3D mobile phone rear cover transfer printing ink and preparation method and application thereof
By using a combination of acrylic resin, modified resin and talc matting powder ink on 3D glass, the problem of poor ink printing on high-curvature 3D glass is solved, achieving efficient, uniform printing effects and strong adhesion. 3D glass surfaces for smartphones and wearable electronics.
Patent Information
- Application Number
- CN202410898628.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-05
AI Technical Summary
Traditional pad printing inks cannot meet the printing needs of high-curvature 3D glass. In particular, the inking effect is not good at concave curvatures, and cannot meet the printing needs of 3D glass front covers for smartphones and wearable electronic products.
Using a combination of acrylic resin, polyester modified acrylic resin and polyester modified hydroxy acrylic resin, combined with talc powder and matting powder as fillers, through specific viscosity and solid content design, the adhesion and resolution of the ink are optimized, using silane Ingredients such as coupling agent and isocyanate curing agent form a pad printing ink suitable for high-curvature 3D glass, and the printing effect is improved through specific preparation methods and baking conditions.
It achieves efficient and uniform printing effects on the 3D glass surface, with neat edges, strong aging resistance, good adhesion, not easy to peel off, and excellent printing edge properties, avoiding the problems of ink spillage and poor adhesion.
Smart Images

Figure BDA0004929826490000061 
Figure BDA0004929826490000071
Abstract
Description
Technical Field
[0001] The invention relates to a 3D mobile phone back cover pad printing ink and a preparation method and application thereof, and relates to C09D, and in particular to the field of coating compositions. Background Art
[0002] With the diversification and refinement of electronic products, the dashboards of smartphones and wearable electronic products can use 3D glass as the front cover, which improves the stylish appearance of terminal electronic products while providing better touch and user experience. However, the ordinary silk screen printing process can no longer meet the printing needs of 3D cover plates, and the printing effect is not good at the concave curvature of the 3D cover plates. The pad printing process can be used to achieve surface printing of 3D glass, but as the curvature of 3D glass increases from the ordinary 50 degrees to 80 degrees or even higher, traditional pad printing inks can no longer meet the printing of 3D glass with higher curvatures. Therefore, it is crucial to develop an ink suitable for printing 3D glass with large curvatures, especially to optimize the ink application effect at the concave curvature and the ink application at the r angle.
[0003] Chinese invention patent CN201910911742.2 discloses an environmentally friendly edge banding ink and its preparation method. It uses a combination of acrylic resins with suitable molecular weights and an anionic polymer dispersant to improve the resin strength and optimize the ink effect. However, it cannot achieve the printing of 3D glass concave surfaces. Chinese invention patent CN201310086603.3 discloses a water-based printing ink and its application. The introduced acrylic resin aminated liquid is an excellent dispersion medium for organic pigments and inorganic pigments, and has excellent compatibility with acrylic polymer emulsions. The water-based printing effect is better, but it still cannot meet the printing requirements of 3D glass inner concave surfaces. Summary of the invention
[0004] In order to improve the printing performance of pad printing ink on the surface of 3D glass of mobile phones, the first aspect of the present invention provides a 3D mobile phone back cover pad printing ink, and the preparation raw materials include, by weight: 50-70 parts of acrylic resin, 10-20 parts of pigment, 10-20 parts of filler, 1-3 parts of adhesive, 5-15 parts of curing agent, 1-10 parts of dispersant, and 1-5 parts of auxiliary agent.
[0005] As a preferred embodiment, the raw materials for preparation include, by weight: 55-65 parts of acrylic resin, 10-14 parts of pigment, 10-14 parts of filler, 1-2 parts of adhesive, 8-12 parts of curing agent, 4-6 parts of dispersant, and 1-2 parts of auxiliary agent.
[0006] As a preferred embodiment, the acrylic resin is a modified acrylic resin, and the modified acrylic resin is selected from one or a combination of hydroxy acrylic resin, polyester modified acrylic resin, polyester modified hydroxy acrylic resin, and silicone modified acrylic resin.
