Heat-conducting nylon 6 composite material with hybrid structure network

Through the melt blending of modified thermally conductive filler GO-EDA/CF@PDA-Al2O3 and nylon 6 resin, a three-dimensional hybrid structure is constructed, which solves the problem of insufficient thermal conductivity of nylon 6 composite materials and achieves efficient thermal conductivity and improved mechanical properties. At the same time, the cost is reduced.

CN118725555APending Publication Date: 2024-10-01FUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410924750.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The thermal conductivity of nylon 6 composite materials is low, making it difficult to meet the heat dissipation requirements of practical applications, and the traditional filled particle composite method results in high cost, heavy weight, and poor processability.

Method used

The modified thermally conductive filler GO-EDA/CF@PDA-Al2O3 is covalently connected through solvothermal reaction to form a three-dimensional hybrid structure and melt-blended with nylon 6 resin to reduce the interface thermal resistance between the filler and the matrix and construct a multi-level thermal conduction pathway.

Benefits of technology

It achieves significant improvement in thermal conductivity and mechanical properties at lower doping levels, reduces the scattering effect of phonons, improves the thermal conductivity and mechanical properties of composite materials, and reduces costs at the same time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004937786880000011
    Figure HDA0004937786880000011
  • Figure HDA0004937786880000012
    Figure HDA0004937786880000012
  • Figure HDA0004937786880000021
    Figure HDA0004937786880000021
Patent Text Reader

Abstract

The invention discloses a heat-conducting nylon 6 composite material with a hybrid structure network and a preparation method of the heat-conducting nylon 6 composite material, and belongs to the field of polymer composite materials. The heat-conducting nylon 6 composite material is prepared from the following raw materials in parts by weight: 5-15 parts of modified heat-conducting filler (GO-EDA / CF (at) PDA-Al2O3) and 85-95 parts of nylon 6 particles. The modified heat-conducting filler is a three-dimensional hybrid structure material formed by connecting three heat-conducting fillers with different dimensions through a chemical reaction, namely GO-EDA / CF (at) PDA-Al2O3. The three heat-conducting fillers with different shapes are connected together through covalent interaction, so that not only is the compatibility of the fillers and nylon 6 improved, but also the interface thermal resistance between the materials is reduced. GO-EDA / CF (at) PDA-Al2O3 and nylon 6 are subjected to melt blending, extrusion granulation and compression molding to prepare the heat-conducting nylon 6 composite material, and the heat-conducting nylon 6 composite material has excellent mechanical property, heat stability and heat-conducting property and is wide in application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer composite materials, and in particular relates to a thermally conductive nylon 6 composite material with a hybrid structure network and a preparation method thereof. Background Art

[0002] With the development of advanced technology, electronic devices are developing towards miniaturization and integration while their performance is constantly improving. The accumulation of heat during operation will reduce the stability and service life of electronic devices. Therefore, thermal management has become a key issue. In recent years, polymer-based thermal interface materials (TIMs) have received widespread attention in thermal management systems due to their superior comprehensive performance. Nylon 6 composites have been widely used in the packaging field due to their good performance and low cost. However, the thermal conductivity of nylon 6 itself is very low (<0.5 W m -1 k -1 ), which is not enough to meet the heat dissipation requirements of practical applications.

[0003] In order to improve the low thermal conductivity of polymers caused by the disordered arrangement of molecular chains and to increase their thermal conductivity coefficient. In the past few decades, a lot of research has been devoted to the preparation of thermally conductive polymer composites by compounding with dispersed filler particles. However, in practical applications, due to the poor compatibility of thermally conductive fillers with the matrix, high filling amounts are often required to achieve high thermal conductivity, resulting in higher costs, heavier weight and poorer processability. By optimizing the surface properties of the filler, the interfacial thermal resistance between the filler and the matrix can be improved, thereby improving the thermal conductivity of the polymer composite. This method effectively reduces the thermal resistance at the interface, allowing heat to be transferred more efficiently in the composite material.

[0004] In recent years, due to the existence of a considerable number of contact interfaces between single dispersed fillers and polymer matrices and the fact that large loads seriously reduce the performance of polymers, these unfavorable factors have limited the potential of thermally conductive fillers in enhancing the thermal conduction of polymers, making it difficult to fully play their role. In order to maximize the use of the excellent thermal conductivity of thermally conductive fillers, people are paying more and more attention to the construction of thermal conductive networks, and have conducted very in-depth research on hybrid fillers with different aspect ratios, sizes and contents. One-dimensional (1D) and two-dimensional (2D) fillers bridge the non-contacting particle fillers (0D) and provide long-distance heat transfer channels; similarly, particle fillers (0D) provide short-distance heat transfer and more contact possibilities; and give fillers a three-dimensional (3D) structure in the composite material. On the one hand, multiple heat conduction pathways can be established to form an efficient heat conduction network to improve the thermal conductivity; on the other hand, the fillers can be evenly distributed in the matrix; thereby improving the mechanical properties of the composite material. Both can effectively reduce the negative impact of the interfacial thermal resistance between fillers and fillers. At the same time, with the help of this multi-dimensional 3D structure, only a relatively small amount of doping is needed to maximize the improvement of thermal conductivity. The 3D skeleton network provides abundant paths and interface contact points for phonon transfer, which helps to reduce the scattering effect of phonons at the interface. Therefore, constructing a continuous 3D structure as a heat conduction channel to achieve efficient heat conduction in the polymer matrix has become an important strategy for preparing high thermal conductivity polymer composites and has gradually become a hot trend in current research.

