Antibacterial printing coating and preparation method thereof, and antibacterial coating structure and preparation method thereof
By using precious metal coordination compounds and organic acids as antibacterial additives in antibacterial inks, and combining polyester-polyamide block polymer materials as dispersants, the problem of long-lasting antibacterial effects of antibacterial inks at room temperature is solved, and the ink is realized Highly effective antibacterial properties.
Patent Information
- Application Number
- CN202410711051.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-03
AI Technical Summary
It is difficult for existing antibacterial inks to achieve long-lasting antibacterial effects at room temperature, and the dispersion effect of antibacterial additives in the ink is poor, which affects the antibacterial performance of printed matter.
Coordination compounds containing precious metals and organic acids are used as antibacterial additives, and polyester-polyamide mixed block polymer materials are used as dispersants. By controlling the heating temperature and dispersant ratio, the antibacterial additives are uniformly dispersed and dispersed in the ink. stability, forming a protective layer to enhance antimicrobial properties.
It achieves long-term antibacterial effect at normal temperature, improves the surface antibacterial performance of antibacterial ink, and ensures that printed matter maintains a high antibacterial effect for a long time.
Smart Images

Figure CN118725641A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of combined coatings, and in particular to an antibacterial printed coating and a preparation method thereof, an antibacterial coating structure and a preparation method thereof. Background Art
[0002] Ink and varnish are commonly used printing coatings. Ink is used to display patterns and texts on substrates through printing or spraying, and varnish is used to enhance the appearance of printed products and can provide gloss, protection, friction resistance and decorative effects for printed products.
[0003] Since printed materials are often transferred and delivered multiple times, such as express delivery, it takes a long time and changes hands from the time the printing is completed to the time it reaches the customer. In this case, people expect the surface of the printed materials to have antibacterial effects, so antibacterial inks came into being.
[0004] Antibacterial ink is a kind of ink prepared by adding antibacterial agent to ink. In view of the fact that the substrate printed with ink is used at room temperature and in view of the above-mentioned long-term antibacterial demand, there is a need for an ink that can have long-term antibacterial effect at room temperature and has good antibacterial effect. Summary of the invention
[0005] An object of the present invention is to provide an antibacterial printing coating which can have a long-term antibacterial effect at room temperature and has a good antibacterial effect.
[0006] In particular, an embodiment of the present invention provides an antibacterial printing coating, comprising the following components in weight percentage: 55-80% coating main material, 2-10% antibacterial additive and 15-40% dispersant;
[0007] The antibacterial additive comprises a coordination compound containing a noble metal and an organic acid, and the density of the antibacterial additive is less than the density of the main coating material;
[0008] The dispersant comprises a polyester-polyamide mixed block polymer material, the polyester block of the dispersant is dissolved in the base oil of the main coating material, and the polyamide block of the dispersant is adsorbed on the surface of the coordination compound containing precious metals of the antibacterial additive.
[0009] Optionally, the dispersant is prepared by copolymerization of fatty acid, lactone compound, hydroxy acid, lactam compound and polyamine.
[0010] Optionally, the antibacterial printing coating is an antibacterial ink, and the antibacterial ink comprises the following components in weight percentage: 60-78% of a coating main body material, 7-10% of an antibacterial additive, and 15-25% of a dispersant.
[0011] Optionally, the antibacterial printing coating is an antibacterial varnish, and the antibacterial varnish comprises the following components in weight percentage: 55-78% of coating main material, 2-8% of antibacterial additive and 20-40% of dispersant.
[0012] In particular, an embodiment of the present invention further provides a method for preparing the antibacterial printing coating described in any one of the above, comprising the following steps:
[0013] The base oil of the coating main material is heated to any value between 40°C and 100°C;
[0014] Adding 15-40% by weight of the dispersant to the base oil, stirring, and keeping warm for 8-15 minutes until the dispersant is completely dissolved;
[0015] Adding 2-10% by weight of the antibacterial additive and stirring until the antibacterial agent is dispersed into a transparent state to form an antibacterial base oil;
[0016] The other materials in the main coating material are mixed with the antibacterial base oil and stirred.
[0017] In particular, an embodiment of the present invention further provides an antibacterial coating structure, including an ink layer, wherein the material of the ink layer includes the above-mentioned antibacterial ink.
[0018] Optionally, the antibacterial coating structure further comprises a varnish layer coated on the surface of the ink layer, and the material of the varnish layer comprises the above-mentioned antibacterial varnish.
[0019] In particular, an embodiment of the present invention further provides a method for preparing the above-mentioned antibacterial coating structure, comprising:
[0020] Coating the antibacterial ink on the surface of the substrate to be printed to form the ink layer;
[0021] The antibacterial varnish is coated on the ink layer after a preset time to form the varnish layer, wherein the preset time is 60-90% of the drying time of the ink layer.
[0022] Optionally, the preset time is 70-80% of the drying time of the ink layer.
[0023] According to the first aspect of the present invention, the dispersant includes a polyester block and a polyamide block, wherein the polyamide block portion can be firmly adsorbed on the surface of the coordination compound containing precious metals of the antibacterial additive, the polyester portion can be well dissolved in the base oil in the ink, and the polymer long chain extends into the base oil. This dispersant can form a protective layer of a certain thickness on the surface of the antibacterial additive particles, reduce the interfacial tension between the two phases, increase wettability, and improve the dispersion stability of the antibacterial additive particles in the base oil. In addition, since the density of the antibacterial additive is less than the density of the main material of the coating, it is possible to avoid precipitation of the antibacterial additive during printing, so that the antibacterial additive particles are adsorbed and dispersed by the dispersant while the antibacterial additive is as much as possible on the surface of the entire antibacterial printing coating, thereby maintaining a high antibacterial performance.
