Modified asphalt for heavy-duty pavement and preparation method thereof
Through the combination of modified SBS and basalt fiber, the high-temperature stability and anti-aging properties of asphalt pavement are improved, and the aging problem of existing asphalt pavement during long-term service is solved. It is especially suitable for strong ultraviolet rays and heavy-load traffic conditions. The use of it extends the service life of the pavement and reduces maintenance costs.
Patent Information
- Application Number
- CN202411022527.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing asphalt pavements are prone to aging during long-term service, causing them to harden at high temperatures and become brittle at low temperatures, affecting their road performance. Especially under strong ultraviolet rays and heavy traffic conditions, maintenance costs are high.
A modified asphalt for heavy-duty pavement is used, which is composed of matrix asphalt, calcium carbonate, modified SBS, basalt fiber, furfural aromatic oil and sulfur. Through the preparation method of modified SBS, click reaction and esterification reaction are used to improve SBS. It has excellent UV resistance and aging resistance, and uses basalt fibers to form a network structure to enhance the adhesion of the asphalt mortar.
It improves the high-temperature stability, anti-rutting ability and anti-aging performance of asphalt mixture, prolongs the service life of the pavement, and reduces later maintenance costs.
Smart Images

Figure BDA0004967707700000101 
Figure BDA0004967707700000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of pavement materials, and in particular to modified asphalt for heavy-load pavement and a preparation method thereof. Background Art
[0002] my country's highway construction started in 1988. With the rapid economic development and industrialization, the total mileage of highways in my country has exceeded 177,000 kilometers, ranking first in the world. Asphalt pavement has the advantages of low noise, vibration reduction, wear resistance, comfortable driving, and convenient maintenance. It accounts for more than 95% of the mileage of highway construction and has become the most common type of pavement. However, due to the characteristics of high temperature softness, low temperature brittleness, and water dispersion of asphalt flexible pavement, coupled with the influence of complex climate environment and heavy traffic, asphalt pavement will age to varying degrees over time, prone to fatigue cracks, spalling, potholes and other problems, reducing driving comfort and service life. Surveys show that after 5 to 8 years of opening to traffic, asphalt pavement gradually ages due to the influence of ultraviolet light, thermal oxygen and other factors, the aging phenomenon of asphalt pavement becomes more severe. The pavement diseases mainly manifest as longitudinal cracks and network cracks on the road surface, which are generated on the road surface and gradually extend to the deep layer, causing structural damage. For highways that have been open to traffic for more than 8 years, milling and resurfacing due to aging and cracking of the pavement account for about 40% to 60% of the major and medium pavement repairs. Therefore, research on improving the anti-aging ability of pavement is related to promoting high-quality infrastructure construction, and is of great significance for extending the service life of asphalt pavement and building high-quality and long-life pavement.
[0003] Styrene-butadiene-styrene (SBS) block copolymers are most widely used in asphalt modification. When modifying asphalt, the styrene segment can play a role in skeleton cross-linking, improving the high-temperature stability of asphalt, and the butadiene segment can ensure that asphalt still has strong stress dissipation ability under low temperature conditions, improving the low-temperature ductility of asphalt.
[0004] Chinese patent document CN112646383A discloses a method for preparing a high-performance stable PPA and SBS composite modified asphalt, which includes the following raw materials: base asphalt, natural asphalt, vegetable asphalt, waste tire rubber powder, thermoplastic elastomer, modified calcium carbonate, modified sulfur, modified starch, organic acid, modified paraffin, hydroxypropyl methylcellulose, antioxidant, solubilizer, stabilizer, PPA polyphosphoric acid, SBS linear modifier. The invention solves the problem that the prepared composite modified asphalt has good high temperature, low temperature and adhesion properties.