[0005] The present invention prepares a thermally conductive nylon 6 composite material by melt blending a modified thermally conductive filler and a nylon 6 resin. The thermally conductive filler is a three-dimensional hybrid structure material formed by connecting three thermally conductive fillers of different dimensions through chemical reaction, namely GO-EDA / CF@PDA-Al2O3. They are covalently connected through solvent thermal reaction and melt blended into a nylon 6 matrix. The ortho-amine effectively establishes a covalent interaction between the oxygen-containing functional groups of GO-EDA and CF@PDA-Al2O3, reduces the interfacial thermal resistance between the filler and nylon 6, and promotes phonon transfer on the interface. At the same time, the filler modified by covalent action does not introduce any defects or voids, thereby ensuring the thermal conductivity efficiency of the modified thermally conductive filler. The three-dimensional interconnected thermally conductive network can more effectively improve the thermal conductivity of the polymer than dispersed fillers because they have an inherent continuous structure. The strong interconnection between the fillers can reduce the scattering of phonons and construct a multi-level heat conduction path. This special effect can further improve the thermal conductivity and mechanical properties of the composite material. Summary of the invention

[0006] The object of the present invention is to provide a heat-conducting nylon 6 composite material with a hybrid structure network and a preparation method thereof, which has good thermal conductivity and mechanical properties.

[0007] To achieve the above object, the present invention adopts the following technical solution: A heat-conducting nylon 6 composite material with a hybrid structure network comprises raw materials by weight: 5-15 parts of modified heat-conducting filler and 85-95 parts of nylon 6 particles.

[0008] Wherein, the preparation of the modified thermal conductive filler comprises the following steps: (1) GO was prepared using natural flake graphite as raw material by the improved Hummers method. 1.5 g of natural flake graphite, 1 g of NaNO3 and 100 mL of concentrated H2SO4 were added to a 500 mL round-bottom flask. The flask was placed in an ice-water bath to keep the temperature of the mixture below 10°C. While stirring, 5 g of KMnO4 was slowly added to the reaction mixture in five portions. Heat to 35°C, stir for 24 h, then slowly add 150 mL of deionized water, heat to 90°C, and continue stirring for about 4 h. Subsequently, 100 mL of deionized water and 5 mL of H2O2 aqueous solution were added, and stirred for another 1 h. After filtering the resulting mixture, it was washed several times with a dilute HCl solution until sulfate ions could no longer be detected in BaCl2. Finally, the sample was freeze-dried. GO was obtained; (2) Add 100 mg of GO prepared in step (1) and 100 mL of deionized water into a 250 mL round-bottom flask and disperse by ultrasonication for 1 h. Then add 100 mg of ethylenediamine and 200 mg of N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride into the flask and mix. Stir at 80 °C for 24 h, and wash the resulting mixture with ethanol and deionized water several times to remove all residues and by-products. Finally, dry the sample in vacuum at 80 °C for 24 h. Obtain GO-EDA; (3) Add 2 g of aluminum oxide to 200 mL of tris(hydroxymethyl)aminomethane solution (10 mM) and stir and ultrasonicate for 1 h. Then add 500 mg of o-phenylenediamine and stir and ultrasonicate for 30 min. Stir the mixture at 60 °C for 6 h. Next, filter the product and wash it with ethanol and deionized water several times. Finally, dry it in vacuum at 80 °C for 24 h. Obtain covalently functionalized Al2O3; (4) Place the carbon fiber in an ethanol-water solution and ultrasonically treat it for 1 h to remove the desizing agent on the surface. Then add 2 g of carbon fiber and 1 g of dopamine hydrochloride to 250 mL of Tris buffer (pH = 8.5) and 150 mL of ethanol, mix, and ultrasonicate for 45 min. Then soak at room temperature for 24 h, and then add the covalently functionalized Al2O3 prepared in step (3) to the suspension and ultrasonicate for 1 h. Then filter and clean the deposited mixed solution, and anneal it in an oven at 200 ° C to finally obtain CF@PDA-Al2O3; (5) 100 mg of GO-EDA prepared in step (2) was placed in a double-necked round-bottom flask and placed on a magnetic stirrer. Then 2 g of ultrasonically treated CF@PDA-Al2O3 and 100 mL of N,N-dimethylformamide were added. Stir at 80°C for 8 h. After stirring, the mixed solution was transferred to a polytetrafluoroethylene-lined autoclave container and subjected to a solvothermal reaction at 200°C for 6 h. After the reaction, the mixture was filtered without washing to retain some unreacted amines on the surface of the material, which facilitated hydrogen bonding between the polymer chain and the filler surface. Finally, the mixture was vacuum dried at 80°C for 24 h. Finally, the modified thermal conductive filler GO-EDA / CF@PDA-Al2O3 was obtained.

[0009] The preparation of the high thermal conductivity nylon 6 composite material comprises the following steps: (1) GO-EDA / CF@PDA-Al2O3 and nylon 6 resin were mixed evenly, the mixture was dried at 80 °C for 24 h, and then extruded into pellets by a twin-screw extruder; (2) The mixed particles prepared in step (1) are first hot-pressed and melted in a flat vulcanizer and then cold-pressed to form a thermally conductive nylon 6 composite material.

