Aerogel composite material as well as preparation method and application thereof
Through the sol-gel reaction of phosphine-based silicon hybrid phenolic resin and fiber mat, an airgel composite material with high-temperature flame retardancy, heat protection and bonding protection properties is prepared, which solves the problem of insufficient flame retardant properties and problems in the existing technology. The problem of insufficient bonding performance is suitable for the insulation layer application of solid rocket motors.
Patent Information
- Application Number
- CN202410709235.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-03
- Publication Date
- 2024-10-01
AI Technical Summary
The application of existing nanoporous materials in the field of internal heat insulation of solid rocket motors is limited by insufficient flame retardant properties, easy powder loss on the surface, and insufficient adhesive properties. The process is complex and difficult to meet the needs of high temperature and high pressure.
Airgel composite materials are prepared by using phosphine-based silicon hybrid phenolic resin matrix and flexible fiber mat through sol-gel reaction. The neutral bonding agent NPBA is used to improve the flame retardancy and bonding performance to form a nanopore structure, combined with fiber reinforcement to Improve toughness and thermal insulation properties.
It improves the material's high-temperature flame retardant properties, prevents powder shedding, enhances the bonding performance with composite solid propellant, provides reliable thermal insulation protection, and is suitable for high-temperature and high-pressure environments.
Smart Images

Figure CN118725583A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of nanoporous materials and resin-based composite materials, and in particular to a preparation, molding process method and application of an aerogel composite material with flame retardancy, heat insulation and bonding protection functions. Background Art
[0002] With the development of spacecraft, solid rocket engines have been widely used, and the types and quantities of demand are growing rapidly, which puts forward higher requirements on the performance and high-quality and efficient manufacturing of solid rocket engines. The main manifestations are: the maximum combustion temperature of solid propellant has reached more than 3000℃, coupled with the scouring of high-pressure hot gas flow, the current ablation-resistant polymer composite material, that is, the insulation layer, urgently needs to be further improved in terms of reducing density and improving ablation resistance; the currently commonly used rubber-based insulation layer molding requires the use of airbag pre-pressing process molding, and the process is complicated, which is one of the bottlenecks of the rapid manufacturing of solid rocket engines, and the molded carbon phenolic composite insulation layer has a small application range due to problems such as high density and brittleness.
[0003] The new integrated heat-insulating composite material with nanoporous structure is a type of aerogel composite material developed in recent years. It adopts a fiber gradient structure design and is formed by a low-pressure RTM molding process of a deeply hybridized phenolic resin. It has the characteristics of density gradient and ceramicization, and has been widely used in the fields of external heat protection of high Mach number spacecraft flying for a long time in and outside the atmosphere. However, its insufficient flame retardant performance under instantaneous high temperature, easy powdering on the surface to form excess materials, and insufficient bonding performance with solid propellants have limited its application in the field of internal heat insulation of solid rocket engines. Summary of the invention
[0004] The technical problem solved by the present application is: to overcome the shortcomings of the prior art, to provide an aerogel composite material with flame retardancy, heat insulation, and bonding protection functions and a preparation method thereof, to improve flame retardancy and toughness, to eliminate powder loss, to bond well with the surface of the composite solid propellant, and to provide reliable thermal insulation protection for the engine casing.
[0005] The technical solutions provided by this application are as follows:
[0006] An aerogel composite material with flame retardancy, heat protection, and bonding protection functions, wherein the sum of the mass percentages is 100%, the phosphinosilicone hybrid phenolic resin matrix is 20-80%, and the flexible fiber felt is 80-20%; wherein the phosphinosilicone hybrid phenolic resin matrix includes a phosphinosilicone resin, a phenolic resin, a curing agent, and a neutral bonding agent NPBA; the above raw materials are mixed with an organic solvent to form a phosphinosilicone hybrid phenolic resin matrix sol and a sol-gel reaction is performed to prepare an aerogel composite material. The nanopore diameter of the aerogel composite material is in the range of 50-1000nm. The aerogel composite material has a thickness of 2-50mm and a density of 120-1400kg / m 3 .
[0007] Furthermore, taking the sum of the mass percentages of the components of the phosphino-silicon hybrid phenolic resin matrix as 100%, the phosphino-silicon hybrid phenolic resin matrix includes 50-60% of phosphino-organic silicone resin, 42-24% of phenolic resin, 7.7-13% of curing agent, and 0.3-3% of neutral bonding agent NPBA.
[0008] Furthermore, the thickness of the flexible fiber felt is 2-50 mm and the density is 120-1400 kg / m 3 The structural forms of the fiber felt include needle-punched mesh, puncture mesh, multi-layer stitching and woven structure; the base material of the fiber felt includes carbon fiber and ceramic fiber; the carbon fiber includes one or more of polyacrylonitrile-based carbon fiber, asphalt-based carbon fiber or graphite-based carbon fiber, and the ceramic fiber includes one or more of quartz fiber, glass fiber, mullite fiber or high silica fiber.
[0009] Furthermore, the molecular structure of the neutral bonding agent NPBA is as shown in formula (1), the molecular pH is controlled between 6.0 and 8.0, and the relative molecular mass is between 3000 and 500000.
[0010] A weakly alkaline catalyst is required for the sol-gel reaction, and the above pH limit ensures that the sol-gel reaction is not affected. Under the above molecular weight limit, the neutral bonding agent NPBA can be well compatible with the phosphine-based silicone resin and the phenolic resin.
