amount to 65%, and then molding, controlling the molding temperature to 170°C, the pressure to 2.8MPa, making a sheet with a thickness of 5mm, cutting and shaping the material, placing it in a magnetizer for magnetization, and obtaining a NdFeB magnetic plastic material.
[0036] Comparative Example 1 This comparative example refers to Example 4, except that no reinforcing agent is added and it is replaced with plastic masterbatch of the same weight, and the rest of the implementation process is exactly the same.
[0037] Comparative Example 2 This comparative example refers to Example 4, except that no reinforcing agent is added and it is replaced by the same weight of titanate coupling agent CS-201, and the rest of the implementation process is exactly the same.
[0038] Samples were taken from the above NdFeB magnetic plastic materials, and the tensile properties were tested according to GB / T 1040.1-2018 standard; the Shore D hardness was tested according to GB / T 531.1-2008 standard; the magnetic properties of the samples were tested by FE-2100HAB-140 permanent magnetic material magnetic measuring instrument; the specific test results are shown in the following table:
[0039] It can be seen from the test data in the above table that the magnetic plastic material prepared in the embodiment has excellent toughness. At the same time, compared with the comparative example, the magnetic performance is stronger at the same magnetic powder ratio.
[0040] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0041] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A NdFeB magnetic plastic material, characterized in that: The composition is made of the following components according to weight percentage: 8-15wt% plastic masterbatch, 0.8-1.2wt% reinforcing agent and 0.1-0.15wt% initiator, and the balance is NdFeB magnetic powder; The strengthening aid is prepared by the following method: Step A1: Mix mercaptoethanol and anhydrous ethanol, heat to 40-50°C, stir and add PTAD in batches to react for 6-8h. After the reaction, remove ethanol by rotary evaporation, freeze to 5°C, wash with n-hexane and dry to obtain an intermediate; Step A2: The intermediate, vinyl chloroacetate, triethylamine and anhydrous tetrahydrofuran are mixed, dry nitrogen is introduced for protection, the temperature is raised to 65-75°C, and the mixture is stirred and refluxed for reaction for 2-3 hours. After the reaction is completed, tetrahydrofuran is removed by rotary evaporation, and the mixture is cooled to room temperature, washed with water, and vacuum dried to obtain a strengthening auxiliary agent.
2. A NdFeB magnetic plastic material according to claim 1, characterized in that: The usage ratio of mercaptoethanol, PTAD and anhydrous ethanol is 0.1 mol: 15-20 mg: 10-15 mL.
3. A NdFeB magnetic plastic material according to claim 2, characterized in that: The usage ratio of the intermediate, vinyl chloroacetate, triethylamine and anhydrous tetrahydrofuran is 0.1 mol: 0.2 mol: 5-8 mL: 40-60 mL.
4. The NdFeB magnetic plastic material according to claim 1, characterized in that: NdFeB magnetic powder is isotropic magnetic powder with a fineness not less than 325 mesh.
5. The NdFeB magnetic plastic material according to claim 1, characterized in that: The plastic masterbatch is chlorinated polyethylene and the initiator is calcium peroxide.
6. A method for preparing a NdFeB magnetic plastic material according to any one of claims 1 to 5, characterized in that: The steps include: Step S1: dissolving the strengthening agent and acetone, adding NdFeB magnetic powder and mixing, baking to remove acetone, adding plastic masterbatch and refining, adding initiator and mixing, crushing the material to obtain composite masterbatch; Step S2: placing the composite masterbatch in a calender for lamination, then molding and shaping, cutting and shaping the material, and magnetizing to obtain a NdFeB magnetic plastic material.
7. The method for preparing a NdFeB magnetic plastic material according to claim 6, characterized in that: The refining temperature is 145-155°C, and the amount of acetone used is 4-5 times the mass of the strengthening additive.
8. The method for preparing a NdFeB magnetic plastic material according to claim 6, characterized in that: The stacking temperature is 120-130°C, the stacking times are 3-5 times, and the single stacking reduction is 55-70%.
9. The method for preparing a NdFeB magnetic plastic material according to claim 6, characterized in that: The molding temperature is 160-170°C and the pressure is 2.5-3MPa.
Citation Information
Patent Citations
Corrosion-resistant magnetic composite material and preparation method therefor
CN105367873A
Polymer / cerium-neodymium-iron-boron magnetic composite material and preparation method thereof
CN106384641A
Metal-ion-loaded polyacrylamide magnetic bead, and preparation method and application thereof
CN109603775A
High-conductivity positive electrode material for lithium battery and preparation method of high-conductivity positive electrode material
CN116826061A
Novel 2-heteroaryl-substituted benzimidazole derivative
SG123486A1