[0010] Furthermore, the temperatures in each zone in the extrusion granulation are 215°C / 220°C / 225°C / 225°C / 230°C / 230°C / 235°C, and the screw speed is set to 30 r / min; the hot pressing temperature is 230°C, the hot pressing time is 10 min, the cold pressing temperature is room temperature, the cold pressing time is 10 min, and the pressure is 10 MPa, finally obtaining a thermally conductive nylon 6 composite material.

[0011] The beneficial effects of the present invention are: (1) The present invention uses a 3D hybrid structure material formed by the covalent reaction of zero-dimensional 0D filler spherical nano-alumina, 1D thermal conductive filler fibrous carbon fiber and 2D thermal conductive filler lamellar graphene oxide as a thermal conductive filler. Doping hybrid fillers in polymers is an effective way to achieve high-performance composite materials. The synergistic effect between thermal conductive fillers of different shapes can achieve a significant increase in the thermal conductivity of the composite material.

[0012] (2) The three-dimensional hybrid filler GO-EDA / CF@PDA-Al2O3 prepared by the present invention improves the interfacial compatibility with the nylon 6 matrix resin, so that the thermal conductive filler can be evenly dispersed inside the composite material. On the one hand, it improves the mechanical properties of the composite material, and on the other hand, it reduces the interfacial thermal resistance between the filler and the matrix, thereby improving the thermal conductivity of the composite material.

[0013] (3) The three-dimensional hybrid filler GO-EDA / CF@PDA-Al2O3 prepared by the present invention can achieve high thermal conductivity of the composite material at a lower doping amount. This is due to the three-dimensional thermal conductive network built by the hybrid filler inside the composite material, which reduces the scattering of phonons and constructs a multi-level heat conduction path, thereby greatly improving the thermal conductivity of the nylon 6 composite material. While ensuring thermal conductivity, it reduces costs and improves the mechanical properties of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a Fourier infrared image of the modified thermal conductive filler prepared in the present invention.

[0015] Figure 2 This is a scanning electron microscope image of the carbon fiber used in the present invention.

[0016] Figure 3 This is a scanning electron microscope image of the thermally conductive nylon 6 composite material prepared in Example 1 of the present invention.

[0017] Figure 4 This is a scanning electron microscope image of the thermally conductive nylon 6 composite material prepared in Example 3 of the present invention.

[0018] Figure 5 This is a scanning electron microscope image of the sample prepared in Comparative Example 1 of the present invention.

[0019] Figure 6 This is a scanning electron microscope image of the cross-section of the distribution of carbon fibers in the nylon 6 matrix.

[0020] Figure 7 This is a scanning electron microscope image of the thermally conductive nylon 6 composite material prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0021] In order to make the contents of the present invention easier to understand, the technical solution of the present invention is further described below in conjunction with specific implementation methods, but the present invention is not limited thereto.

[0022] The preparation of a modified thermally conductive filler comprises the following steps: (1) GO was prepared using natural flake graphite as raw material by the improved Hummers method. 1.5 g of natural flake graphite, 1 g of NaNO3 and 100 mL of concentrated H2SO4 were added to a 500 mL round-bottom flask. The flask was placed in an ice-water bath to keep the temperature of the mixture below 10°C. While stirring, 5 g of KMnO4 was slowly added to the reaction mixture in five portions. Heat to 35°C, stir for 24 h, then slowly add 150 mL of deionized water, heat to 90°C, and continue stirring for about 4 h. Subsequently, 100 mL of deionized water and 5 mL of H2O2 aqueous solution were added, and stirred for another 1 h. After filtering the resulting mixture, it was washed several times with a dilute HCl solution until sulfate ions could no longer be detected in BaCl2. Finally, the sample was freeze-dried. GO was obtained; (2) Add 100 mg of GO prepared in step (1) and 100 mL of deionized water into a 250 mL round-bottom flask and disperse by ultrasonication for 1 h. Then add 100 mg of ethylenediamine and 200 mg of N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride into the flask and mix. Stir at 80 °C for 24 h, and wash the resulting mixture with ethanol and deionized water several times to remove all residues and by-products. Finally, dry the sample in vacuum at 80 °C for 24 h. Obtain GO-EDA; (3) Add 2 g of aluminum oxide to 200 mL of tris(hydroxymethyl)aminomethane solution (10 mM) and stir and ultrasonicate for 1 h. Then add 500 mg of o-phenylenediamine and stir and ultrasonicate for 30 min. Stir the mixture at 60 °C for 6 h. Next, filter the product and wash it with ethanol and deionized water several times. Finally, dry it in vacuum at 80 °C for 24 h. Obtain covalently functionalized Al2O3; (4) Place the carbon fiber in an ethanol-water solution and ultrasonically treat it for 1 h to remove the desizing agent on the surface. Then add 2 g of carbon fiber and 1 g of dopamine hydrochloride to 250 mL of Tris buffer (pH = 8.5) and 150 mL of ethanol, mix, and ultrasonicate for 45 min. Then soak at room temperature for 24 h, and then add the covalently functionalized Al2O3 prepared in step (3) to the suspension and ultrasonicate for 1 h. Then filter and clean the deposited mixed solution, and anneal it in an oven at 200 ° C to finally obtain CF@PDA-Al2O3; (5) 100 mg of GO-EDA prepared in step (2) was placed in a double-necked round-bottom flask and placed on a magnetic stirrer. Then 2 g of ultrasonically treated CF@PDA-Al2O3 and 100 mL of N,N-dimethylformamide were added. Stir at 80°C for 8 h. After stirring, the mixed solution was transferred to a polytetrafluoroethylene-lined autoclave container and subjected to a solvothermal reaction at 200°C for 6 h. After the reaction, the mixture was filtered without washing to retain some unreacted amines on the surface of the material, which facilitated hydrogen bonding between the polymer chain and the filler surface. Finally, the mixture was vacuum dried at 80°C for 24 h. Finally, the modified thermal conductive filler GO-EDA / CF@PDA-Al2O3 was obtained.

