Fluororubber system, fluororubber and preparation method and application thereof
By adding components such as magnetic nanoparticles to fluororubber and performing vulcanization treatment, a fluororubber with high hardness and thermal conductivity is prepared, which solves the problems of poor mechanical properties and insufficient high temperature resistance of fluororubber, and achieves high temperature resistance in high-temperature environments. Stable use and material recycling reduce usage costs.
Patent Information
- Application Number
- CN202310317533.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-01
AI Technical Summary
The existing fluorine rubber has poor mechanical properties, poor high temperature resistance, and is difficult to recycle, resulting in increased use costs.
Fluororubber raw rubber, magnetic nanoparticles, peroxide vulcanizing agent, vulcanization accelerator and processing aids are mixed in specific proportions and vulcanized to prepare a fluororubber system with high hardness, thermal conductivity and magnetic field response properties.
It improves the mechanical properties and thermal conductivity of fluorine rubber, enables stable use in high temperature environments, and realizes material recycling and cost reduction through magnetic field control.
Smart Images

Figure CN118725487A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sealing rubbers, and in particular to a fluororubber system, fluororubber, and a preparation method and application thereof. Background Art
[0002] Fluororubber is one of the special rubbers, which is characterized by containing CF groups on the main chain or side chain. Fluorine is the most electronegative element among all chemical elements. The CF bond is highly stable, and the bond energy is as high as 485kJ / mol, which makes fluororubber stable and exhibits excellent heat resistance, good chemical stability, corrosion resistance and atmospheric aging resistance. Therefore, fluororubber is widely used in oil extraction, oil and gas storage and transportation, automotive oil seals, aerospace and other fields as a special sealing material. However, fluororubber needs to be reinforced with fillers when used to meet the requirements of sealing materials. At present, the most widely used filler in the rubber field is carbon black, which is used to enhance the material.
[0003] CN106317712A discloses a carbon black modified fluororubber, which improves the mechanical properties and chemical stability of the fluororubber. However, when carbon black is added to the fluororubber base, it is easy to agglomerate and fall off during use. In addition, the carbon black particles are large and the reinforcement effect is limited, resulting in poor toughness and processing performance of the fluororubber.
[0004] Since nanomaterials are small in size and have a large specific surface area, they can be in close contact with the rubber in the rubber substrate, improving the mechanical properties of the rubber. Currently, silica nanoparticles, carbon nanotubes, graphene, etc. are added to the fluororubber substrate, which significantly improves the mechanical properties of the fluororubber.
[0005] CN113372667A discloses a method of adding graphene to fluororubber to prepare a fluororubber seal ring with wear resistance. The addition of graphene prolongs the service life of the rubber seal ring. However, the cost of graphene is high, and the dispersion in the fluororubber substrate is difficult to control, which restricts its modification effect, reduces the mechanical properties of the fluororubber, and increases the production cost.
[0006] In summary, there is an urgent need to develop a sealing fluororubber that has good mechanical properties, is resistant to high temperatures, can be recycled, and can effectively reduce the cost of using fluororubber. Summary of the invention
[0007] The purpose of the present invention is to overcome the problems of the prior art that fluororubber has poor mechanical properties, poor high temperature resistance and is difficult to recycle, and to provide a fluororubber system, fluororubber and a preparation method and application thereof.
[0008] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a fluororubber system, wherein, in parts by weight, the fluororubber system comprises: 100 parts by weight of fluororubber raw rubber, 0.5-40 parts by weight of magnetic nanoparticles, 1-10 parts by weight of peroxide vulcanizer, 2-20 parts by weight of vulcanization accelerator, and 1-10 parts by weight of processing aid.
[0009] A second aspect of the present invention provides a method for preparing fluororubber, wherein the method comprises the following steps:
[0010] (1) mixing the above fluororubber system to obtain a fluororubber compound;
[0011] (2) The fluororubber compound is vulcanized to obtain fluororubber.