[0005] However, whether it is the SBS modifier or the base asphalt, it is inevitable that aging will occur during long-term service due to the combined influence of factors such as temperature, sunlight, oxygen, and moisture. Due to the presence of unsaturated bonds, the aged SBS modifier is prone to bond breakage and degradation, which affects the modification effect between it and asphalt, and further affects the road performance of the asphalt mixture. After aging, the base asphalt will become hard and brittle, and it is very easy to crack under low temperature conditions, and the maintenance cost will rise sharply. Therefore, it is of great significance to comprehensively improve the rheological and anti-aging properties of SBS modified asphalt so that it still has ideal road performance after long-term service. Summary of the invention
[0006] In order to solve the shortcomings of the prior art, the purpose of the present invention is to provide a modified asphalt for heavy-load pavement and a preparation method thereof. The prepared modified asphalt has good high-temperature stability, strong anti-rutting ability and anti-aging performance, good durability, and low subsequent maintenance cost. It is particularly suitable for promotion and use in areas with strong ultraviolet rays and heavy traffic.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] A modified asphalt for heavy-load pavement is prepared from the following components by weight: 90-120 parts of base asphalt, 5-10 parts of calcium carbonate, 15-25 parts of modified SBS, 2-10 parts of basalt fiber, 3-6 parts of furfural aromatic oil and 1-5 parts of sulfur.
[0009] Preferably, it is made of the following components in parts by weight: 105 parts of base asphalt, 7.55 parts of calcium carbonate, 20 parts of modified SBS, 6 parts of basalt fiber, 4.5 parts of furfural aromatic oil, and 3 parts of sulfur.
[0010] Preferably, the preparation method of the modified SBS comprises the following steps:
[0011] (1) SBS and 12-mercaptododecanoic acid are added to cyclohexane, and after being stirred and dispersed evenly, azobisisobutyronitrile is added, and the mixture is stirred for reaction, and the product is filtered, washed, and dried to obtain carboxylated SBS;
[0012] (2) Carboxylated SBS and 2-(2'-hydroxy-5'-methylphenyl)benzotriazole are added to DMF, and then EDC·HCl is added for activation by stirring, and 4-dimethylaminopyridine is added for reaction by stirring, and the product is filtered, washed, and spin-dried to obtain the modified SBS.
[0013] Preferably, in step (1), the usage ratio of SBS, 12-mercaptododecanoic acid and cyclohexane is 10 g: 4-8 g: 50-100 mL.
[0014] Preferably, in step (1), the mass ratio of SBS to azobisisobutyronitrile is 10:0.05-0.15.
[0015] Preferably, in step (1), the stirring reaction condition is 45-60° C. for 10-16 hours.
[0016] Specifically, in step (1), the stirring reaction temperature can be 45°C, 47°C, 50°C, 52°C, 55°C, 57°C, 60°C, 62°C, or 65°C; and the stirring reaction time can be 10h, 11h, 12h, 13h, 14h, 15h, or 16h.
[0017] Preferably, in step (2), the usage ratio of carboxylated SBS, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole and DMF is 10 g: 8-16 g: 50-100 mL.
[0018] Preferably, in step (2), the mass ratio of carboxylated SBS, EDC·HCl, and 4-dimethylaminopyridine is 10:10-15:0.5-1.5.
[0019] Preferably, in step (2), the stirring reaction condition is stirring the reaction at room temperature for 18 to 24 hours.
[0020] Specifically, in step (2), the stirring reaction time can be 18h, 19h, 20h, 21h, 22h, 23h, or 24h.
[0021] Preferably, the basalt fiber has a diameter of 13 to 17 μm and a length of 10 to 30 mm.
[0022] Specifically, the diameter of the basalt fiber can be 13μm, 14μm, 15μm, 16μm, or 17μm; the length of the basalt fiber can be 10mm, 12mm, 14mm, 16mm, 18mm, 20mm, 22mm, 24mm, 26mm, 28mm, or 30mm.
