Preparation method of conductive anticorrosive coating with brick-mud structure for aluminum surface

By preparing a brick-and-mud structural coating with a lamellar structure of highly conductive ceramic filler and a negatively charged aluminum matrix, the problem of balancing conductivity and corrosion resistance of the metal aluminum cable shielding layer is solved, achieving high conductivity and strong corrosion resistance. , has important application prospects.

CN118725616AActive Publication Date: 2024-10-01XIAN UNIV OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410774817.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-01
Estimated Expiration
2044-06-17

AI Technical Summary

Technical Problem

It is difficult to achieve an effective balance between conductivity and corrosion resistance on metal aluminum cable shielding layers with existing technology. Traditional coatings have limitations in conductivity and corrosion resistance and cannot meet the needs of metal aluminum cables.

Method used

A preparation method is adopted to prepare a highly conductive ceramic filler with a lamellar structure and a negatively charged aluminum matrix, combined with thermal curing treatment, to form a conductive anti-corrosion coating with a brick-mud structure. The strong interaction between the highly conductive ceramic filler and the negatively charged aluminum surface is used. Electrostatic attraction improves the conductivity and anti-corrosion properties of the coating.

Benefits of technology

It achieves high conductivity and good anti-corrosion properties, improves the bonding force between the coating and the substrate, and solves the problem that the existing coating cannot meet the balance between aluminum conductivity and corrosion resistance, and has important application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725616A_ABST
    Figure CN118725616A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a conductive anticorrosive coating with a brick-mud structure for an aluminum surface. The preparation method comprises the following steps: firstly, preparing a high-conductivity ceramic filler with a lamellar structure by controlling the content of added metal salt and urea and ball milling parameters; secondly, adding the high-conductivity ceramic filler, a defoaming agent and a flatting agent into a solvent, and performing ultrasonic treatment, oscillation and water bath treatment to obtain a ceramic coating; then, the surface of the metal aluminum material is negatively charged through alkaline solution etching, deionized water cleaning and polyanionic conductive polymer solution dipping treatment; and finally, the conductive ceramic coating is spin-coated on the surface of the metal aluminum material, and the conductive anticorrosive coating with the brick mud structure is obtained through thermocuring treatment. The high-conductivity ceramic filler with the lamellar structure in the coating is beneficial to improving the conductivity and uniformity of the ceramic coating, and through strong electrostatic attraction and thermocuring treatment with the surface of aluminum with negative charges, the subsequent coating process is promoted, a brick mud structure is formed, and the effects of high conductivity, good corrosion resistance and good binding force of the coating are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal surface coatings, and in particular relates to a method for preparing a conductive anti-corrosion coating with a brick-mud structure on an aluminum surface. Background Art

[0002] In today's industrial field, the corrosion resistance and electrical conductivity of metal materials are crucial. Especially in the field of electricity, metal aluminum cable shielding, as an important component of wires and cables, usually needs to have high conductivity and corrosion resistance to ensure the quality of electrical signal transmission and extend service life. At present, research on metal surface coatings mainly focuses on traditional organic coatings and metal electroplating, such as polymer coatings, chromate plating, etc. However, these traditional methods have limitations in conductivity and corrosion resistance, and it is difficult to meet the requirements of metal aluminum cable shielding. Therefore, it is imperative to study a new coating preparation method with unique structure, high conductivity and corrosion resistance.

[0003] The Chinese patent "A method for preparing a cathode protection composite conductive anti-corrosion coating on the surface of aluminum" (application number: 202410097473.1, publication number: CN118027808 A) discloses a method for preparing a cathode protection composite conductive anti-corrosion coating on the surface of aluminum. By utilizing the synergistic effect of anode sacrificial fillers, conductive anti-corrosion fillers, silane coupling agents and high molecular polymers, a directional anti-corrosion graphene layer is prepared in the coating, so that the coating has both conductive and anti-corrosion properties. However, the oxidation protection of the anode sacrificial filler is not conducive to conductivity and is not conducive to long-term protection.