[0012] The third aspect of the present invention provides a fluororubber prepared by the above preparation method.
[0013] The fourth aspect of the present invention provides an application of the fluororubber system described in the first aspect or the fluororubber described in the third aspect in sealing;
[0014] Preferably, the sealed working environment temperature is 180-240°C, preferably 170-200°C.
[0015] Compared with the prior art, the fluororubber system, fluororubber and preparation method and application thereof provided by the present invention achieve the following beneficial effects:
[0016] In the fluororubber system of the present invention, the magnetic nanoparticles have good dispersibility in the system and strong ability to combine with the fluororubber, so that the prepared fluororubber has high hardness, high tensile strength, high elongation at break, and 300% strain modulus, and also has high thermal conductivity; when used as a fluororubber sealing material, it can improve the heat dissipation efficiency and reduce the influence of high temperature generated by heat accumulation on the service life of the sealing material.
[0017] The fluororubber of the present invention has magnetic field response performance. Through the regulation of the external magnetic field, the target area can be sealed to achieve the purpose of selective sealing. After the fluororubber is used, it can be effectively enriched through external magnetic field control for recycling, effectively reducing the use cost of the fluororubber. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1-4 is a schematic diagram of the magnetic field response performance of the fluororubber obtained in Example 3; wherein, Figure 1 and 2 This is a picture of a magnet gradually approaching fluororubber. Figure 3 and 4 This is a picture of fluororubber material being adsorbed on the surface of a magnet. DETAILED DESCRIPTION
[0019] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0020] The first aspect of the present invention provides a fluororubber system, wherein, by weight, the fluororubber system comprises: 100 parts by weight of fluororubber raw rubber, 0.5-40 parts by weight of magnetic nanoparticles, 1-10 parts by weight of a peroxide vulcanizer, 2-20 parts by weight of a vulcanization accelerator, and 1-10 parts by weight of a processing aid.
[0021] When the present invention selects each component according to the above specific weight parts to configure the fluororubber system, the fluororubber obtained after processing has the characteristics of high hardness, high tensile strength, elongation at break, strain modulus of 300%, and excellent thermal conductivity.
[0022] In the present invention, the weight proportion of the magnetic nanoparticles may be 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 20, 25, 30, 35 and 40 parts, as well as any value in the range consisting of any two of the above values.
[0023] In some specific embodiments of the present invention, the magnetic nanoparticles are selected from at least one of Fe3O4 nanoparticles, Fe2O3 nanoparticles and nano manganese zinc ferrite. The preferred conditions are used to improve the dispersibility of the magnetic nanoparticles in the fluororubber substrate, so that the fluororubber has better mechanical properties and has the ability of selective sealing.
[0024] Furthermore, the magnetic nanoparticles are Fe3O4 nanoparticles.
[0025] In some specific embodiments of the present invention, the average particle size of the magnetic nanoparticles is 100-500 nm, preferably 200-400 nm.
[0026] In the present invention, the weight parts of the peroxide vulcanizing agent can be 1 part, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts and 10 parts, as well as any value in the range composed of any two of the above values.
[0027] In some specific embodiments of the present invention, the peroxide vulcanizing agent can be an existing peroxide vulcanizing agent that can be used for the vulcanization of fluororubber raw rubber, preferably selected from diisopropylbenzene peroxide, 1,3-bis(tert-butylperoxyisopropyl)benzene, and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane. The use of a preferred peroxide vulcanizing machine can enhance the heat resistance of fluororubber.
[0028] In the present invention, the weight parts of the vulcanization accelerator can be 2 parts, 3 parts, 4 parts, 5 parts, 5.5 parts, 6 parts, 6.5 parts, 7 parts, 7.5 parts, 8 parts, 8.5 parts, 9 parts, 9.5 parts, 10 parts, 12 parts, 14 parts, 16 parts, 18 parts and 20 parts, as well as any value in the range composed of any two of the above values.