[0011] The neutral bonding agent NPBA is copolymerized by acrylonitrile, acrylate and hydroxy acrylate, wherein the acrylate can also be replaced by organic borate and aziridine.
[0012]
[0013] A method for preparing the above-mentioned aerogel composite material having the multifunctionalities of flame retardancy, heat protection and bonding protection, the method comprising the following steps:
[0014] S1: Preparation of phosphino-silicon hybrid phenolic resin matrix sol: prepare a phosphino-silicon resin solution and a phenolic resin solution, and stir the organic solvent, the phosphino-silicon resin solution, the phenolic resin solution, the curing agent, and the neutral bonding agent NPBA to obtain a phosphino-silicon hybrid phenolic resin matrix sol;
[0015] S2: Sol impregnation: placing the fiber reinforcement (i.e., flexible fiber felt) in a mold, and completely impregnating the phosphine-based silicon hybrid phenolic resin matrix sol into the fiber reinforcement;
[0016] S3: Sol-gel reaction: sealing the mold, performing a sol-gel reaction, and cooling to room temperature after the reaction to obtain a composite material;
[0017] S4: Drying of the composite material: The mold is opened, and then the composite material is vacuum dried or supercritically dried to obtain an aerogel composite material having the functions of flame retardancy, heat protection, and bonding protection.
[0018] Furthermore, in step S1, the organic solvent includes one or more of n-butanol, isopropanol, ethanol or ethylene glycol, the mass ratio of the organic solvent to the phosphino-silicon hybrid phenolic resin matrix is (1.0-6):1, and the curing agent is hexamethylenetetramine, and the added amount is 7.7-12ωt% of the mass of the phosphino-silicon hybrid phenolic resin matrix.
[0019] Furthermore, in step S3, the sol-gel reaction temperature is 80-180° C. and the reaction time is 12-48 hours.
[0020] Further, in step S2, the impregnation includes a normal pressure impregnation method, a vacuum assisted impregnation method or a low pressure perfusion method;
[0021] The atmospheric pressure impregnation method is to place the sealed fiber reinforcement in a non-vacuumed mold and use gravity to make the phosphine-based silicon hybrid phenolic resin matrix sol impregnate the fiber reinforcement;
[0022] The vacuum-assisted impregnation method is to first evacuate the sealed mold containing the fiber reinforcement, keep it under vacuum for a certain period of time, and then open the feed valve on the mold to allow the mold to absorb the phosphine-based silicon hybrid phenolic resin matrix sol to fully impregnate the fiber reinforcement;
[0023] The low-pressure infusion method is to inject the phosphine-based silicon hybrid phenolic resin matrix sol into a sealed mold equipped with a fiber reinforcement by vacuum-assisted impregnation, and the pressure is controlled at 1.5-4 bar.
[0024] Furthermore, in step S4, the vacuum drying temperature is 60-120° C., the pressure is -0.09 to -0.01 MPa, and the time is 24-48 hours.
[0025] Furthermore, in step S4, the supercritical drying conditions are: using carbon dioxide as the drying medium, the reaction temperature is 60-80°C, the pressure in the high-pressure reactor is 8-12MPa, the degassing rate is 5-20L / min, and the drying time is 8-20h.
[0026] Further, in step S1, the phosphine-based silicone resin solution is prepared by the following steps:
[0027] Add phosphine-containing organosilicon monomer, organosilicon monomer and the first solvent into the reactor, then add the first catalyst, heat under nitrogen protection to polymerize the monomer, condense and reflux to obtain a phosphine-containing organosilicon resin solution.
[0028] The phosphine-containing organosilicon monomer includes one or more of 2-diphenylphosphinoethyltriethoxysilane, 3-diphenylphosphinoethyltriethoxysilane, 2-diphenylphosphinoethyltrimethoxysilane, 3-diphenylphosphinopropyltrimethoxysilane, diphenylphosphinomethyltriethoxysilane, vinyl (diphenylphosphinoethyl) dimethylsilane, and 6-diphenylphosphinohexyltriethoxysilane.
[0029] The organic silicon monomer includes one or more of ethyl orthosilicate, methyltrimethoxysilane, phenyltrimethoxysilane, dodecyltrimethoxysilane or diphenyldimethoxysilane.
[0030] The molar ratio of the phosphine-containing organosilicon monomer to the organosilicon monomer is (0.1-0.5):1; the first solvent is an alcohol; the first catalyst includes concentrated hydrochloric acid; the molar amount of the catalyst is 2-5% of the organosilicon monomer; the temperature of the polymerization reaction is 70-90°C and the time is 24-48h.
[0031] In the above-mentioned method for preparing the phosphine-based silicone resin solution, the yield of the phosphine-based silicone resin is higher.
[0032] Furthermore, the phenolic resin solution is prepared by the following steps:
[0033] The phenolic resin is dissolved in a solvent and stirred evenly to obtain a phenolic resin solution; the phenolic resin is a thermoplastic phenolic resin; and the solvent is a first solvent.