[0004] The Chinese patent "A method for preparing a friction-resistant self-repairing conductive anti-corrosion coating and coating" (application number: 202410271528.6, publication number: CN118006195 A) discloses a method for preparing a friction-resistant self-repairing conductive anti-corrosion coating and coating. By adding highly conductive MXene and self-repairing microcapsules to the anti-corrosion coating, the anti-friction, self-repairing and anti-corrosion capabilities of the coating can be significantly improved. However, the titanium element in the two-dimensional MXene layer can absorb oxygen. When the titanium element is oxidized to form titanium dioxide particles to improve the anti-corrosion performance, the conductivity of the coating is weakened.

[0005] The Chinese patent "A modified polyurea-based conductive anti-corrosion coating, its preparation method and application" (application number: 202311627526.8, publication number: CN 117903669A) discloses a modified polyurea-based conductive anti-corrosion coating, its preparation method and application, by adding conductive carbon black as the main component, polyaniline and AZO as auxiliary conductive fillers, and using the amino groups carried by polyaniline and the amino functional groups introduced by modified AZO, which can be chemically grafted to the polyurea main chain during the curing process, so that the coating has better conductivity and adhesion, thereby improving the corrosion resistance of the coating. However, conductive carbon black is easy to agglomerate, causing the problem of poor bonding between the coating and the substrate. Summary of the invention

[0006] In view of the problems existing in the prior art, the present invention proposes a method for preparing a conductive anti-corrosion coating with a brick-mud structure on an aluminum surface, focusing on simultaneously improving the conductivity and corrosion resistance of the coating. The method is suitable for the protection of metal aluminum cable shielding layers, and solves the problem that traditional anti-corrosion coatings cannot meet the balance between the conductivity and corrosion resistance of metal aluminum cable shielding layers.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A method for preparing a conductive anti-corrosion coating with a brick-mud structure on an aluminum surface comprises the following steps:

[0009] Step 1, preparing a highly conductive ceramic filler having a lamellar structure;

[0010] The ceramic powder, metal salt, urea and grinding balls are mixed in proportion and subjected to ball milling treatment, and then dissolved in deionized water, dialyzed, centrifuged and vacuum dried to obtain a highly conductive ceramic filler with a lamellar structure;

[0011] Step 2, preparing a highly conductive ceramic coating;

[0012] The highly conductive ceramic filler with a lamellar structure, a defoamer and a leveling agent obtained in step 1 are added to a solvent, and subjected to ultrasonic, oscillation and water bath treatment to obtain a ceramic coating;

[0013] Step 3, negative charge treatment of the aluminum substrate surface;

[0014] The aluminum substrate is ultrasonically cleaned in an organic solvent, then etched with an alkaline solution, cleaned with deionized water, and immersed in a polyanionic conductive polymer solution to obtain an aluminum substrate with a negative charge;

[0015] Step 4, preparing a conductive anti-corrosion coating for a brick-mud structure;

[0016] The highly conductive ceramic coating obtained in step 2 is spin-coated on the negatively charged aluminum substrate obtained in step 3, and subjected to thermal curing treatment to obtain a conductive anti-corrosion coating for a brick-mud structure.

[0017] Furthermore, in terms of mass percentage, the amounts of the various materials in step 1 are: 15%-20% of ceramic powder, 1%-5% of metal salt, 30%-40% of urea and 40%-45% of grinding balls, and the total amount of the above materials is 100%.

[0018] Furthermore, the ceramic powder in step 1 is any one of Ti3AlC2, TiCr2C2, V2C, and MoAlB; the metal salt is any one of nickel chloride, cupric chloride, ferric chloride, and silver chloride; the grinding ball is silicon nitride with a diameter of 5-10 mm; the dialysis bag used in the dialysis has a molecular weight cutoff of 3500-4000, and the dialysis time is 6-12 h; the centrifugal speed is 3500-11000 rpm, and the centrifugal time is 15-30 min; the temperature of the vacuum drying treatment is 30-40°C, and the time is 5-10 h.