[0029] In some specific embodiments of the present invention, the vulcanization accelerator may be an existing vulcanization accelerator that can be used for the vulcanization of fluororubber raw rubber, preferably selected from triallyl isocyanurate and / or triallyl cyanurate.
[0030] In some specific embodiments of the present invention, the fluororubber raw rubber is selected from fluorine-containing olefin rubber.
[0031] Furthermore, the fluororubber raw rubber is selected from tetrafluoroethylene-propylene copolymer or vinylidene fluoride-hexafluoropropylene copolymer. In the present invention, the use of the preferred fluororubber raw rubber is beneficial to improving the high temperature resistance and acid and alkali corrosion resistance of the fluororubber.
[0032] In some specific embodiments of the present invention, the Mooney viscosity ML (1+10, 100° C.) of the fluororubber raw rubber is 35-160.
[0033] In some specific embodiments of the present invention, the processing aid is selected from at least one of calcium stearate, magnesium oxide, and zinc oxide; preferably calcium stearate and magnesium oxide; preferably, the weight ratio of calcium stearate to magnesium oxide is 1:1-4.
[0034] In some preferred embodiments of the present invention, the fluororubber system comprises, by weight: 100 parts by weight of fluororubber raw rubber, 1-30 parts by weight of magnetic nanoparticles, 1-5 parts by weight of peroxide vulcanizer, 5-10 parts by weight of vulcanization accelerator, and 1-5 parts by weight of processing aid.
[0035] A second aspect of the present invention provides a method for preparing fluororubber, the method comprising the following steps:
[0036] (1) mixing the above fluororubber system to obtain a fluororubber compound;
[0037] (2) The fluororubber compound is vulcanized to obtain fluororubber.
[0038] In the present invention, the fluororubber prepared according to the preparation method has good hardness and mechanical properties, namely tensile strength, elongation at break and strain modulus of 300%, and also has good thermal conductivity.
[0039] In the present invention, in step (1), the fluororubber raw rubber is put into an open mill for plasticizing to obtain plasticized rubber, which is then mixed with magnetic nanoparticles, a peroxide vulcanizer, a vulcanization accelerator and a processing aid to obtain a fluororubber compound.
[0040] In some specific embodiments of the present invention, in step (2), the vulcanization process includes: one-stage vulcanization and two-stage vulcanization.
[0041] In some specific embodiments of the present invention, the temperature of the first stage vulcanization is 150° C.-190° C., and the time is 20-40 minutes.
[0042] In some specific embodiments of the present invention, the temperature of the second stage vulcanization is 200° C.-210° C., and the time is 240-480 min.
[0043] The third aspect of the present invention provides a fluororubber prepared by the above preparation method.
[0044] In some specific embodiments of the present invention, the hardness of the fluororubber is greater than or equal to 50HA, preferably 60-80HA; preferably, the tensile strength of the fluororubber is greater than or equal to 10MPa, preferably greater than or equal to 12MPa; preferably, the elongation at break of the fluororubber is greater than or equal to 650%, preferably greater than or equal to 800%; preferably, the maximum decomposition temperature of the fluororubber is 470-520°C, preferably 490-500°C; the thermal conductivity of the fluororubber is greater than or equal to 0.27W·m -1 ·K -1 , preferably greater than or equal to 0.29W·m -1 ·K -1 .
[0045] A fourth aspect of the present invention provides an application of the fluororubber system described in the first aspect or the fluororubber described in the third aspect in sealing.
[0046] The fluororubber of the present invention has good mechanical properties, namely, good hardness and toughness, and exhibits good stability in a high temperature and high pressure environment. The fluororubber can be used in a working environment of 180-240°C, more preferably 170-200°C.
[0047] The present invention will be described in detail below by way of examples. In the following examples, the fluororubber raw material is Asahi Glass Co., Ltd. 100S (tetrafluoroethylene-propylene copolymer, Mooney viscosity ML (1+10, 100° C.) is 160) is a commercially available product.
[0048] The hardness of fluororubber is measured according to GB / T 531.1-2008.