[0034] Beneficial effects:
[0035] The composite material is composed of a porous phosphine-based silicon hybrid phenolic resin matrix and a fiber reinforcement of different weaves. The material uses a phosphine-based silicon flame retardant (i.e., a phosphine-based silicone resin) and a neutral bonding agent to improve the flame retardancy and bonding properties of the hybrid phenolic resin-based aerogel composite material, inhibit the powdering of phenolic particles on its surface, and has excellent thermal insulation and ablation resistance. The density is 0.3-1.2g / cm3 The nanopore diameter is in the range of 50-1000nm, the flame retardancy reaches UL94 V-0 level (hereinafter referred to as V-0 level), and the thermal conductivity is in the range of 0.06-0.12W·m -l ·K -1 The bonding strength with the composite solid propellant is greater than 800KPa, the material ablation retreat is less than 0.001mm / s after the dynamic ablation test with a combustion temperature exceeding 3000℃ and a working time of 5.571s.
[0036] Regarding flame retardancy, taking 2-diphenylphosphinoethyltriethoxysilane (a type of phosphine-containing organosilicon monomer) as an example, the reaction between the oligomer formed during the hydrolysis of the organosilicon monomer and the oligomer is as follows:
[0037]
[0038] Organosilicon monomers such as methyltrimethoxysilane are easily hydrolyzed to form silane oligomers containing a large number of hydroxyl groups. 2-Diphenylphosphinoethyltriethoxysilane has good compatibility with the organosilicon monomer system and will participate in the hydrolysis process of the organosilicon monomer to form phosphine-containing organosilicon oligomers, namely phosphine-based organosilicon resins. When this type of oligomer undergoes a sol-gel reaction with phenolic resin, the phosphine group is incorporated into the resin skeleton of the aerogel composite material, forming an intramolecular synergistic flame retardant system of phosphorus-nitrogen-silicon, which effectively improves the flame retardancy of the material.
[0039] Regarding the adhesion and powder-removal inhibition performance, taking the NPBA molecule with a viscosity-average molecular weight of 8846, a hydroxyl content of 0.165 mol / 100g, and a boron content of 0.372% as an example, its chemical reaction mechanism in the aerogel composite material system and the composite solid propellant bonding layer is as follows:
[0040]
[0041] The enlarged structure of the chemical reaction product is as follows:
[0042]
[0043] NPBA carries multiple hydroxyl groups that can undergo hydroxyl condensation reactions with the remaining phenolic hydroxyl groups in the aerogel composite material. The cyano group can use its own polarity to form hydrogen bonds with phenolic hydroxyl groups or silanols. Through the above chemical reactions and relying on the large molecular weight of NPBA, a tough coating layer can be formed on the surface of the aerogel composite material, thereby preventing the hybrid phenolic resin particles from falling off.
[0044] Composite solid propellants are generally bonded with a polyurethane lining and an insulation layer on the inner wall of an engine housing (i.e., the aerogel composite material obtained in this application). Taking hydroxybutyric acid propellant as an example, a polyurethane lining formed by the reaction of hydroxybutyric acid glue and a curing agent such as IPDI is generally used as an adhesive layer. Adjusting the curing parameters can make the residual part of IPDI have isocyanate groups, and the isocyanate groups can react with the remaining hydroxyl groups of NPBA in the insulation layer on the inner wall of the engine housing, thereby improving the bonding strength.
[0045] In summary, this application at least includes the following beneficial technical effects:
[0046] (1) In the present invention, the phosphine group can be grafted into the phenolic resin structure under the reaction conditions specified in the present application. Under the service environment, the aerogel composite material is subjected to high-temperature gas scouring to form a hard SiC ceramic layer on the surface. The phosphine group is evenly distributed inside the hard SiC ceramic layer formed by the reaction of the phosphine-based organosilicon hybrid phenolic resin with the fiber and the resin, so that the material has excellent flame retardant properties. At the same time, the polarity of the phosphine group can attract the neutral bonding agent, thereby improving the bonding force between the components of the material, so that the toughness and mechanical properties of the material are enhanced.
[0047] (2) The neutral bonding agent in the present invention contains -CN and -OH reactive functional groups and has a high polarity. On the one hand, it can attract or react with the phosphine group inside the material and the -OH in the phenolic resin to form a coating layer, thereby enhancing the binding force between the phenolic resin nanoparticles and significantly reducing the powder loss rate. On the other hand, when the material is used in the field of solid rocket engine insulation layer, the remaining -CN and -OH reactive functional groups can effectively combine with the polyurethane-based lining layer and the residual isocyanate curing agent or hydroxyl group in the composite solid agent to form an effective bonding layer;
[0048] (3) The technical solution of the present invention simultaneously improves the mechanical properties of the composite material, and also gives the material flame retardant and adhesive properties. Through multi-parameter matching, numerous difficulties are overcome, so that the thermal insulation and ablation resistance of the composite material remain unchanged, meeting the basic application requirements in the fields of external heat protection of aerospace vehicles, internal insulation of solid rocket engines, thermal insulation coatings for lithium batteries, and external thermal insulation gaskets for engines. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 It is a sample of the composite material of the present invention.
[0050] Figure 2 It is the microstructure of the composite material of the present invention.
[0051] Figure 3 It is a sample of the composite material and the composite solid propellant jointly pulled apart by the present invention.
[0052] Figure 4 These are samples of the composite material of the present invention before and after ablation. DETAILED DESCRIPTION
[0053] The word "exemplary" is used exclusively herein to mean "serving as an example, embodiment, or illustration." Any embodiment described herein as "exemplary" is not necessarily to be construed as preferred or advantageous over other embodiments. Although various aspects of the embodiments are shown in the drawings, the drawings are not necessarily drawn to scale unless otherwise noted.