[0019] Furthermore, the ball milling treatment time in step 1 is 12-36 hours, and the ball milling speed is 400-1000 rpm.

[0020] Furthermore, in step 2, the mass ratio of the highly conductive ceramic filler, the defoaming agent, the leveling agent and the solvent is 1-3:0.1-0.5:0.1-0.5:3-5.

[0021] Furthermore, the defoaming agent in step 2 is any one of polyaniline, polystyrene sulfonate, and polyacrylamide; the leveling agent is any one of methyl methacrylate polymer, isopentyl 2-ethylhexanoate polymer, and perfluorooctyl vinyl ether polymer; and the solvent is any one of methyl pyrrolidone, dimethylformamide, and dimethyl sulfoxide.

[0022] Furthermore, in step 2, the ultrasonic and oscillation treatment time is 0.5-1h, and the water bath treatment temperature is 30-60°C for 1-5h.

[0023] Furthermore, the organic solvent in step 3 is any one of acetone and ethanol; the alkaline solution is any one of NaOH and KOH, and the concentration is 0.5-2.5 mol / L; the etching time is 10-60s; the polyanionic conductive polymer solution is any one of polystyrene sulfonate, polypropylene sulfonate, and polystyrene sulfonate solution, and the mass proportion of the polyanionic conductive polymer solution is 5-10%; the immersion time is 0.5-2h.

[0024] Furthermore, in step 4, the spin coating speed is 1000-2500 rpm; the thermal curing temperature is 80-120° C., and the thermal curing time is 1-10 h.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The present invention realizes a method for preparing a conductive anti-corrosion coating with a brick-mud structure on an aluminum surface, wherein a highly conductive ceramic filler with a lamellar structure is used to improve the conductivity and uniformity of the ceramic coating, and the subsequent coating process is promoted through strong electrostatic attraction and thermal curing treatment with a negatively charged aluminum surface, forming a "brick-mud structure" to achieve the beneficial effects of high conductivity, good corrosion resistance and good bonding of the coating. The conductive anti-corrosion coating prepared by the present invention solves the problem that the existing coating cannot meet the effective balance between aluminum conductivity and corrosion resistance, and has important application prospects in the shielding layer of metal aluminum cables. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a cross-sectional schematic diagram of a conductive anti-corrosion coating with a brick-mud structure prepared by the present invention;

[0028] In the attached figure, 1-highly conductive ceramic filler with lamellar structure; 2-polyanionic conductive polymer; 3-matrix aluminum. DETAILED DESCRIPTION

[0029] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0030] The theories or mechanisms described and disclosed herein should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0031] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0032] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”

[0033] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0034] The present invention provides a method for preparing a conductive anti-corrosion coating with a brick-mud structure on an aluminum surface, which specifically comprises the following steps:

[0035] Step 1, preparing a highly conductive ceramic filler having a lamellar structure;

[0036] 15%-20% ceramic powder, 1%-5% metal salt, 30%-40% urea and 40%-45% silicon nitride grinding balls are placed in a ball mill and subjected to ball milling treatment at a rotation speed of 400-1000rpm for 12-36h, then dissolved in deionized water, dialyzed in a dialysis bag with a molecular weight cutoff of 3500-4000 for 6-12h, centrifuged at a rotation speed of 3500-11000rpm for 15-30min, and vacuum dried at 30-40℃ for 5-10h to obtain a highly conductive ceramic filler with a lamellar structure; wherein the grinding ball has a diameter of 5-10mm, the total mass fraction of the ceramic powder, metal salt, urea and grinding ball is 100%, the ceramic powder is any one of Ti3AlC2, TiCr2C2, V2C and MoAlB, and the metal salt is any one of nickel chloride, cupric chloride, ferric chloride and silver chloride;

[0037] Step 2, preparing a highly conductive ceramic coating;