[0007] As a preferred embodiment, the polyester-modified acrylic resin has a viscosity of 5000-7000 mPa·s at 25° C. and a solid content of 40-60 wt %.
[0008] As a preferred embodiment, the viscosity of the polyester-modified hydroxy acrylic resin at 25° C. is 15000-20000 mPa·s.
[0009] As a preferred embodiment, the acrylic resin is a combination of a polyester-modified acrylic resin and a polyester-modified hydroxy acrylic resin.
[0010] As a preferred embodiment, the weight ratio of the polyester modified acrylic resin to the polyester modified hydroxy acrylic resin is (10-30): (30-50).
[0011] As a preferred embodiment, the weight ratio of the polyester modified acrylic resin to the polyester modified hydroxy acrylic resin is (15-25): (35-45).
[0012] As a preferred embodiment, the weight ratio of the polyester-modified acrylic resin to the polyester-modified hydroxy acrylic resin is 20:40.
[0013] During the experiment, the applicant found that the combination of two modified acrylic resins has good pad printing properties for 3D glass, can improve the adhesion of 3D glass pad printing, improve the printing effect, and the printed edges are neat and uniform without burrs. The possible reason is speculated to be: a polyester-acrylic copolymer with a solid content of 50wt% and a viscosity of 6000mPa·s is combined with a polyester-modified hydroxy acrylate resin with a viscosity of 16000mPa·s. The prepared resin mother solution has a moderate viscosity, which can balance the viscosity and leveling properties, and maintain a good adhesion effect at the concave curvature of the 3D glass. There will be no ink overflow at the curvature, and there will be no problem of poor adhesion during leveling, thereby improving the pad printing performance at the concave curvature of the 3D glass.
[0014] As a preferred embodiment, the pigment is carbon black.
[0015] As a preferred embodiment, the filler is selected from one or a combination of talcum powder, matting powder, calcium carbonate, barium sulfate, and white carbon black.
[0016] As a preferred embodiment, the filler is a combination of talcum powder and matting powder.
[0017] As a preferred embodiment, the weight ratio of the talc powder to the matting powder is (5-10): (1-5).
[0018] As a preferred embodiment, the weight ratio of talcum powder to matting powder is (7-9): (3-5).
[0019] As a preferred embodiment, the weight ratio of the talcum powder to the matting powder is 8:4.
[0020] The applicant further discovered that using a combination of talcum powder and matting powder as a filler can improve the resolution of printing and enhance the printing effect. The reason may be that using a combination of talcum powder and matting powder as a filler can improve the solid dispersion effect of the ink, and the resulting ink has strong aging resistance and solvent resistance. After being applied to the 3D glass surface, it is not easy to peel off and has excellent gloss.
[0021] As a preferred embodiment, the adhesion agent is a silane coupling agent, and the silane coupling agent is selected from one or a combination of bisaminosilane coupling agent, epoxy silane coupling agent, γ-glycidyl ether propyl trimethoxy silane, and N-β (aminoethyl) -γ-aminopropyl trimethoxy silane.
[0022] As a preferred embodiment, the adhesive agent is an epoxy silane coupling agent.
[0023] As a preferred embodiment, the curing agent is selected from one or a combination of isocyanate curing agents, aliphatic amine curing agents, amide amine curing agents, and aromatic amines.
[0024] As a preferred embodiment, the curing agent is an isocyanate curing agent. Preferably, the curing agent is an XDI isocyanate curing agent.
[0025] As a preferred embodiment, the dispersant is a polyurethane modified dispersant.
[0026] As a preferred embodiment, the auxiliary agent is a leveling agent, and the leveling agent is a silicone leveling agent.
[0027] As a preferred implementation, the fineness of the 3D mobile phone back cover pad printing ink is ≤8 μm.