[0054] Example 1
[0055] Add 2-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane (the molar ratio of the two is 0.1:1) and ethanol into a reactor, then add concentrated hydrochloric acid as a catalyst, the molar amount of HCl in the concentrated hydrochloric acid is 5% of 2-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane, heat to 80°C for monomer polymerization, the reaction time is 24h, condense and reflux to obtain a 2-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane oligomeric mixture, i.e., a phosphino silicone resin solution, wherein the content of the phosphino silicone resin in the 2-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane oligomeric mixture is 95%;
[0056] Dissolve the thermoplastic phenolic resin in isopropanol and stir evenly to obtain a phenolic resin solution with a phenolic resin content of 50%; add 0.095Kg of the oligomeric mixture of 2-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane just prepared to 0.12Kg of the phenolic resin solution, heat to 90°C, reflux for 3h, add 3g of neutral bonding agent NBPA, adjust the pH to about 7, dissolve it in 0.12Kg of isopropanol, and add 0.015Kg of curing agent hexamethylenetetramine. Obtain 0.353Kg of phosphinosilicone hybrid phenolic resin matrix sol. Among them, there are 0.09Kg of phosphinosilicone resin, 0.06Kg of phenolic resin, 0.003Kg of NBPA, 0.18Kg of isopropanol (including isopropanol in the phenolic resin solution) and 0.015Kg of curing agent.
[0057] The density is 370kg / m 3, the 10mm thick polyacrylonitrile-based carbon fiber felt was cut into a square (148g) of 200mm×200mm, placed in a customized stainless steel mold, pressed to a thickness of 5mm, installed the injection port and the outlet, and checked the air tightness of the device. 0.353Kg of phosphinosilicone hybrid phenolic resin matrix sol was transferred to the tank of the RTM injection machine, the heating device was turned on to heat to 60℃ to maintain a constant temperature, the tank was connected to the injection port of the stainless steel mold through a rubber pipe, and the outlet was connected to the vacuum pump through a buffer device; the vacuum pump was turned on to reduce the pressure in the mold to below 2KPa, the tank switch was turned on, and the prepared phosphinosilicone hybrid phenolic resin matrix sol was slowly injected into the mold by vacuum-assisted impregnation method until no bubbles appeared in the sol at the outlet, and then continued to pour for 10min, and finally the injection port and the outlet of the mold were closed, sealed and placed in a vacuum drying oven at 80℃, and after sol-gel reaction and 48h aging molding, the sample was demolded and taken out for drying.
[0058] First, place the formed sample directly in a fume hood and dry it at room temperature and pressure for 48 hours; then place it in a forced air drying oven at 80°C for more than 48 hours, and stop when there is no amine smell; use a knife to remove excess resin on the surface, and then place the dried sample in a 120°C vacuum drying oven to further remove the solvent under vacuum conditions for 24 hours; after drying, wait for the oven to cool to room temperature, take out the sample, and prepare an aerogel composite material with flame retardancy, heat protection, and bonding protection.
[0059] The product obtained in this embodiment is as Figure 1 and Figure 2 shown.
[0060] Example 2
[0061] The difference from Example 1 is that the density of the flexible fiber felt is 370 kg / m 3 , quartz fiber felt with a thickness of 10mm.
[0062] Example 3
[0063] The difference from Example 1 is that the flexible fiber felt is polyacrylonitrile-based carbon fiber and quartz fiber in a mass ratio of 1:1, and the density of the polyacrylonitrile-based carbon fiber and quartz fiber is 370 kg / m 3 , thickness is 10mm.
[0064] Example 4
[0065] Add 2-diphenylphosphinoethyltriethoxysilane and ethyl orthosilicate (the molar ratio of the two is 0.1:1) and ethanol into a reactor, then add concentrated hydrochloric acid as a catalyst, the molar amount of HCl in the concentrated hydrochloric acid is 5% of 2-diphenylphosphinoethyltriethoxysilane and ethyl orthosilicate, heat to 80°C to carry out monomer polymerization reaction, the reaction time is 24 hours, condense and reflux to obtain a hydrolyzed oligomeric mixture of 2-diphenylphosphinoethyltriethoxysilane and ethyl orthosilicate, that is, a phosphino silicone resin solution, wherein the content of the phosphino silicone resin in the hydrolyzed oligomeric mixture of 2-diphenylphosphinoethyltriethoxysilane and ethyl orthosilicate is 95%;
[0066] Thermoplastic phenolic resin was dissolved in isopropanol and stirred evenly to obtain a phenolic resin solution with a resin content of 50%. 0.09 kg of the phenolic resin solution was taken out, and 0.079 kg of the oligomeric mixture of 2-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane prepared just now was added. The temperature was raised to 90°C, and after reflux heating for 3 hours, 3 g of neutral bonding agent NBPA was added, and the pH was adjusted to about 7. The mixture was dissolved in 0.12 kg of isopropanol, and 0.015 kg of curing agent hexamethylenetetramine was added. 0.304 kg of phosphinosilicone hybrid phenolic resin matrix sol was obtained, including 0.075 kg of phosphinosilicone resin, 0.045 kg of phenolic resin, 0.003 kg of NBPA, 0.165 kg of isopropanol and 0.015 kg of curing agent.