[0038] Add the lamellar highly conductive ceramic filler, defoamer and leveling agent in step 1 into the solvent, after ultrasonic and oscillation, place in a water bath for water bath treatment to obtain a ceramic coating. The mass ratio of the highly conductive ceramic filler, defoamer, leveling agent and solvent is 1-3: 0.1-0.5: 0.1-0.5: 3-10; the defoamer is any one of polyaniline, polystyrene sulfonate and polyacrylamide; the leveling agent is any one of methyl methacrylate polymer, 2-ethylhexanoate isopentyl polymer and perfluorooctyl vinyl ether polymer; the solvent is any one of methyl pyrrolidone, dimethylformamide and dimethyl sulfoxide; the ultrasonic and oscillation treatment time is 0.5-1h; the water bath treatment temperature is 30-60°C and the time is 1-5h;

[0039] Step 3: Negative charge treatment of the aluminum substrate surface

[0040] The aluminum substrate is ultrasonically cleaned in an organic solvent for 30 minutes, etched with an alkaline solution for 10-60 seconds, cleaned with deionized water, and immersed in a 5-10% polyanionic conductive polymer solution for 0.5-2 hours to obtain an aluminum substrate with a negative charge. The organic solvent is any one of acetone and ethanol; the alkaline solution is any one of NaOH and KOH, with a concentration of 0.5-2.5 mol / L; the polyanionic conductive polymer solution is any one of polystyrene sulfonate, polypropylene sulfonate, and polystyrene sulfonate solution;

[0041] Step 4: Preparation of conductive anti-corrosion coating for brick-mud structure

[0042] The highly conductive ceramic coating prepared in step 2 is spin-coated on the negatively charged aluminum substrate, and subjected to a heat curing treatment at 80-120° C. for 1-10 hours to obtain a conductive anti-corrosion coating for a brick-mud structure, wherein the spin-coating speed is 1000-2500 rpm.

[0043] Figure 1 It is a cross-sectional schematic diagram of the conductive anti-corrosion coating with a brick-mud structure prepared by the present invention. As can be seen from the figure, a conductive anti-corrosion coating is attached to the aluminum substrate 3, and the cross-section of the conductive anti-corrosion coating with a brick-mud structure is composed of a highly conductive ceramic filler 1 with a lamellar structure and a polyanionic conductive polymer 2 from top to bottom.

[0044] The method for preparing a conductive anticorrosion coating with a brick-mud structure on an aluminum surface disclosed in the present invention prepares a large number of highly conductive ceramic fillers with a lamellar structure by controlling the addition of metal salts, urea and high-energy ball milling time, which is beneficial to improving the conductive performance and uniformity of the coating. By etching the surface of an aluminum substrate and adjusting the concentration and immersion time of a polyanionic conductive polymer solution, an aluminum surface with a negative charge is obtained, which can realize a strong electrostatic assembly and combination with a highly conductive ceramic coating, fully improve the bonding force of the coating, and combined with a thermal curing treatment, a conductive anticorrosion coating with a brick-mud structure on an aluminum surface can be formed, realizing a high-quality coating with high conductivity, strong corrosion resistance and good uniformity.

[0045] A method for preparing a conductive anti-corrosion coating with a brick-mud structure on an aluminum surface, wherein a highly conductive ceramic filler with a lamellar structure is used to improve the conductivity and uniformity of the ceramic coating and promote the subsequent coating process. Through strong electrostatic attraction and thermal curing with the negatively charged aluminum surface, a "brick-mud structure" is formed, achieving the beneficial effects of high conductivity, good corrosion resistance and good bonding of the coating, solving the problem that existing coatings cannot meet the high balance of aluminum conductivity and corrosion resistance, and has important application prospects in metal aluminum cable shielding layers.