[0023] The present invention also claims protection for a method for preparing the modified asphalt for heavy-load pavement, comprising the following steps: heating the base asphalt to 145-150°C, adding furfural aromatic oil and stirring evenly, then heating to 170-180°C, adding calcium carbonate, modified SBS, and basalt fiber in sequence, shearing for 30-50 minutes, and finally adding sulfur and shearing for 5-10 minutes to obtain the modified asphalt for heavy-load pavement.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1) The present invention provides a modified asphalt mixture for heavy-load pavement. Basalt fiber forms a network structure in the asphalt mortar, which can produce reinforcement and bridging effects, enhance the bonding force between the asphalt mortar and the aggregate, and improve the shear deformation resistance of the asphalt mixture. The modified SBS can improve the elasticity of the asphalt, improve the high and low temperature performance of the asphalt, and also has excellent UV resistance and aging resistance. The asphalt mixture prepared by the combination has good high-temperature stability, strong rutting resistance and aging resistance, good durability, and low later maintenance cost. It is particularly suitable for promotion and use in areas with strong ultraviolet rays and heavy traffic.
[0026] 2) The present invention provides a modified SBS. First, an alkyl acid is grafted onto the surface of SBS by utilizing a click reaction between an unsaturated double bond in SBS and a thiol group in 12-mercaptododecanoic acid to obtain a carboxylated SBS. Subsequently, EDC is used as a carboxyl activator and 4-dimethylaminopyridine is used as a catalyst to cause an esterification reaction between the carboxyl group in the carboxylated SBS and the hydroxyl group in 2-(2'-hydroxy-5'-methylphenyl)benzotriazole to obtain a modified SBS. The long-chain alkyl group in the mercaptoalkanoic acid is introduced into the surface of SBS, which increases the compatibility of SBS with an asphalt matrix and improves the chain entanglement between SBS and the polymer, thereby reducing the migration of SBS. rate. In addition, by reacting with the active double bonds in SBS, the activity of SBS is reduced, and its UV resistance and aging resistance are improved. 2-(2'-hydroxy-5'-methylphenyl)benzotriazole is used as a UV absorber and grafted onto the surface of SBS, which can further slow down the UV damage process and improve the anti-aging effect of the modified SBS. The modified SBS finally prepared improves the performance of SBS from the internal chemical structure, effectively solves its resistance to oxygen, ozone and ultraviolet light, and at the same time increases the polarity of SBS, improves the compatibility with asphalt mortar, can significantly improve the performance of asphalt mixture and extend the service life of the road surface. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiments. Of course, the specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.
[0028] Unless otherwise specified, the chemical reagents and materials in the present invention are purchased from commercial sources or synthesized from raw materials purchased from commercial sources.
[0029] The base asphalt model is Korean SK-70;
[0030] Calcium carbonate was purchased from Guangzhou Kaiju CA-800, which is 800 mesh heavy calcium carbonate with a specific surface area of 12300cm 2 / g;
[0031] Furfural aromatic oil was purchased from Hengshui Aoda Chemical Rubber Co., Ltd.;
[0032] Basalt fiber was purchased from Wuhan Qixing New Technology Materials Co., Ltd., with a compressive strength of ≥1050MPa;
[0033] SBS was purchased from Baling Petrochemical Co., Ltd., model YH-791.
[0034] A method for preparing a modified asphalt mixture for heavy-load pavement comprises the following steps:
[0035] (1) 10 g of SBS and 4-8 g of 12-mercaptododecanoic acid are added to 50-100 mL of cyclohexane, and after being stirred and dispersed evenly, 0.05-0.15 g of azobisisobutyronitrile is added, and the mixture is stirred and reacted at 45-60° C. for 10-16 h. The product is filtered, washed, and dried to obtain carboxylated SBS;
[0036] (2) 10 g of carboxylated SBS and 8-16 g of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole are added to 50-100 mL of DMF, followed by adding 10-15 g of EDC·HCl for stirring and activation, and then adding 0.5-1.5 g of 4-dimethylaminopyridine for stirring and reaction at room temperature for 18-24 h, filtering the product, removing EDC and unreacted products with deionized water, and spinning the DMF to obtain the modified SBS;
[0037] (3) 90 to 120 parts of base asphalt are heated to 145 to 150° C., 3 to 6 parts of furfural aromatic oil are added and stirred evenly, and then heated to 170 to 180° C., 5 to 10 parts of calcium carbonate, 15 to 25 parts of modified SBS, and 2 to 10 parts of basalt fiber are added in sequence, and the mixture is sheared for 30 to 50 minutes, and finally 1 to 5 parts of sulfur are added and sheared for 5 to 10 minutes to obtain the modified asphalt for heavy-load pavement.