[0049] The tensile strength, elongation at break and strain 300% modulus of fluororubber are measured in accordance with GB / T 528-2009.
[0050] The maximum decomposition temperature of fluororubber was measured by thermogravimetric analyzer. The test temperature range was from room temperature to 600°C, and the heating rate was 10°C / min.
[0051] The thermal conductivity of fluororubber is tested according to the steady-state heat flow method in ASTM D5470-2017.
[0052] Example 1
[0053] (1) 100 parts by weight of fluororubber raw rubber ( 100S) is put into an open mill for plastication to obtain plasticized rubber;
[0054] (2) The plasticized rubber is put into an open mill for reverse refining, and 1 part of magnetic nanoparticles (Fe3O4 nanoparticles, average particle size of 300 nm), 1 part of vulcanizing agent (diisopropylbenzene peroxide), 5 parts of vulcanization accelerator (triallyl isocyanurate), 1 part of magnesium oxide, and 1 part of calcium stearate are added by weight; after mixing, the rubber is cut left and right, thinned, triangularly packaged, and rolled to obtain a fluororubber mixed rubber, which is then cut into sheets for later use;
[0055] (3) The fluororubber compound is subjected to a first-stage vulcanization at 170° C. for 20 min, and then subjected to a second-stage vulcanization at a high temperature of 200° C. for 240 min, to obtain a high-temperature resistant sealing fluororubber modified with magnetic nanoparticles.
[0056] Example 2
[0057] The method of Example 1 is followed, except that the fluororubber is prepared according to the formula in Table 1.
[0058] Example 3
[0059] The method of Example 1 is followed, except that the fluororubber is prepared according to the formula in Table 1.
[0060] Example 4
[0061] The method of Example 1 is followed, except that the fluororubber is prepared according to the formula in Table 1.
[0062] Example 5
[0063] The method of Example 1 is followed, except that the fluororubber is prepared according to the formula in Table 1.
[0064] Comparative Example 1
[0065] The fluororubber was prepared according to the method of Example 1, except that no magnetic nanoparticles were added. The specific formula is shown in Table 1.
[0066] Comparative Example 2
[0067] The fluororubber was prepared according to the method of Example 1, except that the filler was carbon black of grade N990. The specific formula is shown in Table 1.
[0068] Table 1
[0069]
[0070]
[0071] Test Case
[0072] The mechanical properties of the fluororubbers prepared in the above Examples 1-5 and Comparative Examples 1-2 were tested using a Shore durometer and a universal tensile testing machine to test the mechanical properties of the magnetic nanoparticle-modified high-temperature resistant sealing rubbers. The thermal conductivity of the magnetic nanoparticle-modified high-temperature resistant sealing rubbers was tested using a rubber and plastic thermal conductivity meter. The test results are shown in Table 2.
[0073] The magnetic field response performance of the fluororubber prepared in Example 3 under an external magnetic field was tested using a magnet. The test results are shown in FIG. Figure 1-4 shown.
[0074] Table 2
[0075]
[0076]
[0077] From the results in Table 2, it can be seen that compared with the comparative example, the fluororubber obtained by the technical solution of the present invention has significantly better effects in hardness, tensile stress, elongation at break, thermal conductivity and magnetism control. Figure 1-4 As can be seen from the continuous photos, when the magnet is close to the material prepared in Example 3 ( Figure 1-2 ), can be adsorbed on the surface of the magnet by the magnet, and the adsorption magnetic force is much greater than the material gravity ( Figure 3-4 ), indicating that the fluororubber material of the present invention can quickly generate a magnetic response under the control of an external magnetic field and be firmly attracted by a magnet, so that the fluororubber material can be moved to a designated area for fixed-point sealing under the control of an external magnetic field. Furthermore, the present invention provides a basis for the magnetically controlled installation, recovery and transportation of fluororubber devices.