[0023] Figure 1 This is the Fourier infrared image of the modified thermal conductive filler prepared by the present invention. -1 A broad absorption peak nearby is the stretching vibration peak of Al2O3, 1349 cm -1 The peak of Al-O vibration absorption, 1635 cm -1 A prominent peak can be found, which corresponds to the -NH2 absorption peak of covalently modified Al2O3. -1 A new peak appeared, corresponding to the stretching vibration peak of GO, indicating that GO-EDA and CF@PDA-Al2O3 reacted to successfully prepare GO-EDA / CF@PDA-Al2O3KH560.

[0024] Figure 2 This is a scanning electron microscope image of the carbon fiber used in the present invention. It can be seen that the CF surface is very smooth and has no other impurities.

[0025] Example 1 1) 5 parts by weight of GO-EDA / CF@PDA-Al2O3 and 95 parts by weight of nylon 6 resin were melt-blended and extruded into granules in a twin-screw extruder. The temperatures of each zone in the extrusion granulation were 215℃ / 220℃ / 225℃ / 225℃ / 230℃ / 230℃ / 235℃, respectively, and the screw speed was 30 r / min. 2) The mixed particles were hot-pressed and then cold-pressed in a flat vulcanizer. The hot-pressing temperature was 230°C, the hot-pressing time was 10 min, the cold-pressing temperature was room temperature, the cold-pressing time was 10 min, and the pressure was 10 MPa, and finally a thermally conductive nylon 6 composite material was obtained.

[0026] The preparation steps of GO-EDA / CF@PDA-Al2O3 are as follows: (1) GO was prepared using natural flake graphite as raw material by the improved Hummers method. 1.5 g of natural flake graphite, 1 g of NaNO3 and 100 mL of concentrated H2SO4 were added to a 500 mL round-bottom flask. The flask was placed in an ice-water bath to keep the temperature of the mixture below 10°C. While stirring, 5 g of KMnO4 was slowly added to the reaction mixture in five portions. Heat to 35°C, stir for 24 h, then slowly add 150 mL of deionized water, heat to 90°C, and continue stirring for about 4 h. Subsequently, 100 mL of deionized water and 5 mL of H2O2 aqueous solution were added, and stirred for another 1 h. After filtering the resulting mixture, it was washed several times with a dilute HCl solution until sulfate ions could no longer be detected in BaCl2. Finally, the sample was freeze-dried. GO was obtained; (2) Add 100 mg of GO prepared in step (1) and 100 mL of deionized water into a 250 mL round-bottom flask and disperse by ultrasonication for 1 h. Then add 100 mg of ethylenediamine and 200 mg of N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride into the flask and mix. Stir at 80 °C for 24 h, and wash the resulting mixture with ethanol and deionized water several times to remove all residues and by-products. Finally, dry the sample in vacuum at 80 °C for 24 h. Obtain GO-EDA; (3) Add 2 g of aluminum oxide to 200 mL of tris(hydroxymethyl)aminomethane solution (10 mM) and stir and ultrasonicate for 1 h. Then add 500 mg of o-phenylenediamine and stir and ultrasonicate for 30 min. Stir the mixture at 60 °C for 6 h. Next, filter the product and wash it with ethanol and deionized water several times. Finally, dry it in vacuum at 80 °C for 24 h. Obtain covalently functionalized Al2O3; (4) Place the carbon fiber in an ethanol-water solution and ultrasonically treat it for 1 h to remove the desizing agent on the surface. Then add 2 g of carbon fiber and 1 g of dopamine hydrochloride to 250 mL of Tris buffer (pH = 8.5) and 150 mL of ethanol, mix, and ultrasonicate for 45 min. Then soak at room temperature for 24 h, and then add the covalently functionalized Al2O3 prepared in step (3) to the suspension and ultrasonicate for 1 h. Then filter and clean the deposited mixed solution, and anneal it in an oven at 200 ° C to finally obtain CF@PDA-Al2O3; (5) 100 mg of GO-EDA prepared in step (2) was placed in a double-necked round-bottom flask and placed on a magnetic stirrer. Then 2 g of ultrasonically treated CF@PDA-Al2O3 and 100 mL of N,N-dimethylformamide were added. Stir at 80°C for 8 h. After stirring, the mixed solution was transferred to a polytetrafluoroethylene-lined autoclave container and subjected to a solvothermal reaction at 200°C for 6 h. After the reaction, the mixture was filtered without washing to retain some unreacted amines on the surface of the material, which facilitated hydrogen bonding between the polymer chain and the filler surface. Finally, the mixture was vacuum dried at 80°C for 24 h. Finally, the modified thermal conductive filler GO-EDA / CF@PDA-Al2O3 was obtained.