[0038] The present invention will be further described below through specific embodiments.
[0039] Example 1
[0040] A method for preparing a modified asphalt mixture for heavy-load pavement comprises the following steps:
[0041] (1) 10 g of SBS and 8 g of 12-mercaptododecanoic acid were added to 100 mL of cyclohexane, and after being stirred and dispersed evenly, 0.15 g of azobisisobutyronitrile was added, and the mixture was stirred and reacted at 60° C. for 10 h. The product was filtered, washed, and dried to obtain carboxylated SBS;
[0042] (2) 10 g of carboxylated SBS and 16 g of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole were added to 100 mL of DMF, followed by addition of 15 g of EDC·HCl for activation by stirring, and then 1.5 g of 4-dimethylaminopyridine was added for stirring and reaction at room temperature for 18 h. The product was filtered, and EDC and unreacted products were removed with deionized water. The DMF was then dried to obtain the modified SBS.
[0043] (3) 105 kg of base asphalt was heated to 145° C., 4.5 kg of furfural aromatic oil was added and stirred evenly, then heated to 175° C., 7.5 kg of calcium carbonate, 25 kg of modified SBS, and 6 kg of basalt fiber were added in sequence, and sheared for 40 minutes. Finally, 3 kg of sulfur was added and sheared for 7.5 minutes to obtain the modified asphalt for heavy-load pavement.
[0044] Example 2
[0045] A method for preparing a modified asphalt mixture for heavy-load pavement comprises the following steps:
[0046] (1) 10 g of SBS and 6 g of 12-mercaptododecanoic acid were added to 100 mL of cyclohexane, and after being stirred and dispersed evenly, 0.12 g of azobisisobutyronitrile was added, and the mixture was stirred and reacted at 55° C. for 12 h. The product was filtered, washed, and dried to obtain carboxylated SBS;
[0047] (2) 10 g of carboxylated SBS and 14 g of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole were added to 100 mL of DMF, followed by addition of 14 g of EDC·HCl for activation by stirring, and then 1.2 g of 4-dimethylaminopyridine was added for stirring and reaction at room temperature for 20 h. The product was filtered, and EDC and unreacted products were removed with deionized water. The DMF was then dried to obtain the modified SBS.
[0048] (3) 105 kg of base asphalt was heated to 145° C., 4.5 kg of furfural aromatic oil was added and stirred evenly, then heated to 175° C., 7.5 kg of calcium carbonate, 20 kg of modified SBS, and 6 kg of basalt fiber were added in sequence, and sheared for 40 minutes. Finally, 3 kg of sulfur was added and sheared for 7.5 minutes to obtain the modified asphalt for heavy-load pavement.
[0049] Example 3
[0050] A method for preparing a modified asphalt mixture for heavy-load pavement comprises the following steps:
[0051] (1) 10 g of SBS and 6 g of 12-mercaptododecanoic acid were added to 100 mL of cyclohexane, and after being stirred and dispersed evenly, 0.11 g of azobisisobutyronitrile was added, and the mixture was stirred and reacted at 50° C. for 12 h. The product was filtered, washed, and dried to obtain carboxylated SBS;
[0052] (2) 10 g of carboxylated SBS and 12 g of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole were added to 100 mL of DMF, followed by adding 11 g of EDC·HCl for stirring and activation, and then adding 0.8 g of 4-dimethylaminopyridine for stirring and reaction at room temperature for 22 h. The product was filtered, and EDC and unreacted products were removed with deionized water. The DMF was then dried to obtain the modified SBS.