[0024] Furthermore, this embodiment takes into account factors such as the fact that the antibacterial additive particles have a relatively large proportion of small-sized particles, irregular shapes, and are hollow or have holes, and appropriately increases the amount of dispersant. The final proportion of dispersant is determined to be 15-40%, which has a better dispersion effect.
[0025] According to the second aspect of the present invention, the dispersing effect of the dispersant can be ensured by controlling the heating temperature of the base oil to between 40-100°C. This is because if the temperature is too low, the viscosity of the base oil will be too high, and too many bubbles will be generated during stirring, while if the temperature is too high, the dispersant will decompose and the dispersing effect will be lower. In addition, if the temperature is too high, the viscosity of the base oil will be lower, which will affect the dispersing effect of the antibacterial additive.
[0026] Furthermore, the dispersant is first evenly dispersed in the base oil, and then the antibacterial additive is added, that is, the antibacterial additive is added after the dispersant itself is evenly distributed. Since the dispersant itself is a multi-block material with a high viscosity, if the dispersant and the antibacterial additive are added to the base oil at the same time, it will cause the molecular chains to be entangled, resulting in poor dispersion effect of the antibacterial additive. In other words, by adding the dispersant and the antibacterial additive to the base oil in two steps, the dispersion effect of the antibacterial additive can be further guaranteed.
[0027] According to the third aspect of the present invention, the antibacterial coating structure includes an ink layer and a varnish layer both of which have antibacterial additives, so the content of the antibacterial additives is higher. On the basis of the varnish layer continuing to play an antibacterial role, even if the varnish layer consumes part of the antibacterial additives due to factors such as friction, the underlying ink layer can still play an antibacterial role, and because the density of the antibacterial additives is set to be smaller than the density of the main material of the coating, the antibacterial additives in the ink layer and the varnish layer can be at the upper surface, thereby enhancing the surface antibacterial effect of the structure.
[0028] Furthermore, the connection between the components in the ink layer is manifested in that the dispersant absorbs part of the antibacterial additives, which are dispersed in the antibacterial ink, and other antibacterial additives will be more concentrated on the surface of the ink layer. The antibacterial additives on the surface of this part of the ink layer can be adsorbed by the excess dispersant in the varnish layer, which forms a binding force between the ink layer and the varnish layer, increasing the adhesion of the varnish layer on the ink layer. At the same time, the antibacterial additives in the ink layer are partially bonded to the varnish layer, so that the entire varnish layer has more antibacterial additives, thereby enhancing the antibacterial properties of the antibacterial coating structure.
[0029] According to the fourth aspect of the present invention, coating a varnish layer when the ink layer is more than half dry but not completely dry can, on the one hand, prevent as much as possible the small molecule antibacterial additives in the varnish layer from penetrating through the ink layer to the surface of the substrate and reducing the antibacterial effect; on the other hand, it can also ensure that the dispersant in the varnish layer can be effectively adsorbed with the antibacterial additives in the ink layer, so that the antibacterial coating structure achieves a better antibacterial effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 A flow chart showing a method for preparing an antibacterial printed coating according to an embodiment of the present invention is shown;
[0031] Figure 2 A flow chart showing a method for preparing an antibacterial coating structure according to an embodiment of the present invention is shown;
[0032] Figure 3 A diagram showing the antibacterial additive dispersion effect of the antibacterial ink according to Example 1 of the present invention is shown;
[0033] Figure 4 The antibacterial additive dispersion effect diagram of the antibacterial ink of Comparative Example 6 is shown. DETAILED DESCRIPTION
[0034] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. It is to be understood that the specific embodiments described herein are only used to explain the present application, rather than to limit the present application. It should also be noted that, for ease of description, only some structures related to the present application are shown in the accompanying drawings, rather than all structures. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0035] The terms "including" and "having" and any variations thereof in this application are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device comprising a series of steps or units is not limited to the listed steps or units, but may optionally include steps or units not listed, or may optionally include other steps or units inherent to these processes, methods, products or devices.
[0036] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0037] When preparing ink with antibacterial properties, the inventor used an organic acid antibacterial agent containing a coordination compound of a precious metal in order to make the ink have long-term antibacterial properties at room temperature. The organic acid in this type of antibacterial agent can play a bactericidal role, and the coordination compound containing the precious metal can continuously catalyze the organic acid, so that the organic acid can achieve long-term antibacterial properties at room temperature and under the condition of low concentration. However, when the antibacterial agent is directly dispersed in the ink, it is found that the proportion of the antibacterial agent in the ink is less than 1%, and the dispersion effect is poor. In order to improve the dispersion effect of the antibacterial agent, the inventor added some alcohols, ketones and ester dispersants commonly used in inks to the ink, but the dispersion effect is poor. The inventor also experimented with some polyether-type, polyacrylate-type and their mixed block-type polymer materials as dispersants. The experimental results show that after adding the dispersant, the proportion of the antibacterial agent in the ink is still less than 1%. In order to make the antibacterial agent better dispersed in the ink, the present application provides the following embodiments.
[0038] One embodiment of the present invention provides an antibacterial printing coating, comprising the following components in weight percentage: 55-80% coating main material, 2-10% antibacterial additive and 15-40% dispersant. Specifically, the weight percentage of the coating main material can be, for example, 55%, 65%, 70%, 75% or 80%, or any other value between 55 and 80%. The weight percentage of the antibacterial additive can be, for example, 2%, 3%, 5%, 8% or 10%, or any other value between 2 and 10%. The weight percentage of the dispersant can be, for example, 15%, 17%, 20%, 25% or 40%, or any other value between 15 and 40%.
[0039] The main materials of the coating include base oil, pigment, resin binder, filler, additives, etc. The base oil may include mineral oil and / or vegetable oil. The pigment may be an organic pigment or an inorganic pigment. The resin binder may include colloid oil and / or resin oil. The filler may be, for example, nano calcium carbonate, barium sulfate or kaolin, which functions to change the density of the main materials of the coating. The additives include anti-friction agents, desiccants, etc.