[0078] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A fluororubber system, characterized in that: In parts by weight, the fluororubber system comprises: 100 parts by weight of fluororubber raw rubber, 0.5-40 parts by weight of magnetic nanoparticles, 1-10 parts by weight of peroxide vulcanizer, 2-20 parts by weight of vulcanization accelerator, and 1-10 parts by weight of processing aid.
2. The fluororubber system according to claim 1, wherein: In parts by weight, the fluororubber system comprises: 100 parts by weight of fluororubber raw rubber, 1-30 parts by weight of magnetic nanoparticles, 1-5 parts by weight of peroxide vulcanizer, 5-10 parts by weight of vulcanization accelerator, and 1-5 parts by weight of processing aid.
3. The fluororubber system according to claim 1 or 2, wherein: The fluororubber raw rubber is selected from fluorine-containing olefin rubber, preferably tetrafluoroethylene-propylene copolymer or vinylidene fluoride-hexafluoropropylene copolymer; Preferably, the Mooney viscosity ML (1+10, 100° C.) of the fluororubber raw rubber is 35-160.
4. The fluororubber system according to any one of claims 1 to 3, wherein: The magnetic nanoparticles are selected from at least one of Fe3O4 nanoparticles, Fe2O3 nanoparticles and nano manganese-zinc ferrite, preferably Fe3O4 nanoparticles; Preferably, the average particle size of the magnetic nanoparticles is 100-500 nm, preferably 200-400 nm.
5. The fluororubber system according to any one of claims 1 to 4, wherein: The peroxide curing agent is selected from one of diisopropylbenzene peroxide, 1,3-bis(tert-butylperoxyisopropyl)benzene, and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane; Preferably, the vulcanization accelerator is selected from triallyl isocyanurate and / or triallyl cyanurate; Preferably, the processing aid is selected from at least one of calcium stearate, magnesium oxide, and zinc oxide; preferably calcium stearate and magnesium oxide; Preferably, the weight ratio of calcium stearate to magnesium oxide is 1:1-4.
6. A method for preparing fluororubber, characterized in that: The method comprises the following steps: (1) mixing the fluororubber system according to any one of claims 1 to 5 to obtain a fluororubber compound; (2) The fluororubber compound is vulcanized to obtain fluororubber.
7. The method according to claim 6, in step (2), the vulcanization process comprises: One stage vulcanization and two stage vulcanization; Preferably, the temperature of the first stage vulcanization is 150°C-190°C, and the time is 20-40 minutes; Preferably, the temperature of the second stage vulcanization is 200° C.-210° C., and the time is 240-480 min.
8. A fluororubber obtained by the preparation method according to claim 6 or 7.
9. The fluororubber according to claim 6, characterized in that: The tensile strength of the fluororubber is greater than or equal to 10 MPa, preferably greater than or equal to 12 MPa; Preferably, the elongation at break of the fluororubber is greater than or equal to 650%, preferably greater than or equal to 800%; Preferably, the strain 300% modulus of the fluororubber is greater than or equal to 3 MPa, preferably greater than or equal to 4 MPa; Preferably, the maximum decomposition temperature of the fluororubber is 470-520°C, preferably 490-500°C; Preferably, the thermal conductivity of the fluororubber is greater than or equal to 0.27 W·m -1 ·K -1 , preferably greater than or equal to 0.29W·m -1 ·K -1 .
10. Use of the fluororubber system according to any one of claims 1 to 5 or the fluororubber according to claim 8 or 9 in sealing; Preferably, the sealed working environment temperature is 180-240°C, preferably 170-200°C.
Citation Information
Patent Citations
Rubber compound containing nanoscale, magnetic fillers
CN101044197A
High-temperature-resistant rubber gasket for automobile shock absorbers
CN105482185A
Preparing method of fluororubber / nanofiller composite material
CN106432991A
A fluororubber material used for sealing members resistant to high temperatures and high pressure and a preparing method thereof
CN106633544A
Preparation and process flow of a cochlea-shaped bulletproof, wave-absorbing and high-temperature-resistant material