[0067] The density is 370kg / m 3 , a 10mm thick polyacrylonitrile-based carbon fiber was cut into a square (148g) of 200mm×200mm, placed in a customized stainless steel mold, pressed to a thickness of 5mm, installed the injection port and the outlet, and checked the air tightness of the device. 0.303Kg of phosphinosilicone hybrid phenolic resin matrix sol was transferred to the tank of the RTM injection machine, the heating device was turned on to heat it to 60℃ to maintain a constant temperature, the tank was connected to the injection port of the stainless steel mold through a rubber pipe, and the outlet was connected to the vacuum pump through a buffer device; the vacuum pump was turned on to reduce the pressure in the mold to below 2KPa, the tank switch was turned on, and the prepared phosphinosilicone hybrid phenolic resin matrix sol was slowly injected into the mold by the vacuum-assisted impregnation method until no bubbles appeared in the sol at the outlet, and then continued to pour for 10min, and finally the injection port and the outlet of the mold were closed, sealed and placed in a vacuum drying oven at 85℃, and after sol-gel reaction and 48h aging molding, the sample was demolded and taken out for drying;
[0068] First, the formed sample is directly placed in a supercritical device, with carbon dioxide as the drying medium, the reaction temperature is 80°C, the pressure in the high-pressure reactor is 12MPa, the degassing rate is 10L / min, and the drying time is 12h; after taking it out, put it in an 85°C forced air drying oven for more than 48h, and stop when there is no amine smell; use a knife to remove excess resin on the surface, and then put the dried sample into a 120°C vacuum drying oven, and further remove the solvent under vacuum conditions for 24h; after drying, wait for the oven to cool to room temperature, take out the sample, and prepare an aerogel composite material with flame retardancy, heat protection, and bonding protection.
[0069] Example 5
[0070] The difference from Example 4 is that the flexible fiber felt has a density of 370 kg / m 3 , quartz fiber felt with a thickness of 10mm.
[0071] Example 6
[0072] The difference from Example 4 is that the flexible fiber felt is a polyacrylonitrile-based carbon fiber and a quartz fiber felt in a mass ratio of 1:1, and the density of the polyacrylonitrile-based carbon fiber and the quartz fiber felt is 370 kg / m 3 , thickness is 10mm.
[0073] Example 7
[0074] Add 3-diphenylphosphinopropyltrimethoxysilane and methyltrimethoxysilane (the molar ratio of the two is 0.1:1) and ethanol into a reactor, then add concentrated hydrochloric acid as a catalyst, the molar amount of HCl in the concentrated hydrochloric acid is 5% of 3-diphenylphosphinopropyltrimethoxysilane and methyltrimethoxysilane, heat to 80°C for monomer polymerization, the reaction time is 24h, condense and reflux to obtain an oligomeric mixture of 3-diphenylphosphinopropyltrimethoxysilane and methyltrimethoxysilane, and the content of phosphino silicone resin in the hydrolyzed oligomeric mixture of 3-diphenylphosphinoethyltriethoxysilane and ethyl orthosilicate is 95%;
[0075] Thermoplastic phenolic resin was dissolved in isopropanol and stirred evenly to obtain a phenolic resin solution with a resin content of 50%; 0.276 kg of the phenolic resin solution was taken out, and then 0.338 kg of the oligomeric mixture of 3-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane prepared just now was added, and the temperature was raised to 90°C, and after reflux heating for 3 hours, 6 g of neutral bonding agent NBPA was added, and the pH was adjusted to about 7, and then it was dissolved in 0.384 kg of isopropanol, and 0.046 kg of curing agent hexamethylenetetramine was added to obtain 1.05 kg of phosphinosilicone hybrid phenolic resin matrix sol. Among them, 0.321 kg of phosphinosilicone resin, 0.138 kg of phenolic resin, 0.006 kg of NBPA, 0.522 kg of isopropanol and 0.046 kg of curing agent were added.
[0076] The density is 500kg / m 3 , a hollow polyacrylonitrile-based carbon fiber felt (weight 0.459kg) with a thickness of 5mm, a diameter of 200mm, and a length of 300mm is placed in a customized stainless steel mold, the injection port and the outlet are installed, and the air tightness of the device is checked. The phosphine-based silicon hybrid phenolic resin matrix sol is transferred to the tank of the RTM injection machine, the heating device is turned on to heat it to 60°C to maintain a constant temperature, the tank is connected to the injection port of the stainless steel mold through a rubber pipe, and the outlet is connected to the vacuum pump through a buffer device; the vacuum pump is turned on to reduce the pressure in the mold to below 2KPa, the tank switch is turned on, and 1.05Kg of the prepared phosphine-based silicon hybrid phenolic resin matrix sol is slowly injected into the mold by the vacuum-assisted impregnation method until there are no more bubbles in the sol at the outlet, and then the infusion is continued for 10 minutes, and finally the injection port and the outlet of the mold are closed, sealed and placed in a vacuum drying oven at 80°C, and after sol-gel reaction and 48h aging molding, the sample is demolded and taken out for drying;
[0077] First, place the formed sample directly in a fume hood and dry it at room temperature and pressure for 48 hours; then place it in a forced air drying oven at 80°C for more than 48 hours, and stop when there is no amine smell; use a knife to remove excess resin on the surface, and then place the dried sample in a 120°C vacuum drying oven to further remove the solvent under vacuum conditions for 24 hours; after drying, wait for the oven to cool to room temperature, take out the sample, and prepare a circular tube-shaped aerogel composite material with flame retardancy, heat protection, and bonding protection functions.
[0078] Example 8
[0079] The difference from Example 7 is that the flexible fiber felt has a density of 500 kg / m 3 , hollow quartz fiber felt with a thickness of 5 mm, a diameter of 200 mm, and a length of 300 mm (weight 0.459 kg).