[0040] The antimicrobial additive includes a coordination compound containing a noble metal and an organic acid, and the density of the antimicrobial additive is less than the density of the main coating material. The coordination compound containing a noble metal is a coordination compound formed by a noble metal ion and an organic molecule. The noble metal may be, for example, silver, gold, copper, zinc or platinum. The organic molecule may be, for example, C7H 15 N3、C6H 13 N3、C8H 17 N3 or other organic molecules containing only C, H and N elements. The coordination compound containing the noble metal may be, for example, Pt·C7H 15 N3、Pt·C6H 13 N3、Au·C8H 17 N3, etc. The organic acid may be, for example, citric acid, succinic acid, acetic acid, malic acid or acetic acid. In some embodiments, the organic acid may be, for example, citric acid, malic acid, or a combination of the two. For example, the organic acid may include 97% to 98% citric acid by weight and 0.6% to 1% malic acid by weight.
[0041] The dispersant is a polyester-polyamide mixed block polymer material. The polyester block of the dispersant is dissolved in the base oil of the main material of the coating. The polyamide block of the dispersant interacts with the organic ligand in the coordination compound through hydrogen bonds, van der Waals forces or other interaction forces, thereby combining with the precious metal in the coordination compound.
[0042] In some embodiments, the dispersant is prepared by the following steps:
[0043] Step 1, adding fatty acid, lactone compound, hydroxy acid and lactam compound into a reaction container according to a preset ratio, and adding an appropriate amount of stannous octoate catalyst;
[0044] Step 2: introducing an inert gas into the reaction vessel and heating the reaction vessel to 160° C.-200° C. and keeping the temperature for 10 h-14 h;
[0045] Step 3, cooling the reaction container to room temperature, and pouring the reaction product into excess cold methanol or ethanol to precipitate the polymer;
[0046] Step 4, washing the precipitated first polymer with a cold solvent to remove unreacted monomers and catalyst residues;
[0047] Step 5, drying the washed first polymer in a vacuum drying oven;
[0048] Step 6, adding the first polymer and the polyamine into a reaction container according to a certain proportion, and adding an appropriate amount of toluenesulfonic acid catalyst;
[0049] Step 7, heating the reaction vessel to 120°C-160°C, and keeping the temperature under protective gas for 4h-6h;
[0050] Step 8, cooling the reaction vessel to room temperature;
[0051] Step nine, pouring the reaction product into a cold solvent to precipitate a second polymer;
[0052] Step 10, washing the precipitated second polymer with a cold solvent to remove unreacted monomers and catalyst residues;
[0053] Step eleven, drying the washed second polymer in a vacuum drying oven to finally prepare a dispersant.
[0054] The fatty acid in step 1 can be, for example, stearic acid, palmitic acid, oleic acid, octadecanoic acid, lauric acid, myristic acid, erucic acid, caprylic acid or caproic acid. The lactone compound can be, for example, caprylic acid, caprolactone, methyl caprolactone or other lactone substitutes. The hydroxy acid can be, for example, hydroxystearic acid, hydroxyoleic acid, hydroxycaproic acid or hydroxypalmitic acid. The lactam compound can be, for example, propiolactam, butyrolactam, caprolactam, ethylene lactam or caprolactam substitutes.
[0055] The heating temperature in step 2 can be 160°C, 180°C, 190°C or 200°C, or any other value between 160°C and 200°C, and the insulation time can be 10h, 11h, 12h or 14h, or any other value between 10h and 14h.
[0056] The drying temperature in step five can be any value between 40°C and 60°C, for example, the drying temperature is 40°C, 50°C, or 60°C, and the drying time can be any value between 12h and 24h, for example, the drying time is 12h, 14h, 16h, 18h, 20h, 22h or 24h.
[0057] The polyamine in step six can be, for example, ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, other polyethylenepolyamines or polypropylenepolyamines.
[0058] The heating temperature in step seven can be 120°C, 140°C, 150°C or 160°C, or any other value between 120°C and 160°C, and the insulation time can be 4h, 5h, 5.5h or 6h, or any other value between 4h and 6h.
[0059] The cold solvent in step nine can be ethanol or acetone.
[0060] The drying temperature in step eleven can be any value between 40°C and 60°C, for example, the drying temperature is 40°C, 50°C, or 60°C, and the drying time can be any value between 24h and 48h, for example, the drying time is 24h, 26h, 30h, 32h, 36h, 40h or 48h.
[0061] In the above preparation process, fatty acids, lactone compounds, hydroxy acids and lactam compounds copolymerize to generate copolymers containing ester bonds and amide bonds, and the copolymers containing ester bonds and amide bonds undergo amidation reaction with polyamines to generate high molecular polymers of polyester and polyamide blocks, namely the above dispersant.
[0062] The reaction principle of the above dispersant is shown in the following reaction formulas (1) and (2):
[0063]
[0064] In formula (1) and (2), R1 is a C6-C17 alkyl or olefin group. For example, when R1 is CH3(CH2) 16 When R2 is C3-C7 alkyl or a substituent thereof, for example, when R2 is (CH2)5, it is caprolactone. R3 is C3-C17 alkyl or olefin group, for example, when R3 is (CH2)5, it is hydroxycaproic acid. R4 is C3-C5 alkyl, for example, when R4 is (CH2)5, it is caprolactam. R5 is H or CH3 alkyl or olefin group, for example, when R5 is H, it is polyethylene polyamine. The product of formula (2) is a dispersant, wherein the p and k parts are polyamide blocks, and the n and m parts are polyester blocks.