[0027] Figure 3 This is a scanning electron microscope image of the thermally conductive nylon 6 composite material prepared in Example 1 of the present invention. It can be seen that GO-EDA / CF@PDA-Al2O3KH560 not only has a large amount of alumina attached to it, but also has pieces of GO. The three materials are connected together by chemical bonds to form a three-dimensional hybrid thermal conductive structure, thereby improving the thermal conductivity of the composite material.

[0028] Example 2 1) 10 parts by weight of GO-EDA / CF@PDA-Al2O3 and 90 parts by weight of nylon 6 resin were melt-blended and extruded into granules in a twin-screw extruder. The temperatures of each zone in the extrusion granulation were 215℃ / 220℃ / 225℃ / 225℃ / 230℃ / 230℃ / 235℃, respectively, and the screw speed was 30 r / min. 2) The mixed particles were hot-pressed and then cold-pressed in a flat vulcanizer. The hot-pressing temperature was 230°C, the hot-pressing time was 10 min, the cold-pressing temperature was room temperature, the cold-pressing time was 10 min, and the pressure was 10 MPa, and finally a thermally conductive nylon 6 composite material was obtained.

[0029] The preparation steps of GO-EDA / CF@PDA-Al2O3 are as follows: (1) GO was prepared using natural flake graphite as raw material by the improved Hummers method. 1.5 g of natural flake graphite, 1 g of NaNO3 and 100 mL of concentrated H2SO4 were added to a 500 mL round-bottom flask. The flask was placed in an ice-water bath to keep the temperature of the mixture below 10°C. While stirring, 5 g of KMnO4 was slowly added to the reaction mixture in five portions. Heat to 35°C, stir for 24 h, then slowly add 150 mL of deionized water, heat to 90°C, and continue stirring for about 4 h. Subsequently, 100 mL of deionized water and 5 mL of H2O2 aqueous solution were added, and stirred for another 1 h. After filtering the resulting mixture, it was washed several times with a dilute HCl solution until sulfate ions could no longer be detected in BaCl2. Finally, the sample was freeze-dried. GO was obtained; (2) Add 100 mg of GO prepared in step (1) and 100 mL of deionized water into a 250 mL round-bottom flask and disperse by ultrasonication for 1 h. Then add 100 mg of ethylenediamine and 200 mg of N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride into the flask and mix. Stir at 80 °C for 24 h, and wash the resulting mixture with ethanol and deionized water several times to remove all residues and by-products. Finally, dry the sample in vacuum at 80 °C for 24 h. Obtain GO-EDA; (3) Add 2 g of aluminum oxide to 200 mL of tris(hydroxymethyl)aminomethane solution (10 mM) and stir and ultrasonicate for 1 h. Then add 500 mg of o-phenylenediamine and stir and ultrasonicate for 30 min. Stir the mixture at 60 °C for 6 h. Next, filter the product and wash it with ethanol and deionized water several times. Finally, dry it in vacuum at 80 °C for 24 h. Obtain covalently functionalized Al2O3; (4) Place the carbon fiber in an ethanol-water solution and ultrasonically treat it for 1 h to remove the desizing agent on the surface. Then add 2 g of carbon fiber and 1 g of dopamine hydrochloride to 250 mL of Tris buffer (pH = 8.5) and 150 mL of ethanol, mix, and ultrasonicate for 45 min. Then soak at room temperature for 24 h, and then add the covalently functionalized Al2O3 prepared in step (3) to the suspension and ultrasonicate for 1 h. Then filter and clean the deposited mixed solution, and anneal it in an oven at 200 ° C to finally obtain CF@PDA-Al2O3; (5) 100 mg of GO-EDA prepared in step (2) was placed in a double-necked round-bottom flask and placed on a magnetic stirrer. Then 2 g of ultrasonically treated CF@PDA-Al2O3 and 100 mL of N,N-dimethylformamide were added. Stir at 80°C for 8 h. After stirring, the mixed solution was transferred to a polytetrafluoroethylene-lined autoclave container and subjected to a solvothermal reaction at 200°C for 6 h. After the reaction, the mixture was filtered without washing to retain some unreacted amines on the surface of the material, which facilitated hydrogen bonding between the polymer chain and the filler surface. Finally, the mixture was vacuum dried at 80°C for 24 h. Finally, the modified thermal conductive filler GO-EDA / CF@PDA-Al2O3 was obtained.

[0030] Example 3 1) 15 parts by weight of GO-EDA / CF@PDA-Al2O3 and 85 parts by weight of nylon 6 resin were melt-blended and extruded into granules in a twin-screw extruder. The temperatures of each zone in the extrusion granulation were 215℃ / 220℃ / 225℃ / 225℃ / 230℃ / 230℃ / 235℃, respectively, and the screw speed was 30 r / min. 2) The mixed particles were hot-pressed and then cold-pressed in a flat vulcanizer. The hot-pressing temperature was 230°C, the hot-pressing time was 10 min, the cold-pressing temperature was room temperature, the cold-pressing time was 10 min, and the pressure was 10 MPa, and finally a thermally conductive nylon 6 composite material was obtained.