[0028] A second aspect of the present invention provides a method for preparing a 3D mobile phone back cover pad printing ink, comprising the following steps:
[0029] The prepared raw materials are added in sequence at a dispersing speed of 200-400r / min while being dispersed. After the materials are completely added, they are dispersed at a speed of 600-1000r / min for 5-15min, then ground, and filtered through a 100-300 mesh filter to obtain ink.
[0030] A third aspect of the present invention provides an application of a 3D mobile phone back cover pad printing ink in preparing a back cover glass or a front cover glass of a 3D mobile phone.
[0031] As a preferred embodiment, the printing method of the 3D mobile phone back cover pad printing ink comprises the following steps:
[0032] The 3D mobile phone back cover pad printing ink is pad printed on the 3D mobile phone front cover or back cover glass through the rubber head of a fully automatic pad printing machine, and then baked at a temperature of 150° C.-180° C., kept at a constant temperature for 30 min-60 min, and cooled to obtain a coating with a thickness of 8-12 μm.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] (1) The 3D mobile phone back cover pad printing ink of the present invention adopts a combination of polyester modified acrylic resin and polyester modified hydroxy acrylic resin, which can improve the adhesion of 3D glass pad printing and improve the printing effect. The printed edge is neat and uniform without burrs.
[0035] (2) The 3D mobile phone back cover pad printing ink of the present invention uses a combination of talcum powder and matting powder as filler, which can improve the printing resolution and printing effect. The formed ink has strong aging resistance and solvent resistance. After being applied to the 3D glass surface, it is not easy to peel off and has excellent gloss.
[0036] (3) The 3D mobile phone back cover pad printing ink of the present invention is constructed by pad printing technology, which is simple to operate and can print frames and characters on 3D curved glass. It has excellent adhesion and weather resistance, good printing edge properties, and is not prone to problems such as roughness and chipping. DETAILED DESCRIPTION
[0037] The manufacturers and models of the raw materials prepared in the examples are shown in Table 1.
[0038] Example 1
[0039] A 3D mobile phone back cover pad printing ink, the preparation raw materials of which include, by weight: 60 parts of acrylic resin, 12 parts of pigment, 12 parts of filler, 1 part of adhesive, 10 parts of curing agent, 5 parts of dispersant and 0.5 parts of auxiliary agent.
[0040] The acrylic resin is a combination of polyester modified acrylic resin and polyester modified hydroxy acrylic resin, with a weight ratio of 40:20. The viscosity of the polyester modified acrylic resin at 25°C is 6000 mPa·s, and the solid content is 50wt%. The viscosity of the polyester modified hydroxy acrylic resin at 25°C is 16000 mPa·s.
[0041] The pigment is carbon black.
[0042] The filler is a combination of talcum powder and matting powder, with a weight ratio of 8:4.
[0043] The adhesive is an epoxy silane coupling agent.
[0044] The curing agent is an XDI isocyanate curing agent.
[0045] The dispersant is a polyurethane modified dispersant.
[0046] The auxiliary agent is a leveling agent, and the leveling agent is an organic silicon leveling agent.
[0047] A method for preparing a 3D mobile phone back cover pad printing ink comprises the following steps:
[0048] The prepared raw materials are added in sequence at a dispersing speed of 300r / min while dispersing. After the materials are completely added, they are dispersed at a speed of 800r / min for 10min, and then ground with a horizontal three-roll mill. After the fineness is detected to be ≤8μm, a curing agent is added to obtain the ink.
[0049] Example 2
[0050] A 3D mobile phone back cover pad printing ink and a preparation method thereof, the specific implementation manner is the same as that of Example 1, except that the acrylic resin is a combination of polyester-modified acrylic resin and polyester-modified hydroxy acrylic resin, with a weight ratio of 20:40.
[0051] Example 3
[0052] A 3D mobile phone back cover pad printing ink and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the preparation raw materials include, by weight: 60 parts of acrylic resin, 12 parts of pigment, 12 parts of filler, 1 part of adhesion agent, 10 parts of curing agent, 2 parts of dispersant, and 0.5 parts of auxiliary agent.