[0065] The dispersant in this embodiment includes polyester blocks and polyamide blocks, wherein the polyamide block portion can be firmly adsorbed on the surface of the coordination compound containing precious metals of the antibacterial additive, the polyester portion can be well dissolved in the base oil in the ink, and the polymer long chain extends into the base oil. This dispersant can form a protective layer of a certain thickness on the surface of the antibacterial additive particles, reduce the interfacial tension between the two phases, increase wettability, and improve the dispersion stability of the antibacterial additive particles in the base oil. In addition, since the density of the antibacterial additive is less than the density of the main material of the coating, the precipitation of the antibacterial additive during printing can be avoided, so that the antibacterial additive particles are adsorbed and dispersed by the dispersant, and the antibacterial additive is as much as possible on the surface of the entire antibacterial printing coating, thereby maintaining a high antibacterial performance.
[0066] Furthermore, this embodiment takes into account factors such as the fact that the antibacterial additive particles have a relatively large proportion of small-sized particles, irregular shapes, and are hollow or have holes, and appropriately increases the amount of dispersant. The final proportion of dispersant is determined to be 15-40%, which has a better dispersion effect.
[0067] In one embodiment, the coating main material includes a resin binder, the resin binder includes resin oil and gum oil, the resin oil includes rosin-modified phenolic resin and vegetable oil, and the gum oil includes rosin-modified phenolic resin, vegetable oil and a gelling agent. In one embodiment, the rosin-modified phenolic resin includes the following components in weight percentage: 55.42% rosin, 20.08% octylphenol, 20.10% formaldehyde, 4.21% glycerol and 0.19% PTS catalyst, and the preparation method of the rosin-modified phenolic resin includes:
[0068] Add rosin into the reactor and heat it to 150°C, then add octylphenol and formaldehyde;
[0069] Heat to 200-210°C for addition reaction for 1.5h;
[0070] After the addition, glycerol and PTS catalyst were added;
[0071] Heating to 250-280°C for esterification reaction for 6-8h;
[0072] Take samples to test the acid value and viscosity. The acid value is ≤20, the rotational viscosity is 10000-20000cp, and the release rate is 10-18, which meets the standards.
[0073] Cool down and discharge.
[0074] In this embodiment, by using rosin-modified phenolic resin with high viscosity and molecular weight to make the resin binder, the viscosity of the main coating material can be increased, which is conducive to the stable dispersion of the antibacterial additive.
[0075] In one embodiment, the antibacterial printing coating is an antibacterial ink. The antibacterial ink includes the following components in weight percentage: 60-78% coating main material, 7-10% antibacterial additive and 15-25% dispersant. The weight percentage of the coating main material can be, for example, 60%, 65%, 70%, 75% or 78%, or any value between 60 and 78%. The weight percentage of the antibacterial additive can be, for example, 7%, 8% or 10%, or any value between 7 and 10%. The weight percentage of the dispersant can be, for example, 15%, 17%, 18%, 20% or 25%, or any value between 15 and 25%.
[0076] In another embodiment, the antibacterial printing coating is an antibacterial varnish, and the antibacterial varnish includes the following components in weight percentage: 55-78% of the coating main material, 2-8% of the antibacterial additive and 20-40% of the dispersant. The weight percentage of the coating main material can be, for example, 55%, 60%, 65%, 70% or 78%, or any value in the range of 55-78%; the weight percentage of the antibacterial additive can be, for example, 2%, 3%, 5% or 8%, or any value in the range of 2-8%; the weight percentage of the dispersant can be, for example, 20%, 25%, 30%, 35% or 40%, or any value in the range of 20-40%.
[0077] Figure 1 FIG. 2 is a flow chart showing a method for preparing an antibacterial printing coating according to an embodiment of the present invention. Figure 1 As shown, one embodiment of the present invention also provides a method for preparing the above antibacterial ink, comprising the following steps:
[0078] Step S100, heating the base oil of the main coating material to any value between 40°C and 100°C;
[0079] Step S200, adding 15-40% by weight of a dispersant to the base oil and stirring, and keeping warm for 8-15 minutes until the dispersant is completely dissolved;
[0080] Step S300, adding 2-10% by weight of an antibacterial additive and stirring until the antibacterial agent is dispersed into a transparent state to form an antibacterial base oil;
[0081] Step S400, mixing other materials in the main coating material with the antibacterial base oil and stirring.
[0082] In step S100, during the heating of the base oil of the coating main material, the heating temperature may be, for example, 40° C., 60° C., 80° C. or 100° C. The insulation time in step S200 may be, for example, 8 minutes, 10 minutes, 12 minutes or 15 minutes.
[0083] The corresponding base oil in step S100 is mineral oil and / or vegetable oil. Before step S400, it also includes the step of preparing color base ink, by kneading the resin binder, vegetable oil and pigment, squeezing water, cleaning, vacuuming, coloring and testing moisture and rolling to form a color base ink with a fineness of less than 5 microns, and then the color base ink, filler and some additives are mixed with the antibacterial base oil. The filler here also needs to be rolled to a fineness of less than 5 microns.
[0084] In this embodiment, the heating temperature of the base oil is controlled between 40-100°C to ensure the dispersing effect of the dispersant. This is because if the temperature is too low, the viscosity of the base oil will be too high, and too many bubbles will be generated during stirring, while if the temperature is too high, the dispersant will decompose and the dispersing effect will be low. In addition, if the temperature is too high, the viscosity of the base oil will be small, which will affect the dispersing effect of the antibacterial additive.
[0085] Furthermore, in this embodiment, the dispersant is first evenly dispersed in the base oil, and then the antibacterial additive is added, that is, the antibacterial additive is added after the dispersant itself is evenly distributed. Since the dispersant itself is a multi-block material with a high viscosity, if the dispersant and the antibacterial additive are added to the base oil at the same time, it will cause the molecular chains to be entangled, making the antibacterial additive dispersion effect worse. That is to say, in this embodiment, by adding the dispersant and the antibacterial additive to the base oil in two steps, the dispersion effect of the antibacterial additive can be further guaranteed.