[0031] The preparation steps of GO-EDA / CF@PDA-Al2O3 are as follows: (1) GO was prepared using natural flake graphite as raw material by the improved Hummers method. 1.5 g of natural flake graphite, 1 g of NaNO3 and 100 mL of concentrated H2SO4 were added to a 500 mL round-bottom flask. The flask was placed in an ice-water bath to keep the temperature of the mixture below 10°C. While stirring, 5 g of KMnO4 was slowly added to the reaction mixture in five portions. Heat to 35°C, stir for 24 h, then slowly add 150 mL of deionized water, heat to 90°C, and continue stirring for about 4 h. Subsequently, 100 mL of deionized water and 5 mL of H2O2 aqueous solution were added, and stirred for another 1 h. After filtering the resulting mixture, it was washed several times with a dilute HCl solution until sulfate ions could no longer be detected in BaCl2. Finally, the sample was freeze-dried. GO was obtained; (2) Add 100 mg of GO prepared in step (1) and 100 mL of deionized water into a 250 mL round-bottom flask and disperse by ultrasonication for 1 h. Then add 100 mg of ethylenediamine and 200 mg of N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride into the flask and mix. Stir at 80 °C for 24 h, and wash the resulting mixture with ethanol and deionized water several times to remove all residues and by-products. Finally, dry the sample in vacuum at 80 °C for 24 h. Obtain GO-EDA; (3) Add 2 g of aluminum oxide to 200 mL of tris(hydroxymethyl)aminomethane solution (10 mM) and stir and ultrasonicate for 1 h. Then add 500 mg of o-phenylenediamine and stir and ultrasonicate for 30 min. Stir the mixture at 60 °C for 6 h. Next, filter the product and wash it with ethanol and deionized water several times. Finally, dry it in vacuum at 80 °C for 24 h. Obtain covalently functionalized Al2O3; (4) Place the carbon fiber in an ethanol-water solution and ultrasonically treat it for 1 h to remove the desizing agent on the surface. Then add 2 g of carbon fiber and 1 g of dopamine hydrochloride to 250 mL of Tris buffer (pH = 8.5) and 150 mL of ethanol, mix, and ultrasonicate for 45 min. Then soak at room temperature for 24 h, and then add the covalently functionalized Al2O3 prepared in step (3) to the suspension and ultrasonicate for 1 h. Then filter and clean the deposited mixed solution, and anneal it in an oven at 200 ° C to finally obtain CF@PDA-Al2O3; (5) 100 mg of GO-EDA prepared in step (2) was placed in a double-necked round-bottom flask and placed on a magnetic stirrer. Then 2 g of ultrasonically treated CF@PDA-Al2O3 and 100 mL of N,N-dimethylformamide were added. Stir at 80°C for 8 h. After stirring, the mixed solution was transferred to a polytetrafluoroethylene-lined autoclave container and subjected to a solvothermal reaction at 200°C for 6 h. After the reaction, the mixture was filtered without washing to retain some unreacted amines on the surface of the material, which facilitated hydrogen bonding between the polymer chain and the filler surface. Finally, the mixture was vacuum dried at 80°C for 24 h. Finally, the modified thermal conductive filler GO-EDA / CF@PDA-Al2O3 was obtained.

[0032] Figure 4 This is a scanning electron microscope image of the thermal conductive nylon 6 composite material prepared in Example 3 of the present invention. GO-EDA / CF@PDA-Al2O3KH560 is distributed in large quantities in the matrix resin to form a thermal conductive channel. At the same time, the amino functional groups on the surface of GO-EDA / CF@PDA-Al2O3KH560 enhance the interface interaction between the modified thermal conductive filler and nylon 6, greatly improving the dispersibility and reducing the interface thermal resistance between the matrix and the filler.

[0033] Comparative Example 1 Pure nylon 6 sample.

[0034] 1) Nylon 6 resin was melt-blended and extruded into granules in a twin-screw extruder. The temperatures of each zone in the extrusion granulation were 215°C / 220°C / 225°C / 225°C / 230°C / 230°C / 235°C, and the screw speed was 30 r / min. 2) The mixed particles were hot-pressed and then cold-pressed on a flat vulcanizer. The hot-pressing temperature was 230°C, the hot-pressing time was 10 min, the cold-pressing temperature was room temperature, the cold-pressing time was 10 min, and the pressure was 10 MPa, and finally a pure nylon 6 sample was obtained.

[0035] Figure 5 This is a scanning electron microscope image of the sample prepared in comparative example 1 of the present invention. It can be observed that the cross section of the pure nylon 6 sample is very smooth.

[0036] Figure 6 The SEM image of the cross section of the carbon fiber distribution in the nylon 6 matrix shows that the compatibility of CF with the matrix resin is poor and there is no effective interface interaction.

[0037] Comparative Example 2 1) 5 parts by weight of CF@PDA-Al2O3 and 95 parts by weight of nylon 6 resin were melt-blended and extruded into granules in a twin-screw extruder. The temperatures of each zone in the extrusion granulation were 215℃ / 220℃ / 225℃ / 225℃ / 230℃ / 230℃ / 235℃, respectively, and the screw speed was 30 r / min. 2) The mixed particles were hot-pressed and then cold-pressed in a flat vulcanizer. The hot-pressing temperature was 230°C, the hot-pressing time was 10 min, the cold-pressing temperature was room temperature, the cold-pressing time was 10 min, and the pressure was 10 MPa, and finally a thermally conductive nylon 6 composite material was obtained.