[0080] Example 9
[0081] The difference from Example 7 is that the flexible fiber felt is a hollow polyacrylonitrile-based carbon fiber felt and a quartz fiber felt in a mass ratio of 1:1, and the density of the hollow polyacrylonitrile-based carbon fiber felt and the quartz fiber felt is 500 kg / m 3 , thickness is 5mm, diameter is 200mm and length is 300mm.
[0082] The performance of the aerogel composite materials obtained in Examples 1-9 was tested, and the results are shown in Table 1.
[0083] Table 1 Performance test table of aerogel composite materials of Examples 1-9
[0084]
[0085] The above embodiments illustrate that when different types of fiber felts are used in the composite material, the thermal conductivity of the carbon fiber felt increases and the ablation rate decreases; the thermal conductivity of the quartz fiber felt decreases and the ablation rate increases; the use of different types of phosphine-based silicone resins will be reflected in different ablation properties. For example, 3-diphenylphosphinopropyltrimethoxysilane (methoxy silane) has a fast hydrolysis rate, which is beneficial to increase the phosphine and phenyl content in the phosphine-containing silicone resin product, and has a certain improvement effect on the ablation performance of the final aerogel composite material product, which is higher than the use of 2-diphenylphosphinoethyltriethoxysilane; similarly, ethyl orthosilicate has a fast hydrolysis rate, which is also beneficial to increase the phosphine and phenyl content in the phosphine-containing silicone resin product, and has a certain improvement effect on the ablation performance of the final aerogel composite material product.
[0086] in, Figure 3 Schematic diagram of a combined tearing test of the composite material obtained in Example 1 according to (QJ 2038.1A-2004, Test method for interfacial bonding strength of solid rocket engine combustion chamber Part 1: Rectangular specimen tearing method); Figure 4 This is a schematic diagram of the ablation test of the composite material obtained in Example 1 according to (GJB 323A-1996, ablation test method for ablative materials).
[0087] Example 10
[0088] A phosphine-based organosilicon resin solution is obtained by the following preparation method:
[0089] 2-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane (the molar ratio of the two is 0.1:1) and ethanol are added to the reactor, and then concentrated hydrochloric acid as a catalyst is added. The molar amount of HCl in the concentrated hydrochloric acid is 5% of 2-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane. The monomer polymerization reaction is heated to 80°C for 24 hours, and condensed and refluxed to obtain a mixture of 2-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane oligomers. According to the spectral method, the content of phosphino silicone resin in the mixture of 2-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane oligomers is 95%.
[0090] A phenolic resin solution is obtained by the following preparation method: dissolving thermoplastic phenolic resin in isopropanol and stirring evenly to obtain a phenolic resin solution. The content of phenolic resin in the phenolic resin solution is 50%.
[0091] An aerogel composite material is obtained by the following preparation method:
[0092] According to the content of the product in the oligomeric mixture of 2-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane and the content of phenolic resin in the phenolic resin solution, the above-obtained 0.303 kg of the oligomeric mixture of 2-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane was added to 0.384 kg of the phenolic resin solution and mixed evenly, the temperature was raised to 90°C, and refluxed for 3 hours, and then 5 g of a neutral bonding agent NBPA was added, the pH was adjusted to about 7, and then it was dissolved in 0.378 kg of isopropanol, and 0.048 kg of a curing agent hexamethylenetetramine was added to obtain 1.103 kg of a phosphinosilicone hybrid phenolic resin matrix sol.
[0093] In the phosphinosilicone hybrid phenolic resin matrix sol, the mass of the phosphinosilicone resin is 0.288Kg, the mass of the phenolic resin is 0.192Kg, the neutral bonding agent NBPA is 5g, the mass of isopropanol is 0.57Kg (0.384 / 2+0.378, including the isopropanol in the phenolic resin solution), and the mass of the curing agent is 0.048Kg.
[0094] The density is 600kg / m 3, the 10mm thick polyacrylonitrile-based carbon fiber felt was cut into a square of 200mm×200mm (i.e. the mass of the flexible fiber felt was 0.24kg), put into a customized stainless steel mold, pressed to a thickness of 5mm, installed the injection port and the outlet, and checked the air tightness of the device. 1.103Kg of phosphine-based silicon hybrid phenolic resin matrix sol was transferred to the tank of the RTM injection machine, the heating device was turned on to heat to 60℃ to maintain a constant temperature, the tank was connected to the injection port of the stainless steel mold through a rubber pipe, and the outlet was connected to the vacuum pump through a buffer device; the vacuum pump was turned on to reduce the pressure in the mold to below 2KPa, the tank switch was turned on, and the prepared phosphine-based silicon hybrid phenolic resin matrix sol was slowly injected into the mold by vacuum-assisted impregnation method until no bubbles appeared in the sol at the outlet, and then continued to pour for 10min, and finally the injection port and the outlet of the mold were closed, sealed and placed in a vacuum drying oven at 80℃, and after sol-gel reaction and 48h aging molding, the sample was demolded and taken out for drying.
[0095] First, place the formed sample directly in a fume hood and dry it at room temperature and pressure for 48 hours; then place it in a forced air drying oven at 80°C for more than 48 hours, and stop when there is no amine smell; use a knife to remove excess resin on the surface, and then place the dried sample in a 120°C vacuum drying oven to further remove the solvent under vacuum conditions for 24 hours; after drying, wait for the oven to cool to room temperature, take out the sample, and prepare an aerogel composite material with flame retardancy, heat protection, and bonding protection.