[0086] Some embodiments of the present invention also provide an antibacterial coating structure, which includes an ink layer and a varnish layer coated on the surface of the ink layer, the material of the ink layer includes the antibacterial ink in any of the above embodiments, and the material of the varnish layer includes the antibacterial varnish in any of the above embodiments.
[0087] The antibacterial coating structure of the present embodiment includes an ink layer and a varnish layer both of which contain antibacterial additives, and thus the content of the antibacterial additives is higher. On the basis of the varnish layer continuing to play an antibacterial role, even if the varnish layer consumes part of the antibacterial additives due to factors such as friction, the underlying ink layer can still play an antibacterial role. Moreover, since the density of the antibacterial additives is set to be smaller than the density of the main material of the coating, the antibacterial additives in the ink layer and the varnish layer can be on the upper surface, thereby enhancing the surface antibacterial effect of the structure.
[0088] Furthermore, the amount of dispersant added in the material of the ink layer in this embodiment is insufficient relative to the antibacterial additive, so at least some particles of the antibacterial additive in the ink layer are not adsorbed by the dispersant, while the amount of dispersant added in the material of the varnish layer is excessive relative to the antibacterial additive, so at least some polyamide blocks of the dispersant in the material of the varnish layer are not adsorbed by the antibacterial additive particles. And because the dispersant is evenly distributed in the antibacterial ink and the antibacterial varnish, and the antibacterial additive has a tendency to float on the surface due to its low density, the connection of the components in the ink layer is manifested as the dispersant adsorbing part of the antibacterial additive. This part of the antibacterial additive is dispersed in the antibacterial ink, and the other antibacterial additives will be more concentrated on the surface of the ink layer. The antibacterial additives on the surface of this part of the ink layer can be adsorbed by the excess dispersant in the varnish layer, which forms a binding force between the ink layer and the varnish layer, increasing the adhesion of the varnish layer on the ink layer. At the same time, the antibacterial additives in the ink layer are partially bonded to the varnish layer, so that the entire varnish layer has more antibacterial additives, thereby enhancing the antibacterial properties of the antibacterial coating structure.
[0089] Figure 2 FIG. 1 is a flow chart showing a method for preparing an antibacterial coating structure according to an embodiment of the present invention. Figure 2 As shown, the embodiment of the present application also provides a preparation method for preparing the above antibacterial coating structure, the preparation method comprising:
[0090] Step S10, coating the antibacterial ink on the surface of the substrate to be printed to form an ink layer;
[0091] Step S20, coating the ink layer with antibacterial varnish after a preset time to form a varnish layer, wherein the preset time is 60-90% of the drying time of the ink layer, for example, the preset time is 60%, 85% or 90% of the drying time of the ink layer. In one embodiment, the preset time in step S20 is 70-80% of the drying time of the ink layer, for example, the preset time is 70%, 75% or 80% of the drying time of the ink layer.
[0092] The drying time of the ink layer in step S20 refers to the time required for the ink layer to completely dry.
[0093] The preparation method of this embodiment applies a varnish layer when the ink layer is more than half dry but not completely dry. On the one hand, it can prevent the small molecule antibacterial additives in the varnish layer from penetrating through the ink layer to the surface of the substrate and reducing the antibacterial effect as much as possible. On the other hand, it can also ensure that the dispersant in the varnish layer can be effectively adsorbed with the antibacterial additives in the ink layer, so that the antibacterial coating structure can achieve better antibacterial effect.
[0094] Example 1
[0095] The antibacterial printing coating is an antibacterial ink, comprising the following components in weight percentage: 18% PR57:1 red pigment, 7% 2731 mineral oil, 2% linseed oil, 38% resin binder (wherein the resin binder comprises 65% colloid oil and 35% 218 resin oil), 8% antibacterial additive, 20% dispersant, 2% cobalt naphthenate, 5% nano calcium carbonate. The antibacterial additive comprises the following components in weight percentage: 97.6% citric acid, 1.6% Pt·C7H15N3, and 0.8% malic acid.
[0096] The dispersant in this embodiment is prepared by the following steps:
[0097] Add 284.5 g of stearic acid, 114.1 g of caprolactone, 130.1 g of hydroxycaproic acid and 113.2 g of caprolactam into a reaction container, and add 0.1 g of stannous octoate;
[0098] Argon was introduced into the reaction vessel and the reaction vessel was heated to 180° C. and kept at this temperature for 12 h;
[0099] The reaction vessel was cooled to room temperature, and the reaction product was poured into excess cold methanol to precipitate the polymer;
[0100] washing the precipitated first polymer with cold methanol;
[0101] The washed first polymer was dried in a vacuum drying oven at 50° C. for 20 h;
[0102] The first polymer and 705 g of tetraethylenepentamine were added to a reaction vessel, and 0.7 g of toluenesulfonic acid catalyst was added simultaneously;
[0103] Heat the reaction vessel to 140°C and keep it warm for 6 hours under nitrogen protection;
[0104] Cool the reaction vessel to room temperature;
[0105] pouring the reaction product into a cold solvent to precipitate a second polymer;
[0106] washing the precipitated second polymer with acetone to remove unreacted monomers and catalyst residues;
[0107] The washed second polymer was dried in a vacuum drying oven at 50° C. for 30 hours to finally prepare a dispersant.