[0038] The preparation steps of CF@PDA-Al2O3 are as follows: (1) Add 2 g of aluminum oxide to 200 mL of tris(hydroxymethyl)aminomethane solution (10 mM) and stir and ultrasonicate for 1 h. Then add 500 mg of o-phenylenediamine and stir and ultrasonicate for 30 min. Stir the mixture at 60 °C for 6 h. Next, filter the product and wash it with ethanol and deionized water several times. Finally, dry it in vacuum at 80 °C for 24 h. Obtain covalently functionalized Al2O3; (2) The carbon fiber was placed in an ethanol aqueous solution and ultrasonically treated for 1 h to remove the desizing agent on the surface. Then 2 g of carbon fiber and 1 g of dopamine hydrochloride were added to 250 mL of Tris buffer (pH = 8.5) and 150 mL of ethanol and ultrasonically treated for 45 min. Then, it was immersed at room temperature for 24 h, and then the covalently functionalized Al2O3 prepared in step (3) was added to the suspension and ultrasonically shaken for 1 h. The deposited mixed solution was then filtered and cleaned, and annealed in an oven at 200 ° C to finally obtain CF@PDA-Al2O3.

[0039] Figure 7 This is a scanning electron microscope image of the thermal conductive nylon 6 composite material prepared in comparative example 2 of the present invention. It can be seen that the modified thermal conductive filler CF@PDA-Al2O3 is distributed in the matrix, and many alumina particles are attached to CF@PDA-Al2O3, which further proves the successful preparation of CF@PDA-Al2O3. In addition, the prepared CF@PDA-Al2O3 has good compatibility with the matrix resin and can be connected with nylon 6 resin.

[0040] Comparative Example 3 1) 10 parts by weight of CF@PDA-Al2O3 and 90 parts by weight of nylon 6 resin were melt-blended and extruded into granules in a twin-screw extruder. The temperatures of each zone in the extrusion granulation were 215℃ / 220℃ / 225℃ / 225℃ / 230℃ / 230℃ / 235℃, respectively, and the screw speed was 30 r / min. 2) The mixed particles were hot-pressed and then cold-pressed in a flat vulcanizer. The hot-pressing temperature was 230°C, the hot-pressing time was 10 min, the cold-pressing temperature was room temperature, the cold-pressing time was 10 min, and the pressure was 10 MPa, and finally a thermally conductive nylon 6 composite material was obtained.

[0041] The preparation steps of CF@PDA-Al2O3 are as follows: (1) Add 2 g of aluminum oxide to 200 mL of tris(hydroxymethyl)aminomethane solution (10 mM) and stir and ultrasonicate for 1 h. Then add 500 mg of o-phenylenediamine and stir and ultrasonicate for 30 min. Stir the mixture at 60 °C for 6 h. Next, filter the product and wash it with ethanol and deionized water several times. Finally, dry it in vacuum at 80 °C for 24 h. Obtain covalently functionalized Al2O3; (2) The carbon fiber was placed in an ethanol aqueous solution and ultrasonically treated for 1 h to remove the desizing agent on the surface. Then 2 g of carbon fiber and 1 g of dopamine hydrochloride were added to 250 mL of Tris buffer (pH = 8.5) and 150 mL of ethanol and ultrasonically treated for 45 min. Then, it was immersed at room temperature for 24 h, and then the covalently functionalized Al2O3 prepared in step (3) was added to the suspension and ultrasonically shaken for 1 h. The deposited mixed solution was then filtered and cleaned, and annealed in an oven at 200 ° C to finally obtain CF@PDA-Al2O3.

[0042] Comparative Example 4 1) 15 parts by weight of CF@PDA-Al2O3 and 85 parts by weight of nylon 6 resin were melt-blended and extruded into granules in a twin-screw extruder. The temperatures of each zone in the extrusion granulation were 215℃ / 220℃ / 225℃ / 225℃ / 230℃ / 230℃ / 235℃, respectively, and the screw speed was 30 r / min. 2) The mixed particles were hot-pressed and then cold-pressed in a flat vulcanizer. The hot-pressing temperature was 230°C, the hot-pressing time was 10 min, the cold-pressing temperature was room temperature, the cold-pressing time was 10 min, and the pressure was 10 MPa, and finally a thermally conductive nylon 6 composite material was obtained.

[0043] The preparation steps of CF@PDA-Al2O3 are as follows: (1) Add 2 g of aluminum oxide to 200 mL of tris(hydroxymethyl)aminomethane solution (10 mM) and stir and ultrasonicate for 1 h. Then add 500 mg of o-phenylenediamine and stir and ultrasonicate for 30 min. Stir the mixture at 60 °C for 6 h. Next, filter the product and wash it with ethanol and deionized water several times. Finally, dry it in vacuum at 80 °C for 24 h. Obtain covalently functionalized Al2O3; (2) The carbon fiber was placed in an ethanol aqueous solution and ultrasonically treated for 1 h to remove the desizing agent on the surface. Then 2 g of carbon fiber and 1 g of dopamine hydrochloride were added to 250 mL of Tris buffer (pH = 8.5) and 150 mL of ethanol and ultrasonically treated for 45 min. Then, it was immersed at room temperature for 24 h, and then the covalently functionalized Al2O3 prepared in step (3) was added to the suspension and ultrasonically shaken for 1 h. The deposited mixed solution was then filtered and cleaned, and annealed in an oven at 200 ° C to finally obtain CF@PDA-Al2O3.