[0096] Embodiment 11
[0097] The only difference from Example 10 is:
[0098] According to the content of phosphino silicone resin in the oligomeric mixture of 2-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane and the content of phenolic resin in the phenolic resin solution, the above-obtained 0.252 kg of 2-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane oligomeric mixture was added to 0.32 kg of phenolic resin solution and mixed evenly, heated to 90°C, refluxed for 3 hours, added with 5 g of neutral bonding agent NBPA, adjusted the pH to about 7, dissolved in 0.374 kg of isopropanol, and added with 0.04 kg of curing agent hexamethylenetetramine to obtain 0.925 kg of phosphinosilicone hybrid phenolic resin matrix sol.
[0099] In the phosphinosilicone hybrid phenolic resin matrix sol, the mass of the phosphinosilicone resin is 0.24Kg, the mass of the phenolic resin is 0.16Kg, the mass of the neutral bonding agent NBPA is 5g, the mass of isopropyl alcohol is 0.48Kg, and the mass of the curing agent is 0.04Kg.
[0100] The density is 700kg / m3 The polyacrylonitrile-based carbon fiber felt with a thickness of 10 mm was cut into a square with a size of 200 mm×200 mm (ie, the mass of the flexible fiber felt was 0.28 kg).
[0101] Example 12
[0102] The only difference from Example 10 is:
[0103] According to the content of phosphino silicone resin in the oligomeric mixture of 2-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane and the content of phenolic resin in the phenolic resin solution, the above-obtained 0.337 kg of 2-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane oligomeric mixture was added to 0.256 kg of phenolic resin solution and mixed evenly, heated to 90°C, refluxed for 3 hours, and then 5 g of neutral bonding agent NBPA was added to adjust the pH to about 7 to obtain 0.32 kg of silicone hybrid phenolic resin, which was then dissolved in 0.145 kg of isopropanol, and 0.032 kg of curing agent hexamethylenetetramine was added to obtain 0.741 kg of phosphino silicone hybrid phenolic resin matrix sol.
[0104] In the phosphinosilicone hybrid phenolic resin matrix sol, the mass of the phosphinosilicone resin is 0.192 Kg, the mass of the phenolic resin is 0.128 Kg, the mass of the neutral bonding agent NBPA is 5 g, the mass of the isopropyl alcohol is 0.384 Kg, and the mass of the curing agent is 0.032 Kg.
[0105] The density is 800kg / m 3 The polyacrylonitrile-based carbon fiber felt with a thickness of 10 mm was cut into a square with a size of 200 mm×200 mm (ie, the mass of the flexible fiber felt was 0.32 kg).
[0106] Embodiment 13
[0107] The only difference from Example 10 is:
[0108] According to the content of the product in the oligomeric mixture of 2-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane and the content of phenolic resin in the phenolic resin solution, the above-obtained 0.299 kg of the oligomeric mixture of 2-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane was added to 0.35 kg of the phenolic resin solution and mixed evenly.
[0109] That is, the mass of the phosphine-based silicone resin is 0.284 Kg, and the mass of the phenolic resin is 0.175 Kg.
[0110] Embodiment 14
[0111] The only difference from Example 10 is:
[0112] According to the content of the product in the oligomeric mixture of 2-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane and the content of phenolic resin in the phenolic resin solution, the above-obtained 0.316 kg of the oligomeric mixture of 2-diphenylphosphinoethyltriethoxysilane and methyltrimethoxysilane was added to 0.30 kg of the phenolic resin solution and mixed evenly.
[0113] That is, the mass of the phosphine-based silicone resin is 0.30 Kg, and the mass of the phenolic resin is 0.15 Kg.
[0114] Embodiment 15
[0115] The only difference from Example 10 is that 2 g of neutral bonding agent NBPA is added.
[0116] Example 16
[0117] The only difference from Example 10 is that 8 g of neutral bonding agent NBPA is added.
[0118] The performance of the aerogel composite materials obtained in Examples 10-16 was tested, and the results are shown in Table 2.
[0119]
[0120] According to Table 2, it can be seen that in Examples 10-12, the contents of various components are different, and within the scope of the present application, their mechanical properties, bonding properties and ablation properties are all good.
[0121] In Examples 10, 13-14, the total mass of the phosphine-based silicone resin and the phenolic resin remains unchanged, and the mass ratio of the phosphine-based silicone resin and the phenolic resin is different. As the mass ratio of the phosphine-based silicone resin and the phenolic resin increases, the phosphine groups in the system increase, the bonding strength is enhanced (combined pull-off strength), and the mechanical strength is reduced.
[0122] In Examples 10, 15-16, as the amount of NPBA increases, the bonding strength increases significantly (combined tear strength). When the amount of NPBA is too high, the sol-gel reaction and subsequent mechanical and ablation resistance properties will be affected (the surface will become relatively soft).
[0123] The present application is described in detail above in conjunction with specific implementation methods and exemplary examples, but these descriptions cannot be understood as limiting the present application. Those skilled in the art understand that, without departing from the spirit and scope of the present application, a variety of equivalent replacements, modifications or improvements can be made to the technical solution of the present application and its implementation methods, all of which fall within the scope of the present application. The scope of protection of the present application shall be subject to the attached claims.
[0124] The contents not described in detail in this application specification belong to the common knowledge of those skilled in the art.