[0108] The colloid oil in the resin binder of this embodiment includes the following components in weight percentage: 23.28% rosin, 8.43% octylphenol, 8.44% formaldehyde, 1.77% glycerol, 0.19% PTS catalyst, 19.89% soybean oil, 37.2% JETA-1 kerosene, and 0.8% aluminum isooctanoate. The corresponding preparation method includes the following steps:
[0109] Add rosin into the reactor and heat it to 150°C. After the rosin is dissolved, add octylphenol and formaldehyde;
[0110] Heat to 200°C for addition reaction for 1.5h;
[0111] After the addition, glycerol and PTS catalyst were added;
[0112] The esterification reaction was carried out at 280°C for 8 hours and vacuum was applied for 1 hour;
[0113] Cool down to 200℃, add soybean oil and JETA-1 kerosene, stir evenly, and keep warm for 30 minutes;
[0114] The temperature was lowered to 170°C, aluminum isooctanoate was added and stirred for 1 hour to obtain the colloid oil in the resin binder.
[0115] The rotational viscosity of the prepared colloid oil was detected to be 250,000 mPas, the viscosity was 12, and the yield value was 5000 mPa.
[0116] The antibacterial ink of this embodiment is prepared by the following preparation method:
[0117] Providing raw materials according to the above weight percentages;
[0118] Dispersion by squeezing water: Empty the kneader, open the steam valve, add PR57:1 red pigment into the kneader, control the temperature of the kneader not more than 35℃, control the speed at a low speed, stir for 3 to 5 minutes, add colloid oil and stir until the water is clear, pour water 5 to 7 times;
[0119] Cleaning: Start heating and set the temperature at 85℃, inject tap water into the kneader after pouring water, stop injecting water when the water level exceeds the ink, stir for 5 minutes and then pour water, repeat three times, and control the speed at a low speed;
[0120] Vacuuming: Start vacuuming when the temperature rises to 60℃, control the temperature not to exceed 85℃-120℃, keep the pressure at -0.08MPa--0.1MPa, and control the speed at high speed;
[0121] Color development and moisture testing: After confirming that the color, transparency and moisture content are qualified, turn off the steam and let in condensed water;
[0122] Mixing: Slowly add 218 resin oil and linseed oil under high-speed stirring, and stir thoroughly until there are no lumps;
[0123] Rolling: The dispersed base ink is put into a bead mill for rolling, and then passed through an oblique rolling process, with a fineness of ≤5μm;
[0124] Heat 2731 mineral oil to 80℃;
[0125] Add dispersant to 2731 mineral oil and stir, and keep warm for 10 minutes until the dispersant is completely dissolved;
[0126] adding an antimicrobial additive and stirring until the antimicrobial agent is dispersed to a transparent state to form an antimicrobial base oil;
[0127] The rolled base ink, cobalt cyclohexane acid, nano calcium carbonate and the antibacterial base oil are mixed and stirred.
[0128] Example 2
[0129] The only difference between Example 2 and Example 1 is that the PR57:1 red pigment in Example 1 is replaced with PY12 yellow pigment, the weight percentage of PY12 yellow pigment is 13%, the weight percentage of 2731 mineral oil is 10%, the weight percentage of linseed oil is 4%, and the coloring step is removed.
[0130] Example 3
[0131] The only difference between Example 3 and Example 2 is that the PY12 yellow pigment in Example 2 is replaced with CIPB15:3 blue pigment, the weight percentage of CIPB15:3 blue pigment is 17%, the weight percentage of 2731 mineral oil is 8%, and the weight percentage of linseed oil is 2%.
[0132] Example 4
[0133] This embodiment adopts a dry powder preparation process. The only difference between Embodiment 4 and Embodiment 1 is that the PR57:1 red pigment in Embodiment 1 is replaced with carbon black, the weight percentage of carbon black is 20%, the weight percentage of 2731 mineral oil is 6%, and the weight percentage of linseed oil is 1%, and the steps of squeezing water dispersion, washing, vacuuming and color development to check moisture are removed.
[0134] Example 5
[0135] The antibacterial printing coating is an antibacterial varnish, comprising the following components in weight percentage: 25% JETA-1 kerosene, 14% sesame oil, 14% rosin, 2.5% maleic anhydride, 3.2% glycerol, 0.3% PTS catalyst, 6% antibacterial additive, 28% dispersant, 4% nano calcium carbonate, 1% MAW-331 wax, 1% MAD-801 cobalt desiccant, and 1% MAD-703 manganese desiccant. The antibacterial additive and dispersant in this embodiment are the same as those used in Example 1.
[0136] The preparation method of the antibacterial varnish of this embodiment comprises the following steps:
[0137] Providing raw materials according to the above weight percentages;
[0138] Add rosin into the reactor and heat it to 160°C until the rosin is completely dissolved;
[0139] Add maleic anhydride, heat to 200°C and keep warm for 1.5h;
[0140] Add glycerol and PTS catalyst;
[0141] Continue to raise the temperature to 250°C and keep the temperature, and perform esterification reaction for 5 hours to generate rosin-based resin;
[0142] When the rosin-based resin is cooled to an acid value of ≤25 mg / g and the rotational viscosity is 8000 mPas, sesame oil and 60% JETA-1 kerosene are added;
[0143] The temperature was controlled at 200°C and kept for 30 minutes, and the viscosity, viscosity and yield value were tested. In this embodiment, the viscosity was 500 mPas, the viscosity was 15, and the yield value was 1800 Pa;
[0144] Add dispersant and stir, and keep warm for 8 minutes until the dispersant is completely dissolved;
[0145] Add 8% by weight of an antibacterial additive and stir until the antibacterial agent is dispersed into a transparent state;
[0146] Cool down to 50℃, add nano calcium carbonate, MAW-331 wax, MAD-801 cobalt desiccant and MAD-703 manganese desiccant, and stir at high speed for 30 minutes until uniform;
[0147] Use the remaining kerosene to adjust the viscosity to 7 and then can it be packed.
[0148] Comparative Example 1
[0149] The difference between Comparative Example 1 and Example 1 is that no antibacterial additive and dispersant are added in Comparative Example 1.
[0150] Comparative Example 2
[0151] The only difference between Comparative Example 2 and Example 2 is that no antibacterial additive and dispersant are added in Comparative Example 2.