[0046] Example 1

[0047] A method for preparing a conductive anti-corrosion coating with a brick-mud structure on an aluminum surface comprises the following steps:

[0048] Step 1, preparing a highly conductive ceramic filler having a lamellar structure;

[0049] 20% Ti3AlC2, 5% nickel chloride, 30% urea and 45% silicon nitride grinding balls (with a diameter of 5 mm) were loaded into a ball mill, ball milled at a speed of 400 rpm for 36 hours, dissolved in deionized water, dialyzed for 6 hours in a dialysis bag with a molecular weight cutoff of 3500, centrifuged twice at a speed of 3500 rpm for 30 minutes, and vacuum dried at 30°C for 10 hours to obtain a highly conductive ceramic filler with a lamellar structure;

[0050] Step 2, preparing a highly conductive ceramic coating;

[0051] The lamellar highly conductive ceramic filler, polyaniline, methyl methacrylate polymer and methyl pyrrolidone in step 1 are mixed in a mass ratio of 1:0.1:0.1:10, subjected to ultrasound and vibration for 0.5 h, placed in a water bath, and subjected to water bath treatment at 30° C. for 5 h to obtain a ceramic coating;

[0052] Step 3, negative charge treatment of the aluminum substrate surface;

[0053] The aluminum substrate was ultrasonically cleaned in acetone for 30 min, etched with 0.5 mol / L NaOH solution for 60 s, washed with deionized water, and immersed in 5% polystyrene sulfonate solution for 0.5 h to obtain an aluminum substrate surface with negative charge;

[0054] Step 4: Preparation of conductive anti-corrosion coating for brick-mud structure

[0055] The rotary coating speed was controlled to be 1000 rpm, and the highly conductive ceramic coating prepared in step 2 was coated on the surface of the negatively charged aluminum substrate. After heat curing at 80° C. for 10 h, a conductive anti-corrosion coating for a brick mud structure was obtained.

[0056] Example 2

[0057] A method for preparing a conductive anti-corrosion coating with a brick-mud structure on an aluminum surface comprises the following steps:

[0058] Step 1, preparing a highly conductive ceramic filler having a lamellar structure;

[0059] 20% TiCr2C2, 1% copper chloride, 34% urea and 45% silicon nitride grinding balls (10 mm in diameter) were loaded into a ball mill, milled at a speed of 1000 rpm for 12 h, dissolved in deionized water, dialyzed in a dialysis bag with a molecular weight cutoff of 4000 for 12 h, centrifuged twice at a speed of 11000 rpm for 15 min, and vacuum dried at 40°C for 8 h to obtain a highly conductive ceramic filler with a lamellar structure;

[0060] Step 2, preparing a highly conductive ceramic coating;

[0061] The lamellar highly conductive ceramic filler, polystyrene sulfonate, 2-ethylhexanoate polymer and dimethylformamide in step 1 are mixed in a mass ratio of 3:0.5:0.5:8, subjected to ultrasound and vibration for 1 hour, placed in a water bath, and subjected to water bath treatment at 60°C for 1 hour to obtain a ceramic coating;

[0062] Step 3: Negative charge treatment of the aluminum substrate surface

[0063] The aluminum substrate was ultrasonically cleaned in ethanol for 30 min, etched in 2.5 mol / L NaOH solution for 10 s, washed with deionized water, and immersed in 8% polypropylene sulfonate solution for 0.5 h to obtain an aluminum substrate surface with negative charge;

[0064] Step 4: Preparation of conductive anti-corrosion coating for brick-mud structure

[0065] The rotary coating speed was controlled to be 2500 rpm, and the highly conductive ceramic coating prepared in step 2 was coated on the surface of the negatively charged aluminum substrate. After heat curing at 120° C. for 1 h, a conductive anti-corrosion coating for a brick mud structure was obtained.