[0044] The samples obtained in the embodiments and comparative examples were subjected to performance tests, and the results are shown in Table 1.

[0045] The data in Table 1 show that after doping with CF@PDA-Al2O3, the thermal conductivity of the composite material is improved, and it increases with the increase of the doping amount, which is due to the excellent thermal conductivity of CF@PDA-Al2O3. At the same time, the addition of CF@PDA-Al2O3 improves the tensile strength of the composite material. However, at the same addition amount, the thermal conductivity of the composite material with modified thermal conductive fillers is higher than that of the composite material with unmodified thermal conductive fillers, and the thermal conductivity of the doped CF@PDA-Al2O3 composite material is smaller than that of the doped GO-EDA / CF@PDA-Al2O3 composite material. This is because the internal transfer of the CF@PDA-Al2O3 composite material is still one-dimensional heat conduction with CF as the carrier, so the efficiency of heat conduction will be reduced. The three dimensions of the GO-EDA / CF@PDA-Al2O3 composite material are filled with a three-dimensional multi-path heat conduction channel. On the one hand, CF provides long-distance heat flow transfer for the carrier, and the large specific surface of GO makes the hybrid filler occupy a large free volume inside the composite material, so as to avoid the heat flow from the matrix with low thermal conductivity as much as possible, but from the three-dimensional network built by the hybrid filler. The covalent modification reduces the interfacial thermal resistance between the fillers and between the fillers and the matrix. The thermal conductivity of the composite material is improved. With the continued increase of thermal conductive fillers, the elongation at break of the composite material is greatly reduced, which is caused by the partial agglomeration phenomenon between the fillers. In summary, considering the effects of thermal conductivity and mechanical properties, when 15 parts by weight of modified thermal conductive filler (GO-EDA / CF@PDA-Al2O3) is added, a nylon 6 composite material with good mechanical properties and excellent thermal conductivity can be prepared.

[0046] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.

Claims

1. A thermally conductive nylon 6 composite material having a hybrid structure network, characterized in that: Raw materials by weight: 5-15 parts of modified thermal conductive filler, 85-95 parts of nylon 6 particles; The preparation of the modified thermally conductive filler comprises the following steps: (1) 1.5 g natural flake graphite, 1 g NaNO3 and 100 mL concentrated H2SO4 were mixed, the temperature of the mixture was controlled below 10 °C, 5 g KMnO4 was slowly added in five portions while stirring, the mixture was heated to 35 °C, stirred for 24 h, 150 mL deionized water was slowly added, the temperature was raised to 90 °C, stirring was continued for 4 h, 100 mL deionized water and 5 mL H2O2 solution were added, the mixture was stirred for another 1 h, filtered, washed with dilute HCl solution, and freeze-dried to obtain graphene oxide GO; (2) Mix 100 mg GO and 100 mL deionized water, disperse by ultrasonic for 1 h, and add 100 mg ethylenediamine and 200 mg N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride was stirred at 80 °C for 24 h, washed with ethanol and deionized water, and dried under vacuum at 80 °C for 24 h to obtain GO-EDA; (3) Add 2 g of aluminum oxide to 200 mL of 10 mmol / L tris(hydroxymethyl)aminomethane solution, stir and ultrasonicate for 1 h, add 500 mg of o-phenylenediamine, stir and ultrasonicate for 30 min, stir at 60 °C for 6 h, filter, wash with ethanol and deionized water, and dry in vacuum at 80 °C for 24 h to obtain covalently functionalized Al2O3; (4) The carbon fiber was placed in an ethanol solution and ultrasonically treated for 1 h; 2 g of carbon fiber, 1 g of dopamine hydrochloride, 250 mL of Tris buffer (pH = 8.5) and 150 mL of ethanol were mixed, ultrasonicated for 45 min, immersed at room temperature for 24 h, covalently functionalized Al2O3 was added, ultrasonically shaken for 1 h, filtered, and annealed at 200 °C to obtain CF@PDA-Al2O3; (5) Mix 100 mg GO-EDA, 2 g ultrasonically treated CF@PDA-Al2O3 and 100 mL N,N-dimethylformamide, stir at 80 °C for 8 h, solvothermal reaction at 200 °C for 6 h, filter and vacuum dry at 80 °C for 24 h to obtain the modified thermal conductive filler GO-EDA / CF@PDA-Al2O3.

2. A method for preparing the thermally conductive nylon 6 composite material having a hybrid structure network as claimed in claim 1, characterized in that: The following steps are involved: (1) The modified thermal conductive filler GO-EDA / CF@PDA-Al2O3 and nylon 6 particles were mixed evenly, dried at 80 °C for 24 h, and extruded into granules; (2) First hot pressing and melting and then cold pressing and molding to obtain the thermal conductive nylon 6 composite material with a hybrid structure network.

3. The method according to claim 3, characterized in that: The temperatures in each zone during extrusion granulation were 215°C / 220°C / 225°C / 225°C / 230°C / 230°C / 235°C, and the screw speed was 30 r / min.

4. The method according to claim 3, characterized in that: The hot pressing temperature was 230 °C and the time was 10 min; the cold pressing temperature was room temperature and the time was 10 min at a pressure of 10 MPa.