[0053] (3) 105 kg of base asphalt was heated to 145° C., 4.5 kg of furfural aromatic oil was added and stirred evenly, then heated to 175° C., 7.5 kg of calcium carbonate, 18 kg of modified SBS, and 6 kg of basalt fiber were added in sequence, and sheared for 40 minutes. Finally, 3 kg of sulfur was added and sheared for 7.5 minutes to obtain the modified asphalt for heavy-load pavement.
[0054] Example 4
[0055] A method for preparing a modified asphalt mixture for heavy-load pavement comprises the following steps:
[0056] (1) 10 g of SBS and 4 g of 12-mercaptododecanoic acid were added to 100 mL of cyclohexane, and after being stirred and dispersed evenly, 0.05 g of azobisisobutyronitrile was added, and the mixture was stirred and reacted at 45° C. for 16 h. The product was filtered, washed, and dried to obtain carboxylated SBS;
[0057] (2) 10 g of carboxylated SBS and 8 g of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole were added to 100 mL of DMF, followed by addition of 10 g of EDC·HCl for stirring and activation, and then 0.5 g of 4-dimethylaminopyridine was added for stirring and reaction at room temperature for 24 h. The product was filtered, and EDC and unreacted products were removed with deionized water. The DMF was then dried to obtain the modified SBS.
[0058] (3) 105 kg of base asphalt was heated to 145° C., 4.5 kg of furfural aromatic oil was added and stirred evenly, then heated to 175° C., 7.5 kg of calcium carbonate, 15 kg of modified SBS, and 6 kg of basalt fiber were added in sequence, and sheared for 40 minutes. Finally, 3 kg of sulfur was added and sheared for 7.5 minutes to obtain the modified asphalt for heavy-load pavement.
[0059] Comparative Example 1
[0060] A method for preparing a modified asphalt mixture comprises the following steps:
[0061] (1) 10 g of SBS and 8 g of 12-mercaptododecanoic acid were added to 100 mL of cyclohexane, and after being stirred and dispersed evenly, 0.15 g of azobisisobutyronitrile was added, and the mixture was stirred and reacted at 60° C. for 10 h. The product was filtered, washed, and dried to obtain carboxylated SBS;
[0062] (2) 105 kg of base asphalt was heated to 145° C., 4.5 kg of furfural aromatic oil was added and stirred evenly, then heated to 175° C., 7.5 kg of calcium carbonate, 25 kg of modified SBS, and 6 kg of basalt fiber were added in sequence, and sheared for 40 minutes. Finally, 3 kg of sulfur was added and sheared for 7.5 minutes to obtain the modified asphalt for heavy-load pavement.
[0063] Comparative Example 2
[0064] A method for preparing a modified asphalt mixture comprises the following steps:
[0065] 105 kg of base asphalt was heated to 145° C., 4.5 kg of furfural aromatic oil was added and stirred evenly, then heated to 175° C., 7.5 kg of calcium carbonate, 25 kg of SBS, and 6 kg of basalt fiber were added in sequence, and sheared for 40 minutes. Finally, 3 kg of sulfur was added and sheared for 7.5 minutes to obtain the modified asphalt for heavy-load pavement.
[0066] The modified asphalt prepared in Examples 1 to 4 and Comparative Examples 1 to 2 was subjected to a heat aging test. The asphalt film heating test of T0609-2011 in JTG E20-2011 "Test Procedure for Asphalt and Asphalt Mixtures for Highway Engineering" was performed, and the asphalt was aged at a temperature of 163°C for 10 hours. The ultraviolet aging test was performed on the above materials using an ultraviolet aging box, and the ultraviolet wavelength was 365nm and the intensity was 15mW / cm 2 , the aging temperature is 30℃ and the aging time is 120h.