[0066] Example 3

[0067] Step 1, preparing a highly conductive ceramic filler having a lamellar structure;

[0068] 15% V2C, 5% ferric chloride, 40% urea and 40% silicon nitride grinding balls (with a diameter of 8 mm) were loaded into a ball mill, ball milled at a speed of 800 rpm for 24 hours, dissolved in deionized water, dialyzed with a dialysis bag with a molecular weight cutoff of 3800 for 8 hours, centrifuged twice at a speed of 8000 rpm for 20 minutes and vacuum dried at 35°C for 10 hours to obtain a highly conductive ceramic filler with a lamellar structure;

[0069] Step 2, preparing a highly conductive ceramic coating;

[0070] The lamellar highly conductive ceramic filler, polyacrylamide, perfluorooctyl vinyl ether polymer and dimethyl sulfoxide in step 1 are mixed in a mass ratio of 2:0.3:0.3:3, subjected to ultrasound and vibration for 0.8 hours, placed in a water bath, and subjected to water bath treatment at 40°C for 3 hours to obtain a ceramic coating;

[0071] Step 3: Negative charge treatment of the aluminum substrate surface

[0072] The aluminum substrate was ultrasonically cleaned in ethanol for 30 min, etched in 2 mol / L NaOH solution for 30 s, washed with deionized water, and immersed in 10% polypropylene sulfonate solution for 1 h to obtain an aluminum substrate surface with negative charge;

[0073] Step 4: Preparation of conductive anti-corrosion coating for brick-mud structure

[0074] The rotary coating speed was controlled to be 1500 rpm, and the highly conductive ceramic coating prepared in step 2 was coated on the surface of the negatively charged aluminum substrate. After thermal curing at 100° C. for 3 h, a conductive anti-corrosion coating for a brick mud structure was obtained.

[0075] Example 4

[0076] A method for preparing a conductive anti-corrosion coating with a brick-mud structure on an aluminum surface comprises the following steps:

[0077] Step 1, preparing a highly conductive ceramic filler having a lamellar structure;

[0078] 18% MoAlB, 3% silver chloride, 37% urea and 42% silicon nitride grinding balls (with a diameter of 5 mm) were loaded into a ball mill, ball milled at a speed of 600 rpm for 36 hours, dissolved in deionized water, dialyzed in a dialysis bag with a molecular weight cutoff of 4000 for 10 hours, centrifuged twice at a speed of 600 rpm for 30 minutes and vacuum dried at 40°C for 5 hours to obtain a highly conductive ceramic filler with a lamellar structure;

[0079] Step 2, preparing a highly conductive ceramic coating;

[0080] The lamellar highly conductive ceramic filler, polyaniline, methyl methacrylate polymer and methyl pyrrolidone in step 1 are mixed in a mass ratio of 2:0.2:0.3:5, subjected to ultrasound and vibration for 0.5 h, placed in a water bath, and subjected to water bath treatment at 60° C. for 3 h to obtain a ceramic coating;

[0081] Step 3: Negative charge treatment of the aluminum substrate surface

[0082] The aluminum substrate was ultrasonically cleaned in acetone for 30 min, etched with 1 mol / L KOH solution for 20 s, washed with deionized water, and immersed in 6% polystyrene sulfonate solution for 2 h to obtain an aluminum substrate surface with negative charge;

[0083] Step 4: Preparation of conductive anti-corrosion coating for brick-mud structure

[0084] The rotary coating speed was controlled to be 2000 rpm, and the highly conductive ceramic coating prepared in step 2 was coated on the surface of the negatively charged aluminum substrate. After heat curing at 70° C. for 10 h, a conductive anti-corrosion coating for a brick mud structure was obtained.

[0085] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing a conductive anti-corrosion coating with a brick-mud structure on an aluminum surface, characterized in that: The following steps are involved: Step 1, preparing a highly conductive ceramic filler having a lamellar structure; The ceramic powder, metal salt, urea and grinding balls are mixed in proportion and subjected to ball milling treatment, and then dissolved in deionized water, dialyzed, centrifuged and vacuum dried to obtain a highly conductive ceramic filler with a lamellar structure; Step 2, preparing a highly conductive ceramic coating; The highly conductive ceramic filler with a lamellar structure, a defoamer and a leveling agent obtained in step 1 are added to a solvent, and subjected to ultrasonic, oscillation and water bath treatment to obtain a ceramic coating; Step 3, negative charge treatment of the aluminum substrate surface; The aluminum substrate is ultrasonically cleaned in an organic solvent, then etched with an alkaline solution, cleaned with deionized water, and immersed in a polyanionic conductive polymer solution to obtain an aluminum substrate with a negative charge; Step 4, preparing a conductive anti-corrosion coating for a brick-mud structure; The highly conductive ceramic coating obtained in step 2 is spin-coated on the negatively charged aluminum substrate obtained in step 3, and subjected to thermal curing treatment to obtain a conductive anti-corrosion coating for a brick-mud structure.