[0152] Comparative Example 3
[0153] The difference between Comparative Example 3 and Example 3 is that no antibacterial additive and dispersant are added in Comparative Example 3.
[0154] Comparative Example 4
[0155] The difference between Comparative Example 4 and Example 4 is that no antibacterial additive and dispersant are added in Comparative Example 4.
[0156] Comparative Example 5
[0157] The difference between Comparative Example 5 and Example 1 is that the dispersant in Example 1 is replaced by CH-6.
[0158] Comparative Example 6
[0159] The difference between Comparative Example 6 and Example 1 is that the dispersant in Example 1 is replaced by PEA1:0.8-PCL10.
[0160] Comparative Example 7
[0161] The difference between Comparative Example 7 and Example 1 is that the antibacterial additive in Example 1 is replaced by NiAgAPO-11 / MCM-41.
[0162] Comparative Example 8
[0163] The only difference between Comparative Example 8 and Example 5 is that no antibacterial additive and dispersant are added in Comparative Example 8.
[0164] Comparative Example 9
[0165] The only difference from Example 1 is that the heating temperature of the mineral oil is 30°C.
[0166] Comparative Example 10
[0167] The only difference from Example 1 is that the heating temperature of the mineral oil is 120°C.
[0168] Comparative Example 11
[0169] The only difference from Example 1 is that the antibacterial additive and the dispersant are added to the mineral oil at the same time, stirred until uniform, and kept warm for 10 minutes.
[0170] According to experimental data, when the antibacterial ink in Example 1 is printed on a substrate, it can maintain long-term antibacterial performance against the 4th generation Staphylococcus aureus ATCC6538 for 12 to 15 months without friction, and the antibacterial rate is greater than 80%.
[0171] Figure 3 The figure shows the antibacterial additive dispersion effect of the antibacterial ink according to Example 1 of the present invention. Figure 4 The antibacterial additive dispersion effect diagram of the antibacterial ink of Comparative Example 6 is shown. It should be noted that in order to more clearly observe the dispersion effect of the antibacterial additive, Figure 3 and Figure 4 No colored base ink is added. Figure 3 and Figure 4 It can be seen that the antibacterial additive in the antibacterial ink in Example 1 of the present invention can be well dispersed in the main material of the coating, while the antibacterial additive in Comparative Example 6 is not well compatible with the main material of the coating, which shows that the dispersant in Example 1 has a better dispersion effect.
[0172] Table 1 specifically shows the weight percentage of antibacterial additives that can be effectively dispersed by the dispersants of Example 1, Comparative Example 5, Comparative Example 6, and Comparative Example 7. The percentage of antibacterial additives in Table 1 can be seen from the content of Table 1. The dispersant of Example 1 can effectively disperse 8% of the weight percentage of antibacterial additives into the ink system. The commonly used ink dispersant CH-6 in Comparative Example 5 has a poor dispersing effect on antibacterial additives, and the weight percentage of antibacterial additives in the ink is less than 1%. The dispersant with polyetheramine and polyester segments in Comparative Example 6 cannot well disperse the antibacterial dispersant, which shows that the polyamide block in the dispersant in this application is an important part to ensure the dispersion effect. According to the data corresponding to Comparative Example 7 in Table 1, the dispersant including polyester-polyamide mixed block polymer materials in this application cannot effectively disperse NiAgAPO-11 / MCM-41 type antibacterial additives. According to the data in Table 1, the dispersant in Example 1 can significantly improve the dispersion effect of organic acid antibacterial agents containing noble metal coordination compounds compared with other dispersants.
[0173] Table 1
[0174]
[0175] The theoretical amount of dispersant can be determined according to the specific surface area of the antibacterial additive particles. The larger the specific surface area, the greater the amount of dispersant added. Assuming that all antibacterial additive particles are solid particles, the theoretical amount of dispersant used is 10-15% (weight percentage), but in actual situations, the antibacterial additive includes some solid particles and some hollow particles, so the corresponding amount of dispersant needs to be adjusted accordingly. The antibacterial additive in Example 1 is a nano-scale particle. For an antibacterial additive that includes some hollow spherical particles, in order to effectively disperse the antibacterial additive, the theoretical amount of dispersant needs to be increased. According to the orthogonal test results of different added amounts of dispersant and antibacterial additive (part of the test data is shown in Table 2 below), it is determined that the best effect is achieved when the amount of dispersant is between 15-40% (weight percentage). Tests 1 to 7 in Table 2 only change the weight percentage of the coating main material and the dispersant, and other conditions are consistent with Example 1.
[0176] It can be seen from the test data in Table 2 that when the weight percentage of the dispersant is less than 15%, the dispersion effect is poor, but as the weight percentage of the dispersant increases, the dispersion effect also increases accordingly. When it increases to 15% to 40%, the dispersion effect is relatively stable and maintained at 8%. When the dispersant accounts for more than 40%, the dispersion effect weakens.
[0177] Table 2
[0178]
[0179] In order to verify the antibacterial properties of antibacterial ink and antibacterial varnish, the antibacterial properties of antibacterial varnish and antibacterial inks of different colors were tested against Staphylococcus aureus ATCC 6538, Escherichia coli 8099 and Candida albicans ATCC 10231.
[0180] The test refers to WS / T650-2019 "Antibacterial and Antibacterial Effect Evaluation Method" 5.2.6 Film Test Method. First, the sample is pre-treated, including UV sterilization for 30 minutes. The neutralization solution is SCDLP, and the culture medium is nutrient agar. The shape of the test sample is 5*5cm square and the thickness is 0.1mm. The contact temperature is 36±1℃, RH%>90%. The amount of inoculated bacterial solution is 0.4mL. The covering film is a PE film of 4*4cm square and 0.01mm thick.