[0067] The softening point, penetration and brittle point of the asphalt before and after aging were tested respectively. The penetration, softening point and brittle point tests of modified asphalt were tested with reference to T0604-2011 asphalt penetration test, T0606-2011 asphalt softening point test (ring and ball method) and T0613-1993 asphalt brittle point test (Flas method) in JTG E20-2011 "Test Procedures for Asphalt and Asphalt Mixtures for Highway Engineering".
[0068] The softening point increment, needle penetration residual ratio and brittle point change are calculated according to formula (1), formula (2) and formula (3). The smaller the softening point increment and brittle point change before and after aging, the larger the needle penetration residual ratio, and the better the aging resistance of the asphalt.
[0069] Softening point increment = softening point 老化后 - Softening point 老化前 (1);
[0070] Penetration Residual Ratio = (Penetration 老化后 / Needle Penetration 老化前 )×100%(2);
[0071] Brittle point change = Brittle point 老化后 - Crisp 老化前 (3).
[0072] The specific test results are shown in Table 1.
[0073] Table 1 Test results of modified asphalt aging performance
[0074]
[0075]
[0076] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A modified asphalt for heavy-load pavement, characterized in that: The invention is made of the following components in parts by weight: 90-120 parts of base asphalt, 5-10 parts of calcium carbonate, 15-25 parts of modified SBS, 2-10 parts of basalt fiber, 3-6 parts of furfural aromatic oil and 1-5 parts of sulfur.
2. The modified asphalt for heavy-duty pavement according to claim 1, characterized in that: The preparation method of the modified SBS comprises the following steps: (1) SBS and 12-mercaptododecanoic acid are added to cyclohexane, and after being stirred and dispersed evenly, azobisisobutyronitrile is added, and the mixture is stirred for reaction, and the product is filtered, washed, and dried to obtain carboxylated SBS; (2) Carboxylated SBS and 2-(2'-hydroxy-5'-methylphenyl)benzotriazole are added to DMF, and then EDC·HCl is added for activation by stirring, and 4-dimethylaminopyridine is added for reaction by stirring, and the product is filtered, washed, and spin-dried to obtain the modified SBS.
3. The modified asphalt for heavy-duty pavement according to claim 2, characterized in that: In step (1), the usage ratio of SBS, 12-mercaptododecanoic acid and cyclohexane is 10 g: 4-8 g: 50-100 mL.
4. The modified asphalt for heavy-duty pavement according to claim 2, characterized in that: In step (1), the mass ratio of SBS to azobisisobutyronitrile is 10:0.05-0.
15.
5. The modified asphalt for heavy-load pavement according to claim 2, characterized in that: In step (1), the stirring reaction conditions are 45-60° C. and 10-16 hours.
6. The modified asphalt for heavy-load pavement according to claim 2, characterized in that: In step (2), the usage ratio of carboxylated SBS, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole and DMF is 10 g: 8-16 g: 50-100 mL.
7. The modified asphalt for heavy-load pavement according to claim 2, characterized in that: In step (2), the mass ratio of carboxylated SBS, EDC·HCl, and 4-dimethylaminopyridine is 10:10-15:0.5-1.
5.
8. The modified asphalt for heavy-load pavement according to claim 2, characterized in that: In step (2), the stirring reaction condition is stirring the reaction at room temperature for 18 to 24 hours.
9. The modified asphalt for heavy-load pavement according to claim 1, characterized in that: The basalt fiber has a diameter of 13 to 17 μm and a length of 10 to 30 mm.
10. A method for preparing modified asphalt for heavy-duty pavement according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: heating the base asphalt to 145-150° C., adding furfural aromatic oil and stirring evenly, then heating to 170-180° C., sequentially adding calcium carbonate, modified SBS and basalt fiber, shearing for 30-50 minutes, and finally adding sulfur and shearing for 5-10 minutes to obtain the modified asphalt for heavy-load pavement.