[0053] Example 4
[0054] A 3D mobile phone back cover pad printing ink and a preparation method thereof, the specific implementation manner is the same as that of Example 3, except that the filler is a combination of talcum powder and matting powder, and the weight ratio is 4:8.
[0055] Example 5
[0056] A 3D mobile phone back cover pad printing ink and a preparation method thereof. The specific implementation method is the same as that of Example 2, except that the preparation raw materials include, by weight: 60 parts of acrylic resin, 16 parts of pigment, 12 parts of filler, 1 part of adhesive, 10 parts of curing agent, 5 parts of dispersant, and 0.5 parts of auxiliary agent.
[0057] Comparative Example 1
[0058] A 3D mobile phone back cover pad printing ink and a preparation method thereof, the specific implementation manner is the same as that of Example 2, except that the acrylic resin is a combination of polyester-modified acrylic resin and polyester-modified hydroxy acrylic resin, with a weight ratio of 0:60.
[0059] Comparative Example 2
[0060] A 3D mobile phone back cover pad printing ink and a preparation method thereof, the specific implementation manner is the same as that of Example 2, except that the acrylic resin is a combination of polyester-modified acrylic resin and polyester-modified hydroxy acrylic resin, with a weight ratio of 60:0.
[0061] Comparative Example 3
[0062] A 3D mobile phone back cover pad printing ink and a preparation method thereof, wherein the specific implementation manner is the same as that of Example 2, except that the filler is talcum powder.
[0063] Comparative Example 4
[0064] A 3D mobile phone back cover pad printing ink and a preparation method thereof, wherein the specific implementation manner is the same as that of Example 2, except that the filler is a matting powder.
[0065] Comparative Example 5
[0066] A 3D mobile phone back cover pad printing ink and a preparation method thereof. The specific implementation method is the same as that of Example 2, except that the preparation raw materials include, by weight: 60 parts of acrylic resin, 16 parts of pigment, 12 parts of filler, 0 parts of adhesive, 10 parts of curing agent, 5 parts of dispersant, and 0.5 parts of auxiliary agent.
[0067] Table 1
[0068]
[0069] Performance Testing
[0070] The 3D mobile phone back cover pad printing ink prepared in the embodiment and the comparative example was pad printed on the front cover or back cover glass of the 3D mobile phone by the rubber head of the fully automatic pad printing machine, and then baked at a temperature of 150°C, kept at a constant temperature for 40 minutes, and cooled to obtain a coating with a thickness of 8-12 μm. The surface effect of the ink layer and the printing edge effect were observed, and the performance was tested.
[0071] 1. Adhesion test: Adhesion test was performed on the ink layers of the embodiment and the comparative example according to GB / T 1720-79 (89). The test results are shown in Table 2 below.
[0072] 2. Ink printing edge test: Observe the ink printing edge at 20 times under a microscope to see if there are any defects such as defects such as defects such as scratches, hair pulling, and oil flying.
[0073] 3. Acetone wiping test: In the wear tester, use gauze dipped in acetone to wipe the ink surface 100 times with a load of 1kg, and observe whether there is obvious dissolution, expansion or stratification on the ink surface.
[0074] 4. Insulation value test: Use GM3125 impedance tester to test the surface resistance of the printed board (1 cm between two pens) to test whether the resistance can reach 2500V / >100GΩ.
[0075] 5. QUV aging test: Use QUV aging instrument, set the program to 12 cycles, each cycle is 8 hours, including 4 hours of UV light time (0.63W / m 2 / nm and 60℃) and 4 hours of moisture exposure time. After the test, let it stand at room temperature for two hours to observe whether the color and gloss of the glass surface have obvious changes, whether the appearance of the ink surface has changed, and test whether the conventional adhesion reaches level 1.
[0076] The test results are shown in Table 2 below.