2. The method for preparing a conductive anti-corrosion coating with a brick-mud structure on an aluminum surface according to claim 1, characterized in that: In terms of mass percentage, the amount of each material in step 1 is: ceramic powder 15%-20%, metal salt 1%-5%, urea 30%-40% and grinding ball 40%-45%, and the total of the above materials is 100%.

3. A method for preparing a conductive anti-corrosion coating with a brick-mud structure on an aluminum surface according to any one of claims 1 or 2, characterized in that: The ceramic powder in step 1 is any one of Ti3AlC2, TiCr2C2, V2C, and MoAlB; the metal salt is any one of nickel chloride, cupric chloride, ferric chloride, and silver chloride; the grinding ball is silicon nitride with a diameter of 5-10 mm; the dialysis bag used in the dialysis has a molecular weight cutoff of 3500-4000, and the dialysis time is 6-12 h; the centrifugal speed is 3500-11000 rpm, and the centrifugal time is 15-30 min; the temperature of the vacuum drying treatment is 30-40°C, and the time is 5-10 h.

4. The method for preparing a conductive anti-corrosion coating with a brick-mud structure on an aluminum surface according to claim 1, characterized in that: The ball milling treatment time in step 1 is 12-36 hours, and the ball milling speed is 400-1000rpm.

5. The method for preparing a conductive anti-corrosion coating with a brick-mud structure on an aluminum surface according to claim 1, characterized in that: The mass ratio of the highly conductive ceramic filler, defoamer, leveling agent and solvent in step 2 is 1-3:0.1-0.5:0.1-0.5:3-5.

6. A method for preparing a conductive anti-corrosion coating with a brick-mud structure on an aluminum surface according to any one of claims 1 or 5, characterized in that: The defoaming agent in step 2 is any one of polyaniline, polystyrene sulfonate, and polyacrylamide; the leveling agent is any one of methyl methacrylate polymer, isopentyl 2-ethylhexanoate polymer, and perfluorooctyl vinyl ether polymer; and the solvent is any one of methyl pyrrolidone, dimethylformamide, and dimethyl sulfoxide.

7. The method for preparing a conductive anti-corrosion coating with a brick-mud structure on an aluminum surface according to claim 1, characterized in that: The ultrasonic and oscillation treatment time in step 2 is 0.5-1h, and the water bath treatment temperature is 30-60°C for 1-5h.

8. The method for preparing a conductive anti-corrosion coating with a brick-mud structure on an aluminum surface according to claim 1, characterized in that: The organic solvent in step 3 is any one of acetone and ethanol; the alkaline solution is any one of NaOH and KOH, and the concentration is 0.5-2.5 mol / L; the etching time is 10-60s; the polyanionic conductive polymer solution is any one of polystyrene sulfonate, polypropylene sulfonate, and polystyrene sulfonate solution, and the mass proportion of the polyanionic conductive polymer solution is 5-10%; the immersion time is 0.5-2h.

9. The method for preparing a conductive anti-corrosion coating with a brick-mud structure on an aluminum surface according to claim 1, characterized in that: The spin coating speed in step 4 is 1000-2500 rpm; the thermal curing temperature is 80-120° C., and the thermal curing time is 1-10 h.

Citation Information

Patent Citations

  • Nanoceramic anticorrosive water-based paint

    CN113045976A

  • Method for in-situ growth of coating on aluminum surface, aluminum foil, aluminum-based current collector, electrode and battery

    CN116732515A

  • Preparation method of cathode protection type composite conductive anticorrosive coating on surface of aluminum material

    CN118027808A

  • KR20190078333A