Claims
1. An aerogel composite material, It is characterized in that The composite material comprises the following components, based on the sum of mass percentages being 100%: 20-80% of phosphino-silicon hybrid phenolic resin matrix and 80-20% of flexible fiber felt; wherein the phosphino-silicon hybrid phenolic resin matrix comprises phosphino-organic silicone resin, phenolic resin, curing agent and neutral bonding agent NPBA.
2. An aerogel composite material according to claim 1, It is characterized in that Taking the sum of the mass percentages of the components of the phosphinosilicone hybrid phenolic resin matrix as 100%, the phosphinosilicone hybrid phenolic resin matrix includes 50-60% of phosphinosilicone resin, 42-24% of phenolic resin, 7.7-13% of curing agent and 0.3-3% of neutral bonding agent NPBA.
3. An aerogel composite material according to claim 1, It is characterized in that The molecular structure of the neutral bonding agent NPBA is as shown in formula (1); the pH of the neutral bonding agent NPBA is 6.0-8.0, and the relative molecular mass is 3000-500000; 4. An aerogel composite material according to claim 1, It is characterized in that The thickness of the flexible fiber felt is 2-50 mm, and the density is 120-1400 kg / m; the structure of the fiber felt is selected from needle-punched mesh, puncture mesh, multi-layer stitching and / or braided structure; the material of the fiber felt is selected from carbon fiber or ceramic fiber.
5. An aerogel composite material according to claim 1, It is characterized in that The phosphine-based silicone resin is obtained by polymerization of a phosphine-containing silicone monomer and a silicone monomer, and the molar ratio of the phosphine-containing silicone monomer to the silicone monomer is (0.1-0.5):
1.
6. An aerogel composite material according to claim 5, It is characterized in that The phosphine-containing organosilicon monomer is selected from 2-diphenylphosphinoethyltriethoxysilane, 3-diphenylphosphinoethyltriethoxysilane, 2-diphenylphosphinoethyltrimethoxysilane, 3-diphenylphosphinopropyltrimethoxysilane, diphenylphosphinomethyltriethoxysilane, vinyldiphenylphosphinoethyldimethylsilane or 6-diphenylphosphinohexyltriethoxysilane; The organic silicon monomer is selected from ethyl orthosilicate, methyltrimethoxysilane, phenyltrimethoxysilane, dodecyltrimethoxysilane or diphenyldimethoxysilane.
7. A method for preparing an aerogel composite material, It is characterized in that The following steps are involved: S1: Preparation of phosphino-silicon hybrid phenolic resin matrix sol: uniformly mixing an organic solvent, a phosphino-silicon resin, a phenolic resin, a curing agent and a neutral bonding agent NPBA to obtain a phosphino-silicon hybrid phenolic resin matrix sol; S2: Sol impregnation: placing the flexible fiber felt in a mold, and completely impregnating the phosphine-based silicon hybrid phenolic resin matrix sol into the flexible fiber felt; S3: Sol-gel reaction: sealing the mold, performing a sol-gel reaction, and cooling to room temperature after the reaction to obtain a composite material; S4: drying the composite material; in the dried composite material, based on the sum of mass percentages being 100%, the phosphino-silicon hybrid phenolic resin matrix comprises 20-80% and the flexible fiber felt comprises 80-20%.
8. The method for preparing an aerogel composite material according to claim 7, It is characterized in that In the step S1, a phosphine-based silicone resin solution and a phenolic resin solution are prepared, and according to the content of the phosphine-based silicone resin in the phosphine-based silicone resin solution and the content of the phenolic resin in the phenolic resin solution, an organic solvent, a phosphine-based silicone resin solution, a phenolic resin solution, a curing agent, and a neutral bonding agent NPBA are uniformly stirred to obtain a phosphine-based silicon hybrid phenolic resin matrix sol.
9. A method for preparing an aerogel composite material according to claim 7 or 8, It is characterized in that In the step S1, the organic solvent is selected from n-butanol, isopropanol, ethanol or ethylene glycol; the mass ratio of the organic solvent to the phosphino-silicon hybrid phenolic resin matrix is (1.0-6):1; the curing agent is hexamethylenetetramine, and the added amount of the curing agent is 7.7-12ωt% of the mass of the phosphino-silicon hybrid phenolic resin matrix; In step S3, the sol-gel reaction temperature is 80-180° C. and the reaction time is 12-48 hours.
10. The method for preparing an aerogel composite material according to claim 8, It is characterized in that The phosphine-based silicone resin solution comprises the following preparation steps: Adding a phosphine-containing organosilicon monomer, an organosilicon monomer and a first solvent into a reactor, and then adding a first catalyst, heating under nitrogen protection to polymerize the monomers, condensing and refluxing to obtain a phosphine-containing organosilicon resin solution; The first solvent is alcohol; the first catalyst includes concentrated hydrochloric acid; the molar amount of the catalyst is 2-5% of the molar amount of the organosilicon monomer; the polymerization reaction temperature is 70-90° C. and the time is 24-48 hours.
11. An aerogel composite material according to any one of claims 1 to 6, or an aerogel composite material obtained by the preparation method of an aerogel composite material according to any one of claims 7 to 10, used as an ablation-resistant material for a solid rocket engine combustion chamber, a lithium battery insulation material, a building material, or a pneumatic thermal protection material.
Citation Information
Cited By
Thermal protection composite material and preparation method thereof
CN120757814A