[0181] The specific results of the antibacterial performance test of Examples 1 to 5, Comparative Examples 1 to 4 and Comparative Example 8 on Staphylococcus aureus ATCC 6538 are shown in Table 3 below:
[0182] Table 3
[0183]
[0184]
[0185] The specific results of the antibacterial performance test of Examples 1 to 5, Comparative Examples 1 to 4 and Comparative Example 8 on Escherichia coli 8099 are shown in Table 4 below:
[0186] Table 4
[0187]
[0188] The specific results of the antibacterial performance test of Examples 1 to 5, Comparative Examples 1 to 4 and Comparative Example 8 on Candida albicans ATCC 10231 are shown in Table 5 below:
[0189] Table 5
[0190]
[0191]
[0192] A in Tables 3 to 5 above all represent the logarithmic mean value (unit: CFU / sample) of the number of recovered colonies of each comparative example after 0h of inoculation, B in Tables 3 to 5 above all represent the logarithmic mean value (unit: CFU / sample) of the number of recovered colonies of each comparative example after 24h of inoculation, and C in Tables 3 to 5 all represent the logarithmic mean value (unit: CFU / sample) of the number of recovered colonies of each embodiment after 24h of inoculation. The antibacterial activity value R of each embodiment in Tables 3 to 5 above is R=lg(B / C), and the antibacterial rate R' is R'=(BC) / B×100%. B and C in these two formulas are the values of B and C of the corresponding comparative example and embodiment. For example, Example 1 and Comparative Example 1 are corresponding groups, and B in the calculation formula of the antibacterial activity value R and the antibacterial rate R' of Example 1 is B of Comparative Example 1, and C in the formula is C of Example 1.
[0193] According to the data in Tables 3 to 5, Examples 1 to 5 have antibacterial effects on Staphylococcus aureus ATCC 6538, Escherichia coli 8099 and Candida albicans ATCC 10231. The antibacterial rates of Staphylococcus aureus ATCC 6538 and Escherichia coli 8099 are greater than 99.99%, indicating that they have strong antibacterial effects on Staphylococcus aureus ATCC 6538 and Escherichia coli 8099. Compared with Comparative Examples 1 to 4 and Comparative Example 8 to which no antibacterial additives and dispersants are added, the antibacterial performance is significantly improved.
[0194] Table 6 shows the weight percentage of the final antibacterial additive in the antibacterial inks of Example 1 and Comparative Examples 9 to 11.
[0195] Table 6
[0196] Example 1 Comparative Example 9 Comparative Example 10 Comparative Example 11 Antimicrobial additive weight percentage 8% 5% 3% 4%
[0197] From the data in Table 6, it can be found that when the heating temperature of the base oil of the main material is too high or too low, it will significantly affect the dispersion effect of the antibacterial additive. Adding the antibacterial additive and the dispersant to the base oil at the same time will also significantly reduce the dispersion effect of the antibacterial additive.
[0198] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. An antibacterial printing coating, characterized in that, The invention comprises the following components in weight percentage: 55-80% coating main material, 2-10% antibacterial additive and 15-40% dispersant; The antimicrobial additive comprises a coordination compound containing a noble metal and an organic acid, and the density of the antimicrobial additive is less than the density of the main coating material; The dispersant comprises a polyester-polyamide mixed block polymer material. The polyester block of the dispersant is dissolved in the base oil of the coating main material, and the polyamide block of the dispersant is adsorbed on the surface of the coordination compound containing precious metals of the antibacterial additive.
2. The antibacterial printing coating according to claim 1, characterized in that: The dispersant is prepared by copolymerization of fatty acid, lactone compound, hydroxy acid, lactam compound and polyamine.
3. The antibacterial printing coating according to claim 1 or 2, characterized in that: The antibacterial printing coating is an antibacterial ink, which comprises the following components in weight percentage: 60-78% of a coating main body material, 7-10% of an antibacterial additive, and 15-25% of a dispersant.
4. The antibacterial printing coating according to claim 1 or 2, characterized in that: The antibacterial printing coating is an antibacterial varnish, which comprises the following components in weight percentage: 55-78% of a coating main body material, 2-8% of an antibacterial additive, and 20-40% of a dispersant.
5. A method for preparing the antibacterial printing coating according to claim 3, characterized in that: The following steps are involved: heating the base oil of the coating main material to any value between 40° C. and 100° C.; Adding 15-40% by weight of the dispersant to the base oil, stirring, and keeping warm for 8-15 minutes until the dispersant is completely dissolved; Adding 2-10% by weight of the antibacterial additive and stirring until the antibacterial agent is dispersed into a transparent state to form an antibacterial base oil; The other materials in the main coating material are mixed with the antibacterial base oil and stirred.
6. An antibacterial coating structure, characterized in that: The invention comprises an ink layer, wherein the material of the ink layer comprises the antibacterial ink according to claim 3.
7. The antibacterial coating structure according to claim 6, characterized in that: The invention also includes a varnish layer coated on the surface of the ink layer, wherein the material of the varnish layer includes the antibacterial varnish as claimed in claim 4.
8. A method for preparing the antibacterial coating structure according to claim 7, characterized in that: include: Applying the antibacterial ink on the surface of the substrate to be printed to form the ink layer; The antibacterial varnish is coated on the ink layer after a preset time to form the varnish layer, wherein the preset time is 60-90% of the drying time of the ink layer.
9. The preparation method according to claim 8, characterized in that The preset time is 70-80% of the drying time of the ink layer.
Citation Information
Patent Citations
Antibacterial and bacteriostatic UV offset printing ink
CN101818005A
Antibacterial and bacteriostatic oily ink
CN101818007A
Comb-shaped hyper-dispersant as well as preparation method and application
CN106750342A
Polymeric dispersants containing one or two quaternary amine anchoring groups with improved chemical and thermal stability
CN110214163A
Polyester / polyamide copolymer as well as preparation method and application thereof
CN111234208A