[0077] Table 2
[0078]
[0079] By comparing the performance test results of Example 1-2 and Comparative Example 1-2 in Table 2, it can be seen that the optimal performance ratio of polyester modified acrylic resin and polyester modified hydroxy acrylic resin used in the present application is 1:2; exceeding the ratio has a certain impact on the printing edge effect and acetone resistance.
[0080] By comparing the performance test results of Example 2 and Comparative Examples 3-4 in Table 2, it can be seen that when talcum powder or matting powder is used, talcum powder has lower thixotropic properties, and matting powder has higher thixotropic properties. The ink system will cause poor printing such as ink overflow and incompleteness when the thixotropic properties are lower and higher. When the ratio of talcum powder to matting powder is 2:1, a better printing edge effect is achieved.
[0081] By comparing the performance test results of Example 2 and Comparative Example 5 in Table 2, it can be seen that the use of a sealant has a greater impact on adhesion, and the sealant is a key factor in the adhesion of the ink system to the glass substrate.
Claims
1. A 3D mobile phone back cover pad printing ink, characterized in that: The raw materials for preparation include, by weight: 50-70 parts of acrylic resin, 10-20 parts of pigment, 10-20 parts of filler, 1-3 parts of adhesive, 5-15 parts of curing agent, 1-10 parts of dispersant and 1-5 parts of auxiliary agent.
2. The 3D mobile phone back cover pad printing ink according to claim 1, characterized in that: The acrylic resin is a modified acrylic resin, and the modified acrylic resin is selected from one or a combination of hydroxy acrylic resin, polyester modified acrylic resin, polyester modified hydroxy acrylic resin, and silicone modified acrylic resin.
3. The 3D mobile phone back cover pad printing ink according to claim 2, characterized in that: The polyester modified acrylic resin has a viscosity of 5000-7000 mPa·s at 25° C. and a solid content of 40-60 wt %.
4. The 3D mobile phone back cover pad printing ink according to claim 2, characterized in that: The viscosity of the polyester-modified hydroxy acrylic resin at 25° C. is 15000-20000 mPa·s.
5. The 3D mobile phone back cover pad printing ink according to claim 1, characterized in that: The filler is selected from one or a combination of talcum powder, matting powder, calcium carbonate, barium sulfate, and white carbon black. Preferably, the weight ratio of talcum powder to matting powder is (5-10): (1-5).
6. The 3D mobile phone back cover pad printing ink according to claim 1, characterized in that: The adhesive is a silane coupling agent, and the silane coupling agent is selected from one or a combination of bisaminosilane coupling agent, epoxysilane coupling agent, γ-glycidyl ether propyl trimethoxysilane, and N-β (aminoethyl)-γ-aminopropyl trimethoxysilane.
7. The 3D mobile phone back cover pad printing ink according to claim 1, characterized in that: The curing agent is selected from one or a combination of isocyanate curing agents, aliphatic amine curing agents, amide amine curing agents, and aromatic amines.
8. The 3D mobile phone back cover pad printing ink according to claim 1, characterized in that: The fineness of the 3D mobile phone back cover pad printing ink is ≤8μm.
9. A method for preparing the 3D mobile phone back cover pad printing ink according to any one of claims 1 to 8, characterized in that: The following steps are involved: The prepared raw materials are added in sequence at a dispersing speed of 200-400r / min while being dispersed. After the materials are completely added, they are dispersed at a speed of 600-1000r / min for 5-15min, then ground, and filtered through a 100-300 mesh filter to obtain ink.
10. Use of the 3D mobile phone back cover pad printing ink according to any one of claims 1 to 8 in preparing the back cover glass or front cover glass of the 3D mobile phone claims.
Citation Information
Patent Citations
Ultraviolet-cured alkali washing resin as well as preparation method thereof and preparation method of frosted ink
CN103755557A
Transfer printing mirror-like silver ink as well as preparation method and application thereof